Preparation method of composite conductor
The method of using grooves and protrusions to horizontally move the conductive layers in the composite conductor preparation process addresses the issue of graphene agglomeration, ensuring uniform distribution and improved conductivity.
Patent Information
- Application Number
- CN202310638950.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
AI Technical Summary
Existing methods for preparing composite conductors with graphene and copper face challenges in maintaining uniform and stable distribution of graphene layers due to agglomeration and disordered redistribution during the pressing process, leading to reduced conductivity.
A method involving a first and second conductive layer with a graphene layer in between, utilizing driving mechanisms with grooves and protrusions to horizontally move the first conductive layer, preventing agglomeration and redistributing disordered graphene, ensuring orderly distribution.
Improves the conductivity of the composite conductor by preventing graphene agglomeration and reordering disordered graphene layers, enhancing the structural integrity and conductivity of the composite conductor.
Smart Images

Figure CN119069178A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of conductor technology, and in particular to a method for preparing a composite conductor. Background Art
[0002] Graphene has excellent properties such as high electrical conductivity, high thermal conductivity, high strength, high flexibility, strong chemical inertness, and excellent gas barrier properties. These properties make graphene have great application prospects in many aspects.
[0003] In the field of conductors, graphene is usually mixed with metal copper, silver, etc. to enhance the conductivity, wear resistance, corrosion resistance, etc. of the metal conductive layer. Taking copper as an example, the existing technology mainly uses two methods to prepare copper conductor materials after mixing graphene and copper. One is to press the copper powder and graphene after mixing, and the other is to deposit a graphene layer on the surface of the conductive base layer by CVD method, and then press the conductive base layers containing different graphene layers to form a copper plate, and then process it into other required materials. In the existing pressing of graphene conductive base layers, although graphene can be mixed into copper materials, in the process of extruding different conductive base layers with graphene deposited into copper plates, the graphene layer is easily affected by the extrusion force, causing part of the graphene to re-agglomerate to form graphite, or making the originally ordered graphene distributed again disordered, thereby affecting the overall conductive properties of the graphene conductive base mixed material. After uniform and ordered graphene is formed on the surface of the conductive base layer, during the extrusion process of the conductive base layer, the graphene layer separates the two conductive base layers to form a copper-graphene-copper contact relationship. Due to the characteristics of the molecular structure of graphene itself, it is difficult to form a strong bonding force between graphene and copper. Therefore, during the extrusion process between the conductive base layers, part of the conductive base layer surface will break through the graphene layer to form a copper-copper bond, thereby destroying the graphene layer structure and further affecting the conductivity of the copper-graphene mixed material.
[0004] Therefore, in the process of preparing metal-graphene hybrid conductors, how to ensure the uniform and stable distribution of the graphene layer during the processing needs to be further improved. Summary of the invention
[0005] In view of this, the present application provides a method for preparing a composite conductor, aiming to improve the problem that graphene in the conductive layer is difficult to be evenly and orderly distributed during the pressing process.
[0006] The embodiment of the present application is implemented as follows: a method for preparing a composite conductor comprises:
[0007] Providing a first conductive layer and a second conductive layer, wherein the first conductive layer includes a first conductive base layer and a first graphene layer deposited on the first conductive base layer;
[0008] The second conductive layer is superimposed on the first conductive layer, so that the first graphene layer is placed between the first conductive layer and the second conductive layer; the first conductive layer and the second conductive layer are provided with driving mechanisms that cooperate with each other;
[0009] The second conductive layer and the first conductive layer are pressed together along the thickness direction of the second conductive layer, and the surface of the first conductive layer on which the first graphene layer is deposited is driven to move horizontally to obtain a composite conductor.
[0010] Optionally, in some embodiments of the present application, the driving mechanism includes: a first groove and a second groove provided in the width direction of the first conductive layer, and a first protrusion corresponding to the first groove and a second protrusion corresponding to the second groove provided on the second conductive layer, wherein the first groove and the second groove are spaced apart, and the notches of the first groove and the second groove are located on the side of the first graphene layer away from the first conductive base layer.
[0011] Optionally, in some embodiments of the present application, a plurality of first grooves and a plurality of second grooves are provided, and the plurality of first grooves and the plurality of second grooves are arranged at intervals; a plurality of first protrusions and a plurality of second protrusions are provided, and the plurality of first protrusions correspond to the plurality of first grooves, and the plurality of second protrusions correspond to the plurality of second grooves.
[0012] Optionally, in some embodiments of the present application, the width of the end of the first protrusion is smaller than the width of the first groove, and when the first conductive layer is driven to move horizontally, the gap between the first protrusion and the first groove gradually decreases until the first protrusion and the first groove fit together.
[0013] Optionally, in some embodiments of the present application, the first conductive layer also includes a first electroplating layer, which is arranged on a side of the first graphene layer away from the first conductive base layer, and the first electroplating layer is one of a copper-graphene mixed layer, a silver-graphene mixed layer, a copper-silver-graphene mixed layer, or a copper-nickel-graphene mixed layer.
[0014] Optionally, in some embodiments of the present application, the sidewall of the second groove is connected to the sidewall of the first groove in the width direction of the first conductive layer.
[0015] Optionally, in some embodiments of the present application, the width of the second groove along the width direction of the first conductive layer decreases step by step along the depth direction of the second groove.
[0016] Optionally, in some embodiments of the present application, taking a plane perpendicular to the length direction of the first conductive layer as a cross-section, a cross-section of a sidewall of the second groove is V-shaped.
[0017] Optionally, in some embodiments of the present application, an angle ∠3 between the side wall of the second groove and the upper surface of the first conductive base layer is smaller than an angle ∠4 between the side wall of the second protrusion and the lower surface of the second conductive layer; wherein ∠4 satisfies 20°≤∠4≤70°.
[0018] Optionally, in some embodiments of the present application, the width of the second groove along the width direction of the first conductive layer increases step by step along the depth direction of the second groove.
[0019] Optionally, in some embodiments of the present application, taking a plane perpendicular to the length direction of the first conductive layer as a cross-section, a cross-section of a side wall of the second groove is in an inverted trapezoidal shape.
[0020] Optionally, in some embodiments of the present application, a second bump is convexly provided at the bottom of the second groove, and a second depression corresponding to the second bump is concavely provided at the end of the second protrusion.
[0021] Optionally, in some embodiments of the present application, the length of the second groove in the length direction of the first conductive layer is the same as the length of the first conductive layer; or
[0022] The first conductive layer has a plurality of second grooves in the length direction, the plurality of second grooves are spaced apart along the length direction of the first conductive layer, and the sum of the lengths of the plurality of second grooves is less than the length of the first conductive layer. The second conductive layer has a plurality of second protrusions in the length direction, and the plurality of second protrusions correspond one-to-one to the plurality of second grooves.
[0023] Optionally, in some embodiments of the present application, the first groove includes a first groove section and a second groove section arranged in sequence along its depth direction, the width of the first groove section is gradually reduced along the depth direction, the width of the second groove section is gradually expanded along the depth direction, and the width of the end of the first protrusion is smaller than the width at the connection between the first groove section and the second groove section.
[0024] Optionally, in some embodiments of the present application, an angle ∠1 between the side wall of the first slot segment and the upper surface of the first conductive base layer satisfies 80°≤∠1≤90°, and an angle ∠2 between the side wall of the second slot segment and the upper surface of the first conductive base layer satisfies 35°≤∠2≤60°.
[0025] Optionally, in some embodiments of the present application, a first bump is convexly provided at the bottom of the first groove, and a first depression corresponding to the first bump is concavely provided at the end of the first protrusion.
[0026] Optionally, in some embodiments of the present application, before laminating the second conductive layer and the first conductive layer, the steps include: introducing an inert gas after evacuating the vacuum; and heating the second conductive layer and the first conductive layer respectively so that the temperature of the second conductive layer is higher than the temperature of the first conductive layer.
[0027] Optionally, in some embodiments of the present application, the vacuum degree after evacuation is 1.2×10 -3 ~9.5×10 - 2 Pa;
[0028] The inert gas is one or more of nitrogen, argon and helium;
[0029] After the second conductive layer and the first conductive layer are heated respectively, the temperature of the second conductive layer is 40 to 80° C. higher than the temperature of the first conductive layer;
[0030] The lamination of the second conductive layer and the first conductive layer includes lamination under the following lamination conditions: a lamination temperature of 840 to 890° C.; a lamination pressure of 14 to 50 MPa; and a lamination time of 30 to 80 min.
[0031] In the preparation method of the composite conductor provided in the present application, during the lamination process of the first conductive layer and the second conductive layer, the driving mechanism causes the surface of the first conductive layer on which the first graphene layer is deposited to move horizontally, thereby avoiding graphene agglomeration and simultaneously causing the already agglomerated graphene to be peeled off and reformed into dispersed graphene, so that the disordered graphene is redistributed in an orderly manner under the action of mechanical force, thereby improving the conductivity of the composite conductor. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0033] Figure 1 It is a schematic diagram of the extrusion of the upper conductive base layer and the lower conductive base layer in the prior art;
[0034] Figure 2 is a flow chart of the preparation of the composite conductor provided in the embodiment of the present application;
[0035] Figure 3 is an exploded diagram of a composite conductor structure provided in an embodiment of the present application;
[0036] Figure 4 yes Figure 3 Cross-sectional view along direction A;
[0037] Figure 5 is a schematic structural diagram of a first conductive layer provided in an embodiment of the present application;
[0038] Figure 6 yes Figure 3 A cross-sectional view of the first conductive layer along direction A;
[0039] Figure 7 yes Figure 3 A cross-sectional view of the second conductive layer along direction A;
[0040] Figure 8is another exploded diagram of a composite conductor structure provided in an embodiment of the present application;
[0041] Fig. 9 is an exploded view of another composite conductor structure provided in an embodiment of the present application;
[0042] Fig.10 yes Fig. 9 A cross-sectional view of the first conductive layer along direction B;
[0043] Fig.11 yes Fig. 9 A cross-sectional view of the second conductive layer along direction B;
[0045] 11-upper conductive base layer; 12-lower conductive base layer; 21-upper graphene layer; 22-lower graphene layer;
[0046] 3-composite conductor, 31-first conductive layer; 311-first groove; 3111-first groove section; 3112-second groove section; 312-first protrusion; 313-second groove; 314-second protrusion; 32-second conductive layer; 321-first protrusion; 322-first depression; 323-second protrusion; 324-second depression. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0048] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0049] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0050] In the present application, "at least one" means one or more, and "plurality" means two or more. "One or several", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0051] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0052] like Figure 1 As shown, in the prior art, taking copper foil as an example, after depositing an upper graphene layer 21 and a lower graphene layer 22 on the surfaces of an upper copper foil 11 and a lower copper foil 12, respectively, an upper extrusion force F is applied relatively along the thickness direction of the upper copper foil 11 and the lower copper foil 12. 上 and lower extrusion force F 下 During the pressing process, the upper graphene layer 21 and the lower graphene layer 22 are subjected to the squeezing force, causing the graphene in the upper graphene layer 21 and the lower graphene layer 22 to re-agglomerate to form graphite and redistribute in a disordered manner. During the squeezing process, the surface of part of the upper copper foil 11 and the lower copper foil 12 will break through the upper graphene layer 21 and the lower graphene layer 22 to form a copper-copper bond, causing the structure of the graphene layer to be destroyed, further affecting the conductive properties of the copper foil graphene.
[0053] The technical solution of this application is as follows:
[0054] First, see Figure 2 , Figure 3 , Figure 4 and Figure 5 , the present application embodiment provides a method for preparing a composite conductor 3, comprising:
[0055] S11, providing a first conductive layer 31 and a second conductive layer 32, wherein the first conductive layer 31 includes a first conductive base layer and a first graphene layer deposited on the first conductive base layer;
[0056] S12, superimposing the second conductive layer 32 on the first conductive layer 31, so that the first graphene layer is placed between the first conductive layer 31 and the second conductive layer 32; the first conductive layer 31 and the second conductive layer 32 are provided with driving mechanisms that cooperate with each other;
[0057] S13, pressing the second conductive layer 32 and the first conductive layer 31 together along the thickness direction of the second conductive layer 32, driving the surface of the first conductive layer 31 on which the first graphene layer is deposited to move horizontally, and obtaining a composite conductor.
[0058] In the preparation method of the composite conductor 3 provided in the present application, during the lamination process of the first conductive layer 31 and the second conductive layer 32, the driving mechanism causes the surface of the first conductive layer 31 on which the first graphene layer is deposited to move horizontally, thereby avoiding graphene agglomeration and causing the already agglomerated graphene to be peeled off and re-formed into dispersed graphene, so that the disordered graphene is redistributed in an orderly manner under the mechanical force, thereby improving the conductivity of the composite conductor. In S11:
[0059] In some embodiments, the driving mechanism includes: a first groove 311 and a second groove 313 provided in the width direction of the first conductive layer 31, and a first protrusion 321 corresponding to the first groove 311 and a second protrusion 323 corresponding to the second groove 313 provided on the second conductive layer 32, wherein the first groove 311 and the second groove 313 are arranged at intervals, and the notches of the first groove 311 and the second groove 313 are located on the side of the first graphene layer away from the first conductive base layer.
[0060] It can be understood that during the pressing process of the first conductive layer 31 and the second conductive layer 32, the second protrusion 323 drives the second groove 313 to move in the horizontal direction, which can avoid the agglomeration of graphene. At the same time, the agglomerated or disordered graphene is mechanically exfoliated by extrusion, so that the agglomerated graphene is exfoliated to form dispersed graphene again, and the disordered graphene is redistributed in an orderly manner under the mechanical force, thereby improving the conductivity of the composite conductor 3. In addition, the first protrusion 321 and the first groove 311 can play a role in positioning and fixing the first conductive layer 31 and the second conductive layer 32. When the thickness of the first conductive layer 31 and the second conductive layer 32 is small, the strength of the first conductive layer 31 and the second conductive layer 32 can be increased to prevent them from deformation and wrinkles, and solve the problem of graphene deposition and pressing molding. When the thickness of the first conductive layer 31 and the second conductive layer 32 is large, the thickness of the graphene layer can be increased accordingly, thereby improving the conductivity of the composite conductor 3.
[0061] In some embodiments, a plurality of first grooves 311 and a plurality of second grooves 313 are provided, and the plurality of first grooves 311 and the plurality of second grooves 313 are arranged at intervals; a plurality of first protrusions 321 and a plurality of second protrusions 323 are provided, and the plurality of first protrusions 321 correspond to the plurality of first grooves 311 , and the plurality of second protrusions 323 correspond to the plurality of second grooves 313 .
[0062] In some embodiments, the second conductive layer 32 includes a second conductive base layer and a second graphene layer, and the second graphene layer is pressed onto a side of the first graphene layer facing away from the first conductive base layer.
[0063] In some embodiments, the first conductive layer 31 and the second conductive layer 32 may be copper foil, silver foil or aluminum foil, respectively. Further, the material of the copper foil may be copper, copper alloy or copper-doped graphene.
[0064] In some embodiments, the first conductive layer 31 further includes a first electroplating layer, which is disposed on a side of the first graphene layer away from the first conductive base layer. Accordingly, the second conductive layer 32 may further include a second electroplating layer, which is disposed on a side of the second graphene layer away from the second conductive base layer.
[0065] In some embodiments, the first electroplating layer and the second electroplating layer may be a copper-graphene mixed layer, a silver-graphene mixed layer, a copper-silver-graphene mixed layer or a copper-nickel-graphene mixed layer, respectively. Further, in the first electroplating layer and the second electroplating layer, the content of graphene may be 1.5% to 4.5%, for example, 1.6% to 4.2%, 1.8% to 4%, 2% to 3.8%, 2.2% to 3.6%, 2.4% to 3.5%, etc. Within the content range of graphene, the electroplating layer may play a role in isolating the first graphene layer of the first conductive layer 31 and the second graphene layer of the second conductive layer 32, protecting and fixing the graphene layer, preventing the graphene layer from detaching or causing disordered movement of the graphene due to external force; the first conductive base layer and the second conductive base layer are easy to break through the graphene layer and directly contact during the extrusion process, and the electroplating layer may avoid direct contact between the first conductive base layer and the second conductive base layer, and may also improve the continuous conductivity of the composite conductor 3.
[0066] In some embodiments, the thickness of the first electroplating layer and the second electroplating layer may be 0.35-3 um, for example, 0.5-2.8 um, 0.8-2.5 um, 1-2.2 um, 1.2-2 um, 1.5-1.8 um, etc. Within the thickness range of the electroplating layer, the electroplating layer can effectively prevent the agglomeration and disordered distribution of graphene.
[0067] In some embodiments, the number of layers of the first graphene layer and the second graphene layer can be 1 to 5 layers, for example, 3 layers, 4 layers, 5 layers, 6 layers, 7 layers, etc. Further, the thickness of a single layer of graphene can be 0.334 nm. In other words, the thickness of the first graphene layer and the second graphene layer can be 0.334 to 1.67 nm, respectively, and the total thickness of the graphene layer between the first conductive base layer and the second conductive base layer can be 0.334 to 3.34 nm. Within the thickness range of the graphene layer, the structure of the graphene can be guaranteed to be complete and orderly and evenly distributed.
[0068] In some embodiments, the thickness of the first conductive base layer and the second conductive base layer may be 8-60 um, for example, 10-58 um, 15-55 um, 20-50 um, 25-45 um, 30-40 um, etc.
[0069] In some embodiments, please refer to Figure 6 and Figure 7 , the side wall of the second groove 313 is connected to the side wall of the first groove 311 in the width direction of the first conductive layer 31. More specifically, along the width direction of the first conductive layer 31, the right side wall of the first groove 311 is connected to the left side wall of the second groove 313, the right side wall of the second groove 313 is connected to the left side wall of the second first groove 311, and the right side wall of the second first groove 311 is connected to the left side wall of the third second groove 313.
[0070] Understandable, see Figure 8 The sidewall of the second groove 313 and the sidewall of the first groove 311 may not be connected in the width direction of the first conductive layer 31 , and they may be independently spaced apart from each other.
[0071] In some embodiments, the width of the second groove 313 along the width direction of the first conductive layer 31 gradually decreases along the depth direction of the second groove 313 .
[0072] In at least one embodiment, taking a plane perpendicular to the length direction of the first conductive layer 31 as a cross section, the cross section of the sidewall of the second groove 313 is V-shaped. Correspondingly, the cross section of the second protrusion 323 is V-shaped.
[0073] In some embodiments, the angle between the sidewall of the second groove 313 and the upper surface of the first conductive base layer is smaller than the angle between the sidewall of the second protrusion 323 and the lower surface of the second conductive base layer. During the lamination process of the first conductive layer 31 and the second conductive layer 32, the second protrusion 323 can form a driving force to drive the second groove 313 to move in the horizontal direction to avoid agglomeration of graphene.
[0074] In some embodiments, an included angle ∠3 between the sidewall of the second groove 313 and the upper surface of the first conductive base layer is smaller than an included angle ∠4 between the sidewall of the second protrusion 323 and the lower surface of the second conductive base layer.
[0075] Furthermore, the angle ∠4 between the side wall of the second protrusion 323 and the lower surface of the second conductive base layer satisfies 20°≤∠4≤70°, for example, it can be 25°~65°, 28°~62°, 30°~60°, 35°~55°, 38°~52°, 40°~50°, etc.
[0076] It should be noted that the left side wall and the right side wall of the second groove 313 can be symmetrically arranged or asymmetrically arranged: when the left side wall and the right side wall of the second groove 313 are symmetrically arranged, the angles between the left side wall and the right side wall of the second groove 313 and the upper surface of the first conductive base layer are the same; when the left side wall and the right side wall of the second groove 313 are asymmetrically arranged, the angles between the left side wall and the right side wall of the second groove 313 and the upper surface of the first conductive base layer are different. Correspondingly, when the left side wall and the right side wall of the second groove 313 are symmetrically arranged, the left side wall and the right side wall of the second protrusion 323 are symmetrically arranged, that is, the angles between the left side wall and the right side wall of the second protrusion 323 and the lower surface of the second conductive base layer are the same; when the left side wall and the right side wall of the second groove 313 are asymmetrically arranged, the left side wall and the right side wall of the second protrusion 323 are asymmetrically arranged, that is, the angles between the left side wall and the right side wall of the second protrusion 323 and the lower surface of the second conductive base layer are different.
[0077] In some other embodiments, see Figures 9 to 11 The width of the second groove 313 along the width direction of the first conductive layer 31 increases step by step along the depth direction of the second groove 313 .
[0078] In some embodiments, taking a plane perpendicular to the length direction of the first conductive layer 31 as a cross section, the cross section of the sidewall of the second groove 313 is in an inverted trapezoidal shape.
[0079] In some embodiments, the width of the end of the second protrusion 323 is greater than the opening of the second groove 313 , so that the second protrusion 323 can press the second groove 313 .
[0080] In some embodiments, a second convex block 314 is convexly provided at the bottom of the second groove 313. Accordingly, a second depression 324 corresponding to the second convex block 314 is concavely provided at the end of the second protrusion 323. The second convex block 314 can deform the end of the second protrusion 323 along the width direction of the second groove 313 during the downward extrusion of the second protrusion 323, shear the graphene layer, and make the graphene evenly and orderly distributed.
[0081] It is understood that the shape of the second bump 314 is not limited. Exemplarily, the cross-section of the second bump 314 can be a triangle, a rectangle, a polygon or an irregular shape, with the plane perpendicular to the length direction of the horizontal plane where the first conductive layer 31 is located as the cross-section. The shape of the second recess 324 is the same as that of the second bump 314.
[0082] In some embodiments, the length of the second groove 313 in the length direction of the first conductive layer 31 is the same as the length of the first conductive layer 31 .
[0083] In other embodiments, the first conductive layer 31 has a plurality of second grooves 313 in the length direction, the plurality of second grooves 313 are arranged at intervals along the length direction of the first conductive layer 31, and the sum of the lengths of the plurality of second grooves 313 is less than the length of the first conductive layer 31. Specifically, the total length of the plurality of second grooves 313 is 35% to 70% of the length of the first conductive layer 31, for example, 38% to 68%, 40% to 65%, 42% to 60%, 45% to 58%, 50% to 55%, etc.
[0084] Correspondingly, the second conductive layer 32 has a plurality of second protrusions 323 along the length direction, and the plurality of second protrusions 323 correspond to the plurality of second grooves 313 one by one.
[0085] In some embodiments, the depth of the first groove 311 is 10% to 60% of the thickness of the first conductive base layer, for example, 12% to 58%, 15% to 55%, 18% to 52%, 20% to 50%, 30% to 40%, etc. In other words, the depth of the first groove 311 can be 0.8 to 36 um.
[0086] Accordingly, the height of the first protrusion 321 is 15% to 70% of the thickness of the second conductive base layer, for example, 18% to 68%, 20% to 65%, 25% to 60%, 30% to 50%, 40% to 45%, etc. In other words, the height of the first protrusion 321 can be 1.2 to 42 um, and the height of the first protrusion 321 is greater than the depth of the first groove 311, so that the first protrusion 321 can squeeze the first groove 311.
[0087] In some embodiments, a plurality of first grooves 311 may be provided along the length direction of the first conductive layer 31, and the plurality of first grooves 311 are arranged at intervals along the length direction of the first conductive layer 31. Accordingly, a plurality of first protrusions 321 are provided on the second conductive layer 32, and the plurality of first protrusions 321 correspond to the plurality of first grooves 311 one by one, so as to press the sidewalls of the first grooves 311.
[0088] In some embodiments, the first groove 311 includes a first groove section 3111 and a second groove section 3112 arranged in sequence along its depth direction, the width of the first groove section 3111 is gradually reduced along the depth direction, the width of the second groove section 3112 is gradually expanded along the depth direction, and the width of the end of the first protrusion 321 is smaller than the width of the connection between the first groove section 3111 and the second groove section 3112.
[0089] Furthermore, the width of the connection between the first groove section 3111 and the second groove section 3112 is 0.5um to 2um longer than the width of the end of the first protrusion 321, for example, 0.6um to 1.8um, 0.7um to 1.6um, 0.8um to 1.5um, 0.9um to 1.4um, 1um to 1.2um, etc. Within the width difference range, it is beneficial for the end of the first protrusion 321 to enter the first groove 311 and squeeze the first groove 311.
[0090] In some embodiments, the angle ∠1 between the side wall of the first groove segment 3111 and the upper surface of the first conductive base layer satisfies 80°≤∠1≤90°, for example, it can be 81°~89°, 82°~88°, 83°~87°, 84°~86°, etc. Within the angle range of ∠1, it is helpful to reserve space for the first protrusion 321 to move on the horizontal plane.
[0091] Accordingly, the angle ∠2 between the side wall of the second groove section 3112 and the upper surface of the first conductive base layer satisfies 35°≤∠2≤60°, for example, it can be 38°~58°, 40°~56°, 42°~55°, 44°~54°, 46°~52°, 48°~50°, etc. Within the angle range of ∠2, it is beneficial to fix the first protrusion 321 and promote the pressing of the first conductive base layer and the second conductive layer 32.
[0092] In this way, within the angle range of ∠1 and ∠2, the first protrusion 321 is advantageously pressed against the first groove 311, thereby promoting uniform dispersion of graphene; at the same time, the provision of the first groove segment 3111 and the second groove segment 3112 increases the surface area of the first conductive base layer, thereby increasing the deposition amount of graphene and improving the conductivity of the composite conductor 3 by graphene.
[0093] In some embodiments, a first convex block 312 is convexly disposed at the bottom of the first groove 311. Correspondingly, a first depression 322 corresponding to the first convex block 312 is concavely disposed at the end of the first protrusion 321. In this way, the first convex block 312 can shear the graphene layer during the downward extrusion of the first protrusion 321, so that the graphene is evenly and orderly distributed.
[0094] It can be understood that the shape of the first bump 312 is not limited. For example, the cross-section of the first bump 312 can be a triangle, a rectangle, a polygon or an irregular shape, with the plane perpendicular to the length direction of the horizontal plane where the first conductive layer 31 is located as the cross-section. The shape of the first recess 322 is the same as that of the first bump 312, and the width of the first recess 322 is greater than that of the first bump 312, so as to facilitate the extrusion of the first bump 312 and produce a peeling shearing effect.
[0095] In S13:
[0096] In some embodiments, the width of the end of the first protrusion 321 is smaller than the width of the first groove 311 , and when the first conductive layer 31 is driven to move horizontally, the gap between the first protrusion 321 and the first groove 311 gradually decreases until the first protrusion 321 and the first groove 311 fit together.
[0097] In some embodiments, before laminating the second conductive layer 32 and the first conductive layer 31 , the process includes: introducing an inert gas after evacuating the vacuum.
[0098] In some embodiments, the vacuum degree after evacuation is 1.2×10 -3 ~9.5×10 -2 Pa, for example, can be 2×10 -3 ~8×10 -2 Pa, 3×10 -3 ~7×10 -2 Pa, 4×10 -3 ~6×10 -2 Pa, 5×10 -3 ~5×10 -2 Pa, 6×10 -3 ~4×10 -2 Pa et al.
[0099] In some embodiments, the inert gas may be one or more of nitrogen, argon and helium.
[0100] In some embodiments, laminating the second conductive layer 32 and the first conductive layer 31 includes laminating under the following laminating conditions: a laminating temperature of 840 to 890° C.; a laminating pressure of 14 to 50 MPa; and a laminating time of 30 to 80 min.
[0101] In some embodiments, before the second conductive layer 32 and the first conductive layer 31 are pressed together, the second conductive layer 32 and the first conductive layer 31 are heated separately, so that the temperature of the second conductive layer 32 is higher than that of the first conductive layer 31. Furthermore, the temperature of the second conductive layer 32 is 40 to 80° C. higher than that of the first conductive layer 31, for example, 42 to 78° C., 45 to 75° C., 48 to 72° C., 50 to 70° C., 60 to 65° C., etc. The second conductive layer 32 first undergoes a certain deformation and is pressed together with the first conductive layer 31.
[0102] It should be noted that after the first conductive layer 31 and the second conductive layer 32 are heated to different temperatures, the pressing process begins. During the pressing process, the temperatures of the first conductive layer 31 and the second conductive layer 32 are the same.
[0103] The basic concepts have been described above. Obviously, for those skilled in the art, the above detailed disclosure is only for example and does not constitute a limitation of the present application. Although not explicitly stated herein, those skilled in the art may make various modifications, improvements and amendments to the present application. Such modifications, improvements and amendments are suggested in the present application, so such modifications, improvements and amendments still belong to the spirit and scope of the exemplary embodiments of the present application.
[0104] At the same time, the present application uses specific words to describe the embodiments of the present application. For example, "one embodiment", "an embodiment", and / or "some embodiments" refer to a certain feature, structure or characteristic related to at least one embodiment of the present application. Therefore, it should be emphasized and noted that "one embodiment" or "an embodiment" or "an alternative embodiment" mentioned twice or more in different positions in this specification does not necessarily refer to the same embodiment. In addition, some features, structures or characteristics in one or more embodiments of the present application can be appropriately combined.
[0105] Similarly, it should be noted that in order to simplify the description of the disclosure of this application and thus help understand one or more application embodiments, in the above description of the embodiments of this application, multiple features are sometimes merged into one embodiment, figure or description thereof. However, this disclosure method does not mean that the features required by the object of this application are more than the features mentioned in the claims. In fact, the features of the embodiments are less than all the features of the single embodiment disclosed above.
[0106] Each patent, patent application, patent application publication, and other materials, such as articles, books, specifications, publications, documents, etc., cited in this application is hereby incorporated by reference in its entirety, except for application history documents that are inconsistent with or conflicting with the content of this application, and documents that limit the broadest scope of the claims of this application (currently or later attached to this application). It should be noted that if the descriptions, definitions, and / or use of terms in the attached materials of this application are inconsistent or conflicting with the content of this application, the descriptions, definitions, and / or use of terms in this application shall prevail.
Claims
1. A method for preparing a composite conductor, characterized in that: include: Providing a first conductive layer and a second conductive layer, wherein the first conductive layer includes a first conductive base layer and a first graphene layer deposited on the first conductive base layer; The second conductive layer is superimposed on the first conductive layer, so that the first graphene layer is placed between the first conductive layer and the second conductive layer; the first conductive layer and the second conductive layer are provided with driving mechanisms that cooperate with each other; The second conductive layer and the first conductive layer are pressed together along the thickness direction of the second conductive layer, and the surface of the first conductive layer on which the first graphene layer is deposited is driven to move horizontally to obtain a composite conductor.
2. The preparation method according to claim 1, characterized in that The driving mechanism includes: a first groove and a second groove provided in the width direction of the first conductive layer, and a first protrusion corresponding to the first groove and a second protrusion corresponding to the second groove provided on the second conductive layer, wherein the first groove and the second groove are arranged at intervals, and the notches of the first groove and the second groove are located on the side of the first graphene layer away from the first conductive base layer.
3. The preparation method according to claim 2, characterized in that: There are multiple first grooves and multiple second grooves, and the multiple first grooves and multiple second grooves are arranged at intervals; there are multiple first protrusions and multiple second protrusions, and the multiple first protrusions are correspondingly matched with the multiple first grooves, and the multiple second protrusions are correspondingly matched with the multiple second grooves.
4. The preparation method according to claim 2, characterized in that: The width of the end of the first protrusion is smaller than the width of the first groove. When the first conductive layer is driven to move horizontally, the gap between the first protrusion and the first groove gradually decreases until the first protrusion fits with the first groove.
5. The preparation method according to claim 2, characterized in that: The first conductive layer also includes a first electroplating layer, which is arranged on a side of the first graphene layer away from the first conductive base layer, and the first electroplating layer is one of a copper-graphene mixed layer, a silver-graphene mixed layer, a copper-silver-graphene mixed layer or a copper-nickel-graphene mixed layer.
6. The preparation method according to claim 2, characterized in that: A sidewall of the second groove is connected to a sidewall of the first groove in a width direction of the first conductive layer.
7. The preparation method according to any one of claim 2, characterized in that: The width of the second groove along the width direction of the first conductive layer decreases step by step along the depth direction of the second groove.
8. The preparation method according to claim 7, characterized in that: Taking a plane perpendicular to the length direction of the first conductive layer as a cross section, the cross section of the side wall of the second groove is V-shaped.
9. The preparation method according to claim 7, characterized in that: An angle ∠3 between the side wall of the second groove and the upper surface of the first conductive base layer is smaller than an angle ∠4 between the side wall of the second protrusion and the lower surface of the second conductive layer; wherein ∠4 satisfies 20°≤∠4≤70°.
10. The preparation method according to claim 2, characterized in that: The width of the second groove along the width direction of the first conductive layer increases step by step along the depth direction of the second groove.
11. The preparation method according to claim 10, characterized in that: Taking a plane perpendicular to the length direction of the first conductive layer as a cross section, the cross section of the side wall of the second groove is in an inverted trapezoidal shape.
12. The preparation method according to claim 10, characterized in that: A second convex block is convexly formed at the bottom of the second groove, and a second concave block corresponding to the second convex block is concavely formed at the end of the second protrusion.
13. The preparation method according to any one of claims 6 to 12, characterized in that: The length of the second groove in the length direction of the first conductive layer is the same as the length of the first conductive layer; or The first conductive layer has a plurality of second grooves in the length direction, the plurality of second grooves are spaced apart along the length direction of the first conductive layer, and the sum of the lengths of the plurality of second grooves is less than the length of the first conductive layer, and the second conductive layer has a plurality of second protrusions along the length direction, the plurality of second protrusions correspond one-to-one to the plurality of second grooves.
14. The preparation method according to claim 2, characterized in that: The first groove includes a first groove section and a second groove section arranged in sequence along its depth direction, the width of the first groove section is gradually reduced along the depth direction, the width of the second groove section is gradually expanded along the depth direction, and the width of the end of the first protrusion is smaller than the width of the connection between the first groove section and the second groove section.
15. The preparation method according to claim 14, characterized in that: An angle ∠1 between the side wall of the first slot segment and the upper surface of the first conductive base layer satisfies 80°≤∠1≤90°, and an angle ∠2 between the side wall of the second slot segment and the upper surface of the first conductive base layer satisfies 35°≤∠2≤60°.
16. The preparation method according to claim 2, characterized in that: A first convex block is convexly formed at the bottom of the first groove, and a first concave block corresponding to the first convex block is concavely formed at the end of the first protrusion.
17. The preparation method according to claim 1, characterized in that: Before laminating the second conductive layer and the first conductive layer, the method includes: introducing an inert gas after evacuation; and heating the second conductive layer and the first conductive layer respectively so that the temperature of the second conductive layer is higher than that of the first conductive layer.
18. The preparation method according to claim 17, characterized in that: The vacuum degree after evacuation is 1.2×10 -3 ~9.5×10 -2 Pa; The inert gas is one or more of nitrogen, argon and helium; After the second conductive layer and the first conductive layer are heated respectively, the temperature of the second conductive layer is 40 to 80° C. higher than the temperature of the first conductive layer; The laminating of the second conductive layer and the first conductive layer comprises laminating under the following conditions: a laminating temperature of 840 to 890° C., a laminating pressure of 14 to 50 MPa, and a laminating time of 30 to 80 min.