Processing method of electrochromic film

By combining the steps of stirring, laser treatment, electrostatic spraying and drying, the problems of slow speed, poor stability and large color difference in electrochromic film preparation are solved, and efficient and stable film preparation is achieved.

CN119065168APending Publication Date: 2024-12-03ANHUI SCI & TECH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411370233.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing electrochromic film preparation process has problems such as slow speed, poor stability and large color difference.

Method used

Using the steps of mixing processing, laser treatment, electrostatic spraying and drying, the electrochromic material mixture is dissolved through a stirring device, the metal film is portrayed using a pulsed laser, and the polymer composite electrochromic solution is deposited, and multiple drying is performed. Processed to form a stable electrochromic film.

Benefits of technology

The stability and color difference uniformity of electrochromic films are improved, the processing process is simplified, and efficient film preparation is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119065168A_ABST
    Figure CN119065168A_ABST
Patent Text Reader

Abstract

The invention discloses an electrochromic film processing method which specifically comprises the following steps: S1, mixing and processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring through stirring equipment to dissolve the electrochromic material mixed solution to obtain a polymer solution; the polymer composite electrochromic solution of the electrochromic material is obtained; s2, laser treatment; s3, electrostatic spraying is conducted; s4, drying treatment; the invention relates to the technical field of electrochromic materials. According to the processing method of the electrochromic film, stirring is carried out through stirring equipment, so that the electrochromic material mixed solution is dissolved, a polymer composite electrochromic solution of the electrochromic material is obtained, solutes in the solution can be mixed evenly, the color difference of the electrochromic film is reduced, and the electrochromic film can be obtained through multiple times of electrostatic spraying. The processed electrochromic film is high in stability, and meanwhile the whole method is simple and efficient in process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electrochromic materials, in particular to a processing method of an electrochromic film. Background Art

[0002] Electrochromic materials have outstanding controllability, environmental friendliness, high optical contrast, and great potential in the field of flexible devices and smart wearables. In addition, related devices using electrical stimulation methods or relying on electrical energy have great room for development in the future. Therefore, electrochromic materials have received extensive attention and development in recent years. At present, electrochromic materials and related devices have been used in smart windows, optical blinds, car rearview mirrors, sunglasses, reflective displays, flexible displays, and smart wearables. In a broad sense, electrochromism is the phenomenon that a material undergoes a macroscopically reversible color change under the influence of an external voltage.

[0003] The performance of electrochromic films is determined by the material properties and preparation process, but there is little research on the process in the prior art. The electrochromic films prepared by traditional methods still have the problems of slow speed, poor stability and large color difference.

[0004] Therefore, the present invention provides a method for processing an electrochromic film to solve the above-mentioned problems. Summary of the invention

[0005] In view of the deficiencies of the prior art, the present invention provides a method for processing an electrochromic film, which solves the problems mentioned in the above background technology.

[0006] To achieve the above objectives, the present invention is implemented by the following technical solutions: A method for processing an electrochromic film, specifically comprising the following steps:

[0007] S1, mixing processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring the electrochromic material mixed solution by a stirring device to dissolve the electrochromic material mixed solution, to obtain a polymer composite electrochromic solution of the electrochromic material;

[0008] S2, laser processing: preparing an ITO film and a metal film, and using a pulsed laser to carve the metal film on the ITO film;

[0009] S3, electrostatic spraying: electrostatic spraying is performed by electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate to obtain an initial electrochromic film;

[0010] S4, drying treatment: drying the initial electrochromic film in step S3, and after drying, electrostatic spraying is performed again through electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate again to form a stable electrochromic film.

[0011] Furthermore, in step S1, the stirring device continues stirring for 20-30 minutes, and the rotation speed of the stirring device is controlled at 100-160 r / min.

[0012] Furthermore, the polymer solution needs to be deoxygenated before use.

[0013] Furthermore, the electrochromic material is specifically an inorganic electrochromic material, preferably tungsten trioxide.

[0014] Furthermore, the polymer solution is prepared by dissolving a polymer in a solvent, wherein the polymer includes one or more of polymethyl methacrylate, polyvinyl alcohol, and polyurethane, and the solvent includes one or more of methanol, acetone, acetonitrile, and tetrahydrofuran.

[0015] Furthermore, the drying temperature in step S4 is 40-50° C., and the drying time is 10-20 min.

[0016] Furthermore, the model of the electrostatic spraying equipment in step S3 and step S4 is MY-801.

[0017] Beneficial Effects

[0018] The present invention provides a method for processing an electrochromic film. Compared with the prior art, the present invention has the following advantages:

[0019] Beneficial effects:

[0020] The processing method of the electrochromic film comprises the following steps: stirring the electrochromic material mixture by a stirring device to dissolve the electrochromic material mixture, obtaining a polymer composite electrochromic solution of the electrochromic material, so that the solutes in the solution can be mixed evenly, reducing the color difference of the electrochromic film, and performing electrostatic spraying multiple times to make the processed electrochromic film highly stable. Meanwhile, the entire method process is simple and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The present invention is a flow chart of the method. DETAILED DESCRIPTION

[0022] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] See also Figure 1 The present invention provides three technical solutions: specifically the following embodiments:

[0024] Example 1

[0025] A method for processing an electrochromic film comprises the following steps:

[0026] S1, mixing processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring the electrochromic material mixed solution by a stirring device to dissolve the electrochromic material mixed solution, thereby obtaining a polymer composite electrochromic solution of the electrochromic material;

[0027] S2, laser processing: prepare the ITO film and the metal film, and use a pulsed laser to carve the metal film on the ITO film;

[0028] S3, electrostatic spraying: electrostatic spraying is performed by electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate to obtain an initial electrochromic film;

[0029] S4, drying treatment: drying the initial electrochromic film in step S3, and after drying, electrostatic spraying is performed again through electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate again to form a stable electrochromic film.

[0030] In this embodiment, in step S1, the stirring device continues stirring for 20 minutes, and the rotation speed of the stirring device is controlled at 100 r / min.

[0031] In this embodiment, the electrochromic material is specifically an inorganic electrochromic material, preferably tungsten trioxide.

[0032] In this embodiment, the polymer solution is prepared by dissolving a polymer in a solvent, the polymer includes one or more of polymethyl methacrylate, polyvinyl alcohol, and polyurethane, and the solvent includes one or more of methanol, acetone, acetonitrile, and tetrahydrofuran.

[0033] In this embodiment, the drying temperature in step S4 is 40° C. and the drying time is 10 minutes.

[0034] Example 2

[0035] S1, mixing processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring the electrochromic material mixed solution by a stirring device to dissolve the electrochromic material mixed solution, thereby obtaining a polymer composite electrochromic solution of the electrochromic material;

[0036] S2, laser processing: prepare the ITO film and the metal film, and use a pulsed laser to carve the metal film on the ITO film;

[0037] S3, electrostatic spraying: electrostatic spraying is performed by electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate to obtain an initial electrochromic film;

[0038] S4, drying treatment: drying the initial electrochromic film in step S3, and after drying, electrostatic spraying is performed again through electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate again to form a stable electrochromic film.

[0039] In this embodiment, in step S1, the stirring device continues stirring for 25 minutes, and the rotation speed of the stirring device is controlled at 130 r / min.

[0040] In this embodiment, the electrochromic material is specifically an inorganic electrochromic material, preferably tungsten trioxide.

[0041] In this embodiment, the polymer solution is prepared by dissolving a polymer in a solvent, the polymer includes one or more of polymethyl methacrylate, polyvinyl alcohol, and polyurethane, and the solvent includes one or more of methanol, acetone, acetonitrile, and tetrahydrofuran.

[0042] In this embodiment, the drying temperature in step S4 is 45° C. and the drying time is 15 minutes.

[0043] Example 3

[0044] S1, mixing processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring the electrochromic material mixed solution by a stirring device to dissolve the electrochromic material mixed solution, thereby obtaining a polymer composite electrochromic solution of the electrochromic material;

[0045] S2, laser processing: prepare the ITO film and the metal film, and use a pulsed laser to carve the metal film on the ITO film;

[0046] S3, electrostatic spraying: electrostatic spraying is performed by electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate to obtain an initial electrochromic film;

[0047] S4, drying treatment: drying the initial electrochromic film in step S3, and after drying, electrostatic spraying is performed again through electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate again to form a stable electrochromic film.

[0048] In this embodiment, in step S1, the stirring device continues stirring for 30 minutes, and the rotation speed of the stirring device is controlled at 160 r / min.

[0049] In this embodiment, the electrochromic material is specifically an inorganic electrochromic material, preferably tungsten trioxide.

[0050] In this embodiment, the polymer solution is prepared by dissolving a polymer in a solvent, the polymer includes one or more of polymethyl methacrylate, polyvinyl alcohol, and polyurethane, and the solvent includes one or more of methanol, acetone, acetonitrile, and tetrahydrofuran.

[0051] In this embodiment, the drying temperature in step S4 is 50° C. and the drying time is 20 minutes.

[0052] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0053] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0054] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for processing an electrochromic film, characterized in that: The specific steps include: S1, mixing processing: selecting an electrochromic material mixed solution, pouring the electrochromic material mixed solution into a corresponding polymer solution, and then stirring the electrochromic material mixed solution by a stirring device to dissolve the electrochromic material mixed solution, to obtain a polymer composite electrochromic solution of the electrochromic material; S2, laser processing: preparing an ITO film and a metal film, and using a pulsed laser to carve the metal film on the ITO film; S3, electrostatic spraying: electrostatic spraying is performed by electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate to obtain an initial electrochromic film; S4, drying treatment: drying the initial electrochromic film in step S3, and after drying, electrostatic spraying is performed again through electrostatic spraying equipment to deposit the polymer composite electrochromic solution in step S1 on the surface of the metal film substrate again to form a stable electrochromic film.

2. The method for processing an electrochromic film according to claim 1, characterized in that: In step S1, the stirring device continues stirring for 20-30 minutes, and the rotation speed of the stirring device is controlled at 100-160 r / min.

3. The method for processing an electrochromic film according to claim 1, characterized in that: The polymer solution needs to be deoxygenated before use.

4. The method for processing an electrochromic film according to claim 1, characterized in that: The electrochromic material is specifically an inorganic electrochromic material, preferably tungsten trioxide.

5. The method for processing an electrochromic film according to claim 1, characterized in that: The polymer solution is prepared by dissolving a polymer in a solvent, wherein the polymer includes one or more of polymethyl methacrylate, polyvinyl alcohol, and polyurethane, and the solvent includes one or more of methanol, acetone, acetonitrile, and tetrahydrofuran.

6. The method for processing an electrochromic film according to claim 1, characterized in that: The drying temperature in step S4 is 40-50° C. and the drying time is 10-20 min.

7. The method for processing an electrochromic film according to claim 1, characterized in that: The model of the electrostatic spraying equipment in step S3 and step S4 is MY-801.

Citation Information

Patent Citations

  • Method for preparing electrochromic film and an electrochromic device

    CN106371258A

  • Porous electrochromic film and preparation method thereof, polychromatic electrochromic film and preparation method thereof, and electrochromic device and preparation method thereof

    CN111474792A

  • Electrochromic device

    EP0682284A2