ZIF-8 in-situ characterization method and ZIF-8-based N-doped graphite material preparation method

Through in-situ liquid phase TEM characterization and high-temperature rapid carbonization method, the observation problems of ZIF-8 nucleation growth process and the problem of insufficient low-temperature discharge capacity of graphite materials were solved, and N doping with high discharge specific capacity and good rate performance was prepared. Graphite material improves the cycle stability of lithium-ion batteries.

CN119064637APending Publication Date: 2024-12-03HEFEI UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410338606.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The prior art cannot observe the nucleation and growth process of ZIF-8 in real time in solution, which limits the study of its morphological control and growth kinetics. The discharge capacity of graphite negative electrode materials is insufficient at low temperatures, and the traditional carbonization method consumes a large energy consumption. Long time.

Method used

In situ liquid phase TEM characterization method is used to observe the nucleation and growth process of ZIF-8 in real time, and prepare N-doped graphite materials through high-temperature rapid carbonization method to achieve a carbonization process with short sintering time and low energy consumption.

Benefits of technology

Real-time observation of the ZIF-8 nucleation growth process was achieved, and N-doped graphite materials with high discharge specific capacity and good rate performance were prepared, which improved the cycle stability of lithium-ion batteries at room temperature, low temperature and high temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119064637A_ABST
    Figure CN119064637A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of battery preparation, and relates to a ZIF-8 in-situ characterization method and a ZIF-8-based N-doped graphite material preparation method, the method comprises the following steps: S1, preparing a zinc acetate dihydrate solution and a 2-methylimidazole solution; s2, mixing and stirring the zinc acetate dihydrate solution prepared in the step S1 with a 2-methylimidazole solution for 20 seconds, and then standing for 24 hours to obtain a solution after standing; s3, carrying out centrifugal washing on the solution obtained after standing in the step S2, so as to obtain centrifuged ZIF-8; s4, putting the centrifuged ZIF-8 into an air blast drying oven at 55 DEG C, and drying, so as to obtain dried ZIF-8; and S5, carrying out high-temperature rapid carbonization on the dried ZIF-8 to obtain the N-doped graphite material. The change of ZIF-8 particles in the reaction liquid can be observed in real time, meanwhile, the high-temperature rapid carbonization method is low in energy consumption and short in time, the obtained N-doped graphite material has N-doped defects and a 3D structure, and the performance of a lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of battery preparation, and specifically relates to an in-situ characterization method of ZIF-8 and a method for preparing N-doped graphite material based on ZIF-8. Background Art

[0002] At present, the synthesis method of ZIF-8 is relatively mature. By controlling certain experimental parameters such as precursor solution concentration, reaction temperature, reaction time, etc. to adjust the nucleation and growth of nanocrystals, ZIF-8 with specific morphology and size is successfully synthesized. However, the growth mode of ZIF-8 is still unclear. The main experimental obstacle is that the nucleation and growth process of ZIF-8 cannot be observed in situ in the solution, that is, the physical and chemical processes occurring in the nucleation and growth of ZIF-8 cannot be observed in real time. Only relying on some traditional characterization methods, due to the discontinuity of information obtained from one reaction point to another, the intermediate reaction process is like a dark box operation, which greatly limits the research on the related basic theories such as ZIF-8 nucleation and growth mechanism, morphology control mechanism and growth kinetics. Therefore, how to observe the growth of ZIF-8 from a microscopic scale is the key to solving the above problems.

[0003] As the negative electrode material of lithium secondary batteries, graphite has a relatively low and stable lithium insertion platform. When used as a negative electrode, it has the advantages of good cycle stability and abundant resources, making graphite a commercial lithium negative electrode material. However, the graphite negative electrode has a low theoretical specific capacity and can hardly release capacity at low temperatures. In order to solve these problems, some researchers have modified graphite. They found that N-doped graphite has a high discharge specific capacity and good rate performance. The carbonized ZIF-8 itself is an N-doped graphite structure, and its 3D structure can increase the Li + However, the current carbonization method is to sinter in the atmosphere for a long time, which consumes a lot of energy and takes a long time. Therefore, how to achieve a sintering method with short sintering time and low energy consumption is the key to solving the above problems. Summary of the invention

[0004] The purpose of the present application is to provide an in-situ characterization method of ZIF-8 and a method for preparing N-doped graphite material based on ZIF-8, which can observe the physical and chemical processes occurring in the nucleation and growth of ZIF-8 in real time in situ in the solution, and provide a high-temperature rapid carbonization method with short sintering time and low energy consumption.

[0005] In a first aspect, the present application provides an in situ characterization method of ZIF-8, comprising the following steps:

[0006] Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution;

[0007] Step S2: taking out the first graphene copper mesh, and dropping the zinc acetate dihydrate solution and 2-methylimidazole solution described in step S1 onto the first graphene copper mesh;

[0008] Step S3: taking out the second graphene copper mesh, and covering the second graphene copper mesh on the first graphene copper mesh to obtain a packaged ZIF-8 sample;

[0009] Step S4: placing the packaged ZIF-8 sample into a TEM to obtain in-situ liquid phase characterization results of ZIF-8.

[0010] In a second aspect, the present application provides a method for preparing an N-doped graphite material based on ZIF-8, comprising the following steps:

[0011] Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution;

[0012] Step S2: mixing the zinc acetate dihydrate solution prepared in step S1 with the 2-methylimidazole solution and stirring for 20 seconds, and then standing for 24 hours to obtain a solution after standing;

[0013] Step S3: centrifugally washing the solution after standing in step S2 to obtain ZIF-8 after centrifugation;

[0014] Step S4: placing the centrifuged ZIF-8 in a 55° C. forced air drying oven for drying to obtain dried ZIF-8;

[0015] Step S5: rapidly carbonizing the dried ZIF-8 at high temperature to obtain N-doped graphite material.

[0016] In a possible implementation manner, step S5 includes:

[0017] Step S501: a fixed object is arranged on a surface of a substrate, and the dried ZIF-8 is placed between the fixed object and the substrate;

[0018] Step S502: Arranging electrodes on the other surface of the substrate, wherein the electrodes include a positive electrode and a negative electrode arranged at intervals;

[0019] Step S503: placing the fixed part, substrate, ZIF-8 and electrodes into a housing and sealing the housing;

[0020] Step S504: Argon gas is introduced into the shell to fill the shell with argon gas atmosphere, a current of appropriate magnitude is selected to energize the electrodes, and the dried ZIF-8 is rapidly carbonized at high temperature to obtain N-doped graphite material.

[0021] In a possible implementation manner, the substrate is graphite felt.

[0022] In a possible implementation manner, the contact area between the electrode and the substrate is as large as possible.

[0023] In a possible implementation manner, the high temperature rapid carbonization temperature is 800° C. and is kept at this temperature for 20 seconds.

[0024] In a possible implementation manner, after step S5, the following step is further included:

[0025] Step S6: taking out the first graphene copper mesh, and placing the N-doped graphite material described in step S5 on the first graphene copper mesh;

[0026] Step S7: taking out the second graphene copper mesh, and covering the second graphene copper mesh on the first graphene copper mesh to obtain a packaged N-doped graphite material sample;

[0027] Step S8: placing the packaged N-doped graphite material sample into a TEM to obtain an in-situ characterization result of the N-doped graphite material.

[0028] In a third aspect, the present application provides a negative electrode plate, wherein the negative electrode plate comprises an N-doped graphite material prepared by the method described in the second aspect.

[0029] In a fourth aspect, the present application provides a method for preparing a negative electrode sheet as described in the third aspect, comprising: mixing the N-doped graphite material, the conductive agent super P and the binder sodium alginate in a ratio of 8:1:1, then adding an appropriate amount of deionized water for ball milling, uniformly coating the obtained slurry on a copper foil, and then drying at 55°C to obtain an N-doped graphite negative electrode sheet.

[0030] In a fifth aspect, the present application provides a secondary battery, wherein the secondary battery comprises the negative electrode plate as described in the third aspect.

[0031] Compared with the prior art, the present application obtains N-doped ZIF-8 derivatives by observing the growth process of ZIF-8 and high-temperature rapid sintering through in-situ liquid phase TEM. The in-situ liquid phase TEM characterization method of the present application directly drips the solution before the reaction into the graphene copper mesh for encapsulation, and can observe the changes of ZIF-8 particles in the reaction solution in real time, which plays an important role in ZIF-8 morphology control and reaction kinetics research. The high-temperature rapid carbonization method of the present application has low energy consumption, short time and green environmental protection. N-doped graphite material can be obtained by high-temperature rapid carbonization of ZIF-8. The N-doped graphite material has N-doping defects and 3D structure. The synergistic effect of the two improves the performance of lithium-ion batteries, so that it can be stably cycled at room temperature, low temperature and high temperature.

[0032] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application so that it can be implemented in accordance with the contents of the specification, and to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the following is a detailed description of the preferred embodiments of the present application in conjunction with the accompanying drawings as follows.

[0033] Based on the detailed description of the specific embodiments of the present application in combination with the accompanying drawings below, those skilled in the art will become more aware of the above and other objects, advantages and features of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions in the embodiments of the present application or the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can also be obtained based on these drawings without creative work. In all drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, each element or part is not necessarily drawn according to the actual scale.

[0035] Figure 1 A schematic diagram of a process for in-situ characterization of ZIF-8 provided in this application;

[0036] Figure 2 The transmission electron microscopy image of ZIF-8 obtained by in-situ liquid phase observation provided in this application;

[0037] Figure 3 A schematic diagram of a process for preparing an N-doped graphite material based on ZIF-8 provided in this application;

[0038] Figure 4 This is a scanning electron microscope image of the N-doped graphite material obtained by in-situ observation provided in this application;

[0039] Figure 5 XPS element characterization of each secondary battery provided in this application;

[0040] Figure 6 Cycle curves of each secondary battery provided in this application at room temperature;

[0041] Figure 7 The rate curves of the secondary batteries provided in this application at room temperature;

[0042] Figure 8 Cycle curves of each secondary battery at low temperature provided in this application;

[0043] Fig. 9 The following are the cycle curves of the secondary batteries under high temperature provided in this application. DETAILED DESCRIPTION

[0044] To make the purpose, technical scheme and advantages of the embodiment of the present application clearer, the technical scheme in the embodiment of the present application will be clearly and completely described below in conjunction with the accompanying drawings in the embodiment of the present application. Obviously, the described embodiment is a part of the embodiment of the present application, rather than all of the embodiments. In the following description, specific details such as specific configuration and components are provided only to help fully understand the embodiments of the present application. Therefore, it should be clear to those skilled in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present application. In addition, for clarity and brevity, the description of known functions and structures is omitted in the embodiment.

[0045] It should be understood that the references to "one embodiment" or "this embodiment" throughout the specification mean that the specific features, structures, or characteristics associated with the embodiment are included in at least one embodiment of the present application. Therefore, the references to "one embodiment" or "this embodiment" appearing throughout the specification do not necessarily refer to the same embodiment. In addition, these specific features, structures, or characteristics may be combined in any suitable manner in one or more embodiments.

[0046] In addition, the present application may repeat reference numerals and / or letters in different examples. This repetition is for the purpose of simplicity and clarity, and does not in itself indicate the relationship between the various embodiments and / or settings discussed.

[0047] The term "and / or" in this article is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, B exists alone, and A and B exist at the same time. The term " / and" in this article describes another type of association object relationship, indicating that there can be two relationships. For example, A / and B can mean: A exists alone, and A and B exist alone. In addition, the character " / " in this article generally indicates that the previous and next associated objects are in an "or" relationship.

[0048] The term "at least one" in this article is merely a description of the association relationship of associated objects, indicating that there may be three relationships. For example, at least one of A and B can mean: A exists alone, A and B exist at the same time, and B exists alone.

[0049] It should also be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusions.

[0050] Example 1

[0051] A ZIF-8 in-situ characterization method of the present embodiment, such as Figure 1 As shown, the method comprises the following steps:

[0052] Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution.

[0053] Specifically, 0.3 g of zinc acetate dihydrate was added to 5 ml of deionized water to prepare a zinc acetate dihydrate solution; 1.12 g of 2-methylimidazole was added to 5 ml of deionized water to prepare a 2-methylimidazole solution.

[0054] Step S2: Take out the first graphene copper mesh, and drop the zinc acetate dihydrate solution and 2-methylimidazole solution described in step S1 onto the first graphene copper mesh.

[0055] Step S3: Take out the second graphene copper mesh, and cover the second graphene copper mesh on the first graphene copper mesh to obtain a packaged ZIF-8 sample.

[0056] Step S4: placing the packaged ZIF-8 sample into a TEM to obtain in-situ liquid phase characterization results of ZIF-8.

[0057] Figure 2 This is the transmission electron microscopy image of ZIF-8 obtained by in-situ liquid phase observation. Figure 2 It can be seen that with the increase of time, some small particles aggregate on the surface of the nucleated ZIF-8, causing the area of ​​ZIF-8 to gradually increase.

[0058] Example 2

[0059] A method for preparing an N-doped graphite material based on ZIF-8 in this embodiment is as follows: Figure 3 As shown, the method comprises the following steps:

[0060] Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution.

[0061] Specifically, 0.3 g of zinc acetate dihydrate was added to 5 ml of deionized water to prepare a zinc acetate dihydrate solution; 1.12 g of 2-methylimidazole was added to 5 ml of deionized water to prepare a 2-methylimidazole solution.

[0062] Step S2: The zinc acetate dihydrate solution prepared in step S1 and the 2-methylimidazole solution are mixed and stirred for 20 seconds, and then allowed to stand for 24 hours to obtain a solution after standing.

[0063] Step S3: The solution after standing in step S2 is centrifuged and washed to obtain ZIF-8 after centrifugation.

[0064] Step S4: placing the centrifuged ZIF-8 in a 55° C. forced air drying oven for drying to obtain dried ZIF-8.

[0065] Step S5: rapidly carbonizing the dried ZIF-8 at high temperature to obtain N-doped graphite material.

[0066] The step S5 comprises:

[0067] Step S501: a fixed part is arranged on one surface of a substrate, and 1.2 g of the dried ZIF-8 is placed between the fixed part and the substrate; the substrate is graphite felt.

[0068] Step S502: Arranging electrodes on the other surface of the substrate, the electrodes comprising a positive electrode and a negative electrode arranged at intervals; the contact area between the electrodes and the substrate is as large as possible to ensure that the current can flow evenly through the graphite felt, making the temperature field uniform.

[0069] Step S503: putting the fixed part, substrate, ZIF-8 and electrodes into a shell and sealing it.

[0070] Step S503: Argon gas is introduced into the housing to fill the housing with argon gas atmosphere, and a suitable current is selected to energize the electrodes to perform high-temperature rapid carbonization on the dried ZIF-8 to obtain N-doped graphite material. A suitable current is selected to raise the temperature required for high-temperature rapid carbonization of ZIF-8 to 800°C, and the temperature is kept for 20 seconds, and then the temperature is naturally cooled to obtain 0.4g N-doped graphite material, named URS-800°C.

[0071] Step S6: taking out the first graphene copper mesh, and placing the N-doped graphite material described in step S5 on the first graphene copper mesh;

[0072] Step S7: taking out the second graphene copper mesh, and covering the second graphene copper mesh on the first graphene copper mesh to obtain a packaged N-doped graphite material sample;

[0073] Step S8: placing the packaged N-doped graphite material sample into a TEM to obtain an in-situ characterization result of the N-doped graphite material.

[0074] Figure 4 This is the SEM image of N-doped graphite material obtained by in-situ observation. Figure 4 It can be seen that after high-temperature rapid carbonization, ZIF-8 still maintains the original ZIF-8 skeleton, with some shrinkage on the surface, and the N-doped graphite sintered by high-temperature rapid carbonization method is uniform in size.

[0075] Comparative Example 1

[0076] Step S1: Same as Example 2.

[0077] Step S2: Same as Example 2.

[0078] Step S3: Same as Example 2.

[0079] Step S4: Same as Example 2.

[0080] Step S5: After the dried 1g ZIF-8 is placed in a tubular furnace with an argon atmosphere, the temperature is increased from 25°C to 800°C at a heating rate of 2°C / min, and the temperature is kept at 800°C for 2h, followed by natural cooling to obtain 0.5g N-doped graphite material, named ZIF-8-800°C.

[0081] The N-doped graphite material obtained in Example 2 and the N-doped graphite material in Comparative Example 1 were used to prepare negative electrode sheets and secondary batteries respectively according to the following methods.

[0082] Preparation of negative electrode sheet using N-doped graphite material:

[0083] The N-doped graphite material, the conductive agent super P and the binder sodium alginate were mixed in a ratio of 8:1:1, and then an appropriate amount of deionized water was added for ball milling. The obtained slurry was evenly coated on the copper foil and then dried at 55°C to obtain the N-doped graphite negative electrode sheet.

[0084] Use lithium sheet as counter electrode, and assemble with N-doped graphite negative electrode sheet, electrolyte and separator into secondary battery:

[0085] (1) At room temperature, ethylene carbonate and diethyl carbonate were mixed in a mass ratio of 1:1, and LiPF 6 , after fully mixing, let stand for 24 hours to obtain an electrolyte;

[0086] (2) punching the ceramic-coated polyethylene material into a disc with a diameter of 16 mm, transferring it to a vacuum drying oven at 55° C., and vacuum drying it for 24 h to obtain a diaphragm;

[0087] (3) In a glove box where the water and oxygen content is less than 0.1 ppm, a lithium sheet is used as a counter electrode and assembled into a secondary battery with an N-doped graphite negative electrode sheet, the electrolyte obtained in step (1), and the diaphragm obtained in step (2).

[0088] The electrochemical performance of each secondary battery assembled in the above secondary battery embodiment was tested respectively, and the test conditions were as follows:

[0089] The Neware test system was used to test each secondary battery, and the following three test parameters were set for testing:

[0090] (1) The charge and discharge voltage range is 0.01 to 3 V, the temperature is 25°C, and the cycle is 200 times at 0.5 A / g;

[0091] (2) The charge and discharge voltage range is 0.01 to 3 V, the temperature is -20°C, and the cycle is 200 times at 0.2 A / g;

[0092] (3) The charge and discharge voltage range is 0.01 to 3 V, the temperature is 70°C, and the cycle is 200 times at 0.2 A / g.

[0093] The Neware test system was used to perform high-rate performance tests on secondary batteries with a voltage range of 0.01 to 3 V and a current density of 0.1 A / g-0.2 A / g-0.5 A / g-1 A / g-2 A / g-4 A / g-0.2 A / g.

[0094] The EDX characterization of Example 2 and Comparative Example 1 is shown in Table 1, and the XPS element characterization is shown in Figure 5 The EDX element contents in Table 1 are compared with Figure 5 From the XPS element content, it can be seen that the N content of the sample after high-temperature rapid sintering is higher.

[0095] Table 1:

[0096] Sample name C (wt%) N (wt%) O(wt%) Zn (wt%) Example 2 33.88 24.34 7.64 34.14 Comparative Example 1 47.89 19.33 6.12 26.67

[0097] From the test results of Example 1, Example 6 and Comparative Example 1 in Table 1, it can be seen that the capacity retention rate of the waste lithium iron phosphate positive electrode material of Comparative Example 1 after 100 cycles at 1C current density is only 87%, while the capacity retention rate of the lithium iron phosphate positive electrode material of Example 1 and Example 6 after 100 cycles at 1C current density is above 90%. The RLFP-80℃ / 6h of Example 1 has a capacity of 125.1mAh·g after 100 cycles at 1C current density. -1 The discharge capacity of the RLFP-700℃ / 2h obtained after short-time annealing at 1C current density after 100 cycles is 135.34mAh·g -1 The discharge specific capacity is as high as 97%, and the capacity retention rate is as high as 97%. It can be seen that the lithium iron phosphate positive electrode material regenerated by the low-temperature liquid phase method has good electrochemical properties, and the electrochemical properties of the lithium iron phosphate positive electrode material obtained by the low-temperature liquid phase method combined with short-time annealing are further improved.

[0098] The results of the performance tests on each secondary battery are as follows: Figure 6-Figure 9 shown.

[0099] Figure 6 is the cycle curve of each secondary battery at room temperature, Figure 6It can be seen that the URS-800℃ battery after high-temperature rapid carbonization has a higher discharge specific capacity than the ZIF-8-800℃ battery after tubular furnace carbonization, and the capacity remains at 453mAh / g after 200 cycles. This is mainly because the higher content of pyridinic nitrogen and pyrrolic nitrogen in the URS-800℃ sample can provide more active sites for lithium-ion batteries, thereby improving the performance of the battery.

[0100] Figure 7 is the rate performance curve of each secondary battery at room temperature, Figure 7 It can be seen that the discharge specific capacity of URS-800℃ after high-temperature rapid carbonization can still be maintained at 235mAh / g after cycling at a high current density of 4A / g, which shows that the rapidly sintered URS-800℃ sample has more advantages as a negative electrode for lithium-ion batteries.

[0101] Figure 8 is the cycle curve of each secondary battery at -20℃ low temperature, Figure 8 It can be seen that the URS-800℃ after high-temperature rapid carbonization can still stably cycle at a current density of 0.2A / g at low temperature, and the discharge specific capacity is maintained at 268mAh / g after 200 cycles. This is mainly because the N-doped graphite material obtained by this high-temperature rapid carbonization has a 3D structure and N-doping defects, which can provide more sites for lithium ion transmission, alleviate the disadvantage of slow lithium ion transmission at low temperatures, and enable it to stably cycle at low temperatures.

[0102] Fig. 9 is the cycle curve of each secondary battery at 70℃. Fig. 9 It can be seen that the URS-800℃ after high temperature rapid carbonization can still be stably cycled at a current density of 0.2A / g at high temperature, and the discharge specific capacity is maintained at 847mAh / g after 40 cycles. This is mainly because the N-doped graphite material obtained by this high temperature rapid carbonization in the present application has a 3D structure, and the structure will not be destroyed during the cycle, reducing the generation of side reactions during the cycle of the battery, thereby stabilizing the cycle.

[0103] The present application obtains N-doped ZIF-8 derivatives by observing the growth process of ZIF-8 and high-temperature rapid sintering through in-situ liquid phase TEM. The in-situ liquid phase TEM characterization method of the present application directly drips the solution before the reaction into the graphene copper mesh for encapsulation, and can observe the changes of ZIF-8 particles in the reaction solution in real time, which plays an important role in ZIF-8 morphology control and reaction kinetics research. The high-temperature rapid carbonization method of the present application has low energy consumption, short time and green environmental protection. N-doped graphite material can be obtained by high-temperature rapid carbonization of ZIF-8. The N-doped graphite material has N-doping defects and 3D structure. The synergistic effect of the two can increase the transmission sites of lithium ions on the material, thereby improving the discharge specific capacity and cycle stability of the battery, so that it can be stably cycled at room temperature, low temperature and high temperature, and improves the performance of lithium-ion batteries.

[0104] The above is only the preferred embodiment of the present application, which does not limit the protection scope of the present application. For those skilled in the art, the present application may have various changes and modifications. Within the spirit and principle of the present application, the changes, modifications, replacements, integrations and parameter changes of these embodiments by conventional substitutions or capable of achieving the same functions without departing from the principles and spirit of the present application shall fall within the protection scope of the present application.

Claims

1. An in situ characterization method for ZIF-8, It is characterized in that include: Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution; Step S2: taking out the first graphene copper mesh, and dropping the zinc acetate dihydrate solution and 2-methylimidazole solution described in step S1 onto the first graphene copper mesh; Step S3: taking out the second graphene copper mesh, and covering the second graphene copper mesh on the first graphene copper mesh to obtain a packaged ZIF-8 sample; Step S4: placing the packaged ZIF-8 sample into a TEM to obtain in-situ liquid phase characterization results of ZIF-8.

2. A method for preparing N-doped graphite material based on ZIF-8, It is characterized in that include: Step S1: preparing zinc acetate dihydrate solution and 2-methylimidazole solution; Step S2: mixing the zinc acetate dihydrate solution prepared in step S1 with the 2-methylimidazole solution and stirring for 20 seconds, and then standing for 24 hours to obtain a solution after standing; Step S3: centrifugally washing the solution after standing in step S2 to obtain ZIF-8 after centrifugation; Step S4: placing the centrifuged ZIF-8 in a 55° C. forced air drying oven for drying to obtain dried ZIF-8; Step S5: rapidly carbonizing the dried ZIF-8 at high temperature to obtain N-doped graphite material.

3. A method for preparing an N-doped graphite material based on ZIF-8 according to claim 2, It is characterized in that The step S5 comprises: Step S501: a fixed object is arranged on a surface of a substrate, and the dried ZIF-8 is placed between the fixed object and the substrate; Step S502: Arranging electrodes on the other surface of the substrate, wherein the electrodes include a positive electrode and a negative electrode arranged at intervals; Step S503: placing the fixed part, substrate, ZIF-8 and electrodes into a housing and sealing the housing; Step S504: Argon gas is introduced into the shell to fill the shell with argon gas atmosphere, a current of appropriate magnitude is selected to energize the electrodes, and the dried ZIF-8 is rapidly carbonized at high temperature to obtain N-doped graphite material.

4. A method for preparing an N-doped graphite material based on ZIF-8 according to claim 3, It is characterized in that The substrate is graphite felt.

5. A method for preparing an N-doped graphite material based on ZIF-8 according to claim 3, It is characterized in that The contact area between the electrode and the substrate is as large as possible.

6. A method for preparing an N-doped graphite material based on ZIF-8 according to claim 3, It is characterized in that The temperature of the high-temperature rapid carbonization is 800° C., and the temperature is kept for 20 seconds.

7. A method for preparing an N-doped graphite material based on ZIF-8 according to claim 2, It is characterized in that After step S5, the method further includes: Step S6: taking out the first graphene copper mesh, and placing the N-doped graphite material described in step S5 on the first graphene copper mesh; Step S7: taking out the second graphene copper mesh, and covering the second graphene copper mesh on the first graphene copper mesh to obtain a packaged N-doped graphite material sample; Step S8: placing the packaged N-doped graphite material sample into a TEM to obtain an in-situ characterization result of the N-doped graphite material.

8. A negative electrode sheet, It is characterized in that The negative electrode plate comprises an N-doped graphite material obtained by the method as described in any one of claims 2 to 7.

9. A method for preparing a negative electrode sheet according to claim 8, It is characterized in that The N-doped graphite material, the conductive agent super P and the binder sodium alginate were mixed in a ratio of 8:1:1, and then an appropriate amount of deionized water was added for ball milling. The obtained slurry was evenly coated on a copper foil and then dried at 55° C. to obtain an N-doped graphite negative electrode sheet.

10. A secondary battery, It is characterized in that The battery comprises the negative electrode sheet as claimed in claim 8.

Citation Information

Cited By

  • Preparation method of graphite composite negative electrode material of lithium ion battery

    CN119943906A