MOS device and preparation method thereof

By designing the body region structure of different doping types and materials in SiC MOSFETs and in contact with the gate dielectric, the problem of the interface state limitation between the body region material and the gate oxygen is solved, and the channel mobility and conductivity are improved.

CN119069537AActive Publication Date: 2024-12-03ZHUHAI GREE ELECTRONIC COMPONENTS CO LTD +1

Patent Information

Application Number
CN202411565542.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-05
Publication Date
2024-12-03
Estimated Expiration
2044-11-05

AI Technical Summary

Technical Problem

The low channel mobility of existing SiC MOSFET devices leads to poor conductivity, mainly due to the limitations of factors such as the interface state between body area materials and gate oxygen materials.

Method used

A MOS device is designed, and its body region structure includes the first body region and the second body region of different doping types and materials, and contacts the gate dielectric through different semiconductor materials, avoiding the interface state of the body region material and the gate oxygen material. The limitations of the channel increase the channel mobility.

Benefits of technology

By improving channel mobility, the current transmission efficiency and speed are improved, and the conductive performance and reliability of the device are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069537A_ABST
    Figure CN119069537A_ABST
Patent Text Reader

Abstract

The invention discloses an MOS (Metal Oxide Semiconductor) device and a preparation method thereof, the MOS device comprises a substrate and a drift layer on one side of the substrate, the drift layer is provided with a first surface deviating from the substrate, the MOS device further comprises at least one source region structure, the source region structure comprises a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region have a first doping type, the second heavily doped region has a second doping type, the first body region is at least located at one side, close to the substrate, of the first heavily doped region and the second heavily doped region, and the first body region and the drift layer have different semiconductor materials; and the gate structure comprises a gate and a first gate medium, the first gate medium is at least located between the gate and the source region structure, and the first gate medium is at least in contact with the first body region and the second heavily doped region. The problem of low channel mobility of the MOS device in the prior art is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the semiconductor field, and in particular, to a MOS device and a method for manufacturing the same. Background Art

[0002] Silicon-based IGBTs dominate high-voltage and high-current scenarios, but they cannot withstand high-frequency conditions and have high power consumption. SiC's high-voltage and high-temperature resistance allows it to cover the voltage resistance level of silicon-based IGBTs with only simpler MOSFET devices, while avoiding its high energy consumption disadvantages. Under the same environment, silicon carbide-based MOSFETs reduce energy losses by 66% compared to silicon-based IGBTs of the same specifications, mainly due to a significant reduction in switching losses. In the new energy vehicle industry, SiC can be used to drive and control inverters, on-board chargers, and fast charging piles for motors. In photovoltaic power generation, leading photovoltaic inverter companies have currently adopted SiC power devices to replace silicon devices.

[0003] Channel mobility is one of the important parameters of SiC MOSFET. Channel mobility refers to the migration speed of electrons or holes in the channel under the action of an electric field. In MOSFET, channel mobility determines the transmission efficiency and speed of current. The higher the channel mobility, the faster the migration speed of electrons or holes in the channel, and the better the conductivity of the device.

[0004] Due to the influence of the material itself, SIC and other factors such as the SiC / SiO2 interface state greatly limit the channel mobility of SiC and reduce the conductive performance of the device. Summary of the invention

[0005] The present application provides a MOS device and a method for manufacturing the same, so as to solve the problem of low channel mobility of the MOS device in the related art.

[0006] According to one aspect of the present application, a MOS device is provided, comprising: a substrate and a drift layer on one side of the substrate, the drift layer having a first surface facing away from the substrate, the MOS device also comprising: at least one source region structure, the source region structure comprising a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region having a first doping type, the second heavily doped region having a second doping type, the first body region being at least located on a side of the first heavily doped region and the second heavily doped region close to the substrate, the first body region and the drift layer having different semiconductor materials; a gate structure, the gate structure comprising a gate and a first gate dielectric, the first gate dielectric being at least located between the gate and the source region structure, wherein the first gate dielectric is in contact with at least the first body region and the second heavily doped region.

[0007] Optionally, the source region structure further includes: a second body region, the second body region is located on a side of the first body region close to the substrate and in contact with the first body region, the second body region has the first doping type, and the second body region and the drift layer have the same semiconductor material.

[0008] Optionally, the material of the first body region includes silicon material, and the material of the second body region includes silicon carbide material.

[0009] Optionally, the source region structure includes a first source region structure and a second source region structure, the first source region structure has a second surface facing away from the substrate, the first source region structure is located in the drift layer and the second surface is located in the first surface, the second source region structure is located on a side of the drift layer facing away from the substrate, and the first source region structure is not in contact with the second source region structure; the gate structure is located on a side of the drift layer facing away from the substrate, and the gate structure is in contact with a first side surface of the second source region structure and a portion of the second surface of the first source region structure, respectively, wherein the first side surface is a side surface of the second source region structure close to the first source region structure.

[0010] Optionally, the MOS device further includes: a current extension region, wherein the current extension region is located in the drift layer and contacts the first source region structure, the side of the current extension region facing away from the first source region structure contacts the first side, and the current extension region has a second doping type.

[0011] Optionally, the doping concentration of the current extension region is 100 to 1000 times the doping concentration of the drift layer.

[0012] Optionally, the MOS device further includes: a first conductive layer, the first conductive layer is located on a side of the first heavily doped region and a portion of the second heavily doped region away from the substrate, and the first conductive layer forms an ohmic contact with the source region structure.

[0013] According to one aspect of the present application, a method for preparing a MOS device is provided, which is used to prepare any one of the MOS devices, and the preparation method includes: providing a substrate; forming a drift layer on the substrate, the drift layer having a first surface facing away from the substrate; forming a source region structure, the source region structure including a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region have a first doping type, the second heavily doped region has a second doping type, the first body region is at least located on a side of the first heavily doped region and the second heavily doped region close to the substrate, and the first body region and the drift layer have different semiconductor materials; forming a gate structure, the gate structure including a gate and a first gate dielectric, the first gate dielectric is at least located between the gate and the source region structure, wherein the first gate dielectric is in contact with at least the first body region and the second heavily doped region.

[0014] Optionally, the steps of forming the source region structure include: using a deposition process to form a first material layer on the drift layer respectively; using an ion implantation process to implant ions into the first material layer respectively to form the first body region; using an ion implantation process to implant ions of different doping types into the first body region respectively to form the first heavily doped region and the second heavily doped region.

[0015] Optionally, the preparation method also includes forming a second body region, which is located on the side of the first body region close to the substrate and in contact with the first body region, and the preparation steps include: injecting ions into the first material layer and the second material layer, the first material layer forming the first body region, and the second material layer forming the second body region, wherein the second material layer is a portion of the drift layer located in the drift layer and in contact with the first material layer, and the ratio of the depth of ion implantation in the first material layer and the second material layer in the second direction is 1:2~1:6, and the second direction is perpendicular to the first surface.

[0016] Through the technical solution of the present application, a MOS device is provided, in which the first body region is made of a material different from that of the drift layer, and different semiconductor materials exhibit different carrier mobilities after contacting the first gate dielectric. By setting semiconductor materials with different carrier mobilities for the first body region, factors such as the interface state between the body region material and the gate oxide material in the prior art that greatly limit the channel mobility of the body region are avoided, and the channel mobility is improved to improve the transmission efficiency and speed of the current, thereby improving the conductivity of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0018] Figure 1 is a schematic cross-sectional structure diagram of a MOS device provided according to an embodiment of the present application;

[0019] Figure 2 is a flow chart of a method for preparing a MOS device according to an embodiment of the present application;

[0020] Figure 3 It is a schematic diagram of the cross-sectional structure of a substrate after a drift layer is formed on a substrate in a method for preparing a MOS device provided in an embodiment of the present application;

[0021] Figure 4 is Figure 3 A schematic diagram of the cross-sectional structure of the substrate after the first trench is formed on the drift layer shown;

[0022] Figure 5 is Figure 4 A schematic diagram of the cross-sectional structure of the substrate after the first material layer is formed on the drift layer shown;

[0023] Figure 6 is Figure 5 A schematic diagram of the cross-sectional structure of the substrate after the first body region is formed in the first material layer;

[0024] Figure 7 is Figure 6 A schematic diagram of the cross-sectional structure of the substrate after the first heavily doped region and the second heavily doped region are formed in the first body region;

[0025] Figure 8 is Figure 5 The schematic cross-sectional structure diagram of the substrate after the first body region and the second body region are formed in the first material layer and the second material layer;

[0026] Fig. 9 is Figure 8 A schematic diagram of the cross-sectional structure of the substrate after the first heavily doped region and the second heavily doped region are formed in the first body region;

[0027] Fig.10 is Fig. 9 A schematic diagram of the cross-sectional structure of the substrate after a current extension region is formed in the drift layer shown;

[0028] Fig.11 is Fig.10 The schematic diagram of the cross-sectional structure of the substrate after the first gate dielectric is formed on the first source region structure and the side surface of the second source region structure is shown;

[0029] Fig.12 is Fig.11 A schematic cross-sectional structure diagram of a substrate after a gate is formed on the first gate dielectric shown;

[0030] Fig.13 is Fig.12 A schematic cross-sectional structure diagram of the substrate after a second gate dielectric is formed on the gate shown;

[0031] Fig.14 is Fig.13 The schematic cross-sectional structure diagram of the substrate behind the first conductive layer on the first heavily doped region and the second heavily doped region is shown;

[0032] Fig.15 is Fig.14 The cross-sectional structure diagram of the base body is shown after a second conductive layer is formed on the first conductive layer, source region structure and gate structure and a third conductive layer is formed on the substrate.

[0033] The above drawings include the following reference numerals:

[0034] 10. substrate; 20. drift layer; 201. first surface; 21. preliminary drift layer; 30. source region structure; 301. first heavily doped region; 302. second heavily doped region; 303. first body region; 3031. first material layer; 3032. second material layer; 304. second body region; 31. first source region structure; 32. second source region structure; 321. first side surface; 33. first trench; 40. gate structure; 401. gate; 4011. second side surface; 401 2. The third side; 402. The first gate dielectric; 4021. The first sub-gate dielectric layer; 4022. The second sub-gate dielectric layer; 50. The current extension region; 61. The first conductive layer; 62. The second conductive layer; 63. The third conductive layer; 70. The second gate dielectric; 71. The third sub-gate dielectric; 711. The first low-pressure epoxy alkyl silicone oil layer; 712. The second low-pressure epoxy alkyl silicone oil layer; 72. The fourth sub-gate dielectric; 721. The first tetraethyl orthosilicate layer; 722. The second tetraethyl orthosilicate layer. DETAILED DESCRIPTION

[0035] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0036] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0037] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0038] As described in the background technology, in the MOSFET of the prior art, the channel mobility determines the transmission efficiency and speed of the current. The higher the channel mobility, the faster the migration speed of electrons or holes in the channel, and the better the conductivity of the device. In the MOSFET of the prior art, due to the influence of the material itself, in addition, due to factors such as the interface state between the existing body material and the gate oxide material, the channel mobility of the MOSFET device is greatly limited, thereby reducing the conductivity of the device. In order to solve the above technical problems, the present application provides a MOS device and a method for preparing the MOS device.

[0039] According to one aspect of the present application, a MOS device is provided, such as Figure 1 As shown, the MOS device includes: a substrate 10 and a drift layer 20 on one side of the substrate 10, the drift layer 20 has a first surface 201 away from the substrate 10, and the MOS device also includes: at least one source region structure 30, the source region structure 30 includes a first heavily doped region 301, a second heavily doped region 302 and a first body region 303, the first heavily doped region 301 and the first body region 303 have a first doping type, the second heavily doped region 302 has a second doping type, the first body region 303 is at least located on a side of the first heavily doped region 301 and the second heavily doped region 302 close to the substrate 10, and the first body region 303 and the drift layer 20 have different semiconductor materials; a gate structure 40, the gate structure 40 includes a gate 401 and a first gate dielectric 402, the first gate dielectric 402 is at least located between the gate 401 and the source region structure 30, wherein the first gate dielectric 402 is in contact with at least the first body region 303 and the second heavily doped region 302. The first body region 303 in the device uses a semiconductor material different from that of the drift layer 20. Different semiconductor materials exhibit different carrier mobilities after contacting the first gate dielectric 402. By setting semiconductor materials with different carrier mobilities for the first body region, factors such as the interface state between the body region material and the gate oxide material in the prior art that greatly limit the channel mobility of the body region are avoided. The channel mobility is improved to improve the transmission efficiency and speed of the current, thereby improving the conductivity of the device.

[0040] Specifically, the substrate 10, the drift layer 20, and the second heavily doped region 302 have the same doping type, and the doping concentration of the drift layer 20 is 1.0×10 15 cm -3 ~1.0×10 16 cm -3 , wherein the doping concentration of the substrate 10 is higher than the doping concentration of the drift layer 20, and the resistivity of the substrate 10 is 0.016Ωcm~0.024Ωcm. The doped substrate 10 can reduce the on-resistance of the MOS device, and the substrate 10 has a high concentration so that an ohmic contact is formed at the drain end, further reducing the on-resistance of the device, thereby improving the performance of the device. In addition, the role of the drift layer 20 is to bear the main breakdown voltage. Those skilled in the art can meet the breakdown voltage of the product by adjusting the thickness of the drift layer 20. For example, when the thickness of the drift layer 20 is 9μm~11μm, the breakdown voltage of the MOS device is 1200V, and when the thickness of the drift layer 20 is 5μm~7μm, the breakdown voltage of the MOS device is reduced to 650V.

[0041] In some optional embodiments, such as Figure 1 As shown, the source region structure 30 also includes: a second body region 304 , which is located on the side of the first body region 303 close to the substrate 10 and contacts the first body region 303 , has a first doping type, and has the same semiconductor material as the drift layer 20 .

[0042] Specifically, in the MOS device, the source region structure 30 has a first body region 303 and a second body region 304, wherein the first body region 303 and the second body region 304 have different materials but the same doping type, and the material of the second body region 304 is the same as the drift layer 20, wherein the mobility refers to the migration speed of electrons or holes in the channel under the action of the electric field, and by setting the first body region 303 to a semiconductor material with a high carrier mobility, the conduction capability of the device can be greatly improved. However, in order to control the thickness of the MOS device, the thickness of the first body region 303 is often set to be relatively thin, which easily leads to a narrow width of the depletion layer formed in the contact area between the first body region 303 and the drift layer 20, and the high concentration of carriers in the second heavily doped region 302 easily passes through the narrow first body region 303, resulting in a large leakage anomaly in the MOS device. The second body region 304 is set below the first body region 303, while increasing the thickness of the body region, preventing the leakage anomaly of the MOS device and improving the reliability of the MOS device.

[0043] In some optional embodiments, the material of the first body region includes silicon material, and the material of the second body region includes silicon carbide material.

[0044] Specifically, silicon carbide (SiC) material has the advantages of large bandgap, high thermal conductivity, high breakdown field strength, and high electron saturation drift velocity. MOS devices made of silicon carbide have the characteristics of high power, high frequency, and high temperature. However, the electron mobility of SiC material is 900cm 2 / Vs, compared with other semiconductor materials, using silicon carbide as the body region material is not conducive to the electron mobility of the channel, reducing the conduction capability of the MOS device. In addition, due to the large difference in energy levels between the silicon carbide material and the first gate dielectric material, the interface state of SiC / SiO2 is large, resulting in a lower mobility of the body region composed of SiC.

[0045] The material of the first body region includes silicon material. For example, the material of the first body region may be single crystal silicon material. Single crystal silicon is a high-purity crystalline silicon with excellent electrical properties, chemical stability and mechanical strength. The electron mobility is 1000 cm 2 / Vs to 1500cm 2 / Vs seconds, specifically 1250cm 2 / Vs. The electron mobility of single crystal silicon is affected by many factors, including impurity content, crystal defects, lattice structure, etc. Among them, impurity content is one of the main factors affecting the electron mobility of single crystal silicon. The effect of impurity elements will cause the impurity energy level to appear in the crystal band gap, and the electron capture and release process will occur, thereby improving the electron mobility of the channel. In addition, due to the small difference in energy levels between the carbon material and the first gate dielectric material, the interface state of Si / SIO2 is small, which leads to the actual mobility of the Si body region being 10 times the actual mobility of the SiC body region, thereby improving the channel carrier mobility of the MOS device and improving the conductivity of the device.

[0046] Exemplarily, the first body region and the second body region both have a first doping type, wherein the doping concentration is 5×1.0×10 16 cm -3 ~1.5×10 17 cm -3 The thickness ratio of the first body region and the second body region in the direction perpendicular to the first plane is 1:1~1:4. The first body region is silicon-based, which can improve the channel mobility of the MOS device. The second body region is silicon carbide-based, which can prevent the MOS device from leaking electricity, thereby significantly improving the reliability of the device.

[0047] In some optional embodiments, such as Figure 1As shown, the source region structure 30 includes a first source region structure 31 and a second source region structure 32, the first source region structure 31 has a second surface facing away from the substrate, the first source region structure 31 is located in the drift layer 20 and the second surface is located in the first surface 201, the second source region structure 32 is located on the side of the drift layer 20 facing away from the substrate 10, and the first source region structure 31 is not in contact with the second source region structure 32; the gate structure 40 is located on the side of the drift layer 20 facing away from the substrate 10, and the gate structure 40 is in contact with the first side surface 321 of the second source region structure 32 and part of the second surface of the first source region structure 31, wherein the first side surface 321 is the side of the second source region structure 32 close to the first source region structure 31. The first gate dielectric 402 is located on the second side surface 4011 and the bottom surface of the gate 401, and the second side surface 4011 is the side of the gate 401 close to the second source region structure 32.

[0048] Specifically, in the prior art, for planar MOS, there is a problem that the electric field strength generated by the oxide layer above the gate region is high and the on-resistance is large; while the on-resistance of the trench MOS device is smaller, but there is a problem that the electric field strength at the corner below the trench is much greater than that at other positions. Under the same applied voltage and the same gate oxide thickness, the electric field strength at the corner of the trench is about 3 times that of the electric field in the middle of the planar MOS gate oxide, and the gate oxide is easily broken down in advance. In the above embodiment, by setting the first source region structure in the trench and the second source region structure on the side away from the substrate, the MOS device has the characteristics of both a planar MOS device and a trench MOS device, and has both a planar channel and a vertical channel, with a smaller on-resistance and a better balanced electric field distribution, so that the electric field originally concentrated in the oxide layer below the gate region and the corner of the trench is dispersed, reducing the risk of the gate being broken down in advance. At the same time, since the semi-planar semi-trench structure changes the gate shape, the overlapping area between the gate and the drain is reduced, so the gate-drain charge Q gd , gate-drain capacitance C gd (also called Miller capacitance) are effectively reduced, which improves the switching speed of the device and reduces switching losses.

[0049] In other optional embodiments, such as Figure 1 As shown, the MOS device also includes: a current extension region 50, which is located in the drift layer 20 and contacts the first source region structure 31, and the side of the current extension region 50 away from the first source region structure 31 contacts the first side 321, and the current extension region 50 has a second doping type.

[0050] Specifically, a current extension region is formed in the drift layer between the first source region structure and the second source region structure. When the device is turned on, the current flows through the channel of the first source region structure and the second source region structure through the current extension region. The current extension region has a higher electron mobility and a stronger conduction capability, which can reduce the on-resistance of the device.

[0051] In some optional embodiments, the doping concentration of the current extension region is 100 to 1000 times the doping concentration of the drift layer.

[0052] Specifically, the current extension region and the drift layer have the second doping type, and the doping concentration of the current extension region is 1.0×10 19 cm -3 ~1.0×10 20 cm -3 , the doping concentration of the drift layer is 1.0×10 15 cm -3 ~1.0×10 16 cm -3 The doping concentration of the current extension region is about 100 to 1000 times that of the ordinary drift region. In semiconductor materials, carriers mainly come from doping. When the doping concentration increases, the number of carriers increases. Under the same level of other conditions, the carrier mobility can be increased by more than 100 times. When the MOS device is turned on, the on-resistance of the device is reduced. The current extension region in the source structure and the gate structure can increase the carrier mobility by more than 100 times, and the resistance of the corresponding JFET terminal structure of the MOS device can be reduced to more than 1 / 100 of it, so as to reduce the difficulty of preparing the MOS device.

[0053] In some optional embodiments, such as Figure 1 As shown, the MOS device further includes: a first conductive layer 61 , which is located on a side of the first heavily doped region 301 and a portion of the second heavily doped region 302 away from the substrate, and forms an ohmic contact with the source region structure 30 .

[0054] Specifically, the material of the first conductive layer includes a metal material. The first conductive layer contacts the first heavily doped region and part of the second heavily doped region to form a metal material-semiconductor material structure and a barrier layer. Since the doping concentration of the first heavily doped region and the second heavily doped region is 1.0×10 19 cm -3 ~1.0×10 20 cm -3 , with a higher doping concentration, carriers can pass through the barrier by tunneling effect, thus forming a low-resistance ohmic contact, thereby reducing the on-resistance of the device.

[0055] In some specific embodiments, the material of the first conductive layer includes but is not limited to Ni and Ti, and the thickness is 200 nm to 400 nm. Those skilled in the art can make a selection according to the product, and this application does not specifically limit it.

[0056] In some other embodiments, Figure 1 As shown, the MOS device further includes: a second gate dielectric 70, a second conductive layer 62 and a third conductive layer 63, wherein the second gate dielectric 70 is at least located at the third side surface 4012 and the top surface of the gate 401 opposite to the second side surface 4011, and the second gate dielectric 70 is respectively in contact with the gate 401, the first gate dielectric 402 and a part of the source region structure 30; the second conductive layer 62 is located on the side of the first conductive layer 61, the gate structure 40, the second gate dielectric 70 and the source region structure 30 away from the substrate 10, and the second conductive layer 62 is respectively in contact with the first conductive layer 61, the second gate dielectric 70 and a part of the source region structure 30; the third conductive layer 63 is located on the side of the substrate 10 away from the drift layer 20, wherein the second conductive layer 62 and the third conductive layer 63 are respectively used as the source electrode and the drain electrode of the MOS device, and play the role of current input and output of the MOS device.

[0057] Wherein, the material of the second gate dielectric may include but is not limited to SIO2, Al2O3, AlN, HfO2 and Si3N4, which is not specifically limited in this application. In the first direction, the thickness of the second gate oxide layer and the thickness of the first gate oxide layer are 6000A~12000A and 400A~800A respectively, and in the second direction, the thickness of the second gate oxide layer and the thickness of the first gate oxide layer are 6000A~12000A and 400A~800A respectively, the first direction is perpendicular to the first plane, and the second direction is parallel to the first surface.

[0058] In addition, the materials of the second conductive layer and the third conductive layer include, but are not limited to, alloy materials composed of any one or more of Ag, Cu, Al, Au, Ti, Ni, Pt and Pb metals. Those skilled in the art can make reasonable selections according to actual needs, and no specific limitation is made without application. Among them, the thickness of the second conductive layer is 2μm~6μm, and the thickness of the third conductive layer is 200nm~400nm. Exemplarily, the material of the second conductive layer can be AlCu, and the material of the third conductive layer can be TiNiAg. Both AlCu and TiNiAg have good electrical conductivity, which improves the electrical conductivity of the device.

[0059] According to one aspect of the present application, a method for preparing a MOS device is provided, which is used to prepare any MOS device, such as Figure 2 As shown, the preparation method comprises:

[0060] Step S101: providing a substrate;

[0061] Step S102: forming a drift layer on the substrate, wherein the drift layer has a first surface facing away from the substrate;

[0062] Step S103: forming a source region structure, the source region structure comprising a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region having a first doping type, the second heavily doped region having a second doping type, the first body region being located at least on one side of the first heavily doped region and the second heavily doped region close to the substrate, and the first body region and the drift layer having different semiconductor materials;

[0063] Step S104: forming a gate structure, the gate structure comprising a gate and a first gate dielectric, the first gate dielectric being at least located between the gate and the source region structure, wherein the first gate dielectric is in contact with at least the first body region and the second heavily doped region.

[0064] By adopting the above-mentioned preparation method of the embodiment of the present application, on the basis of the traditional MOS device, a semiconductor material different from the drift layer is adopted as the body material. Different semiconductor materials exhibit different carrier mobilities after contacting the first gate dielectric. By setting semiconductor materials with different carrier mobilities for the first body region, factors such as the interface state between the body material and the gate oxide material in the prior art that greatly limit the channel mobility of the body region are avoided, and the channel mobility is improved to improve the transmission efficiency and speed of the current, thereby improving the conductivity of the device.

[0065] The following will describe in more detail the exemplary embodiments of the method for preparing the MOS device provided by the present application in conjunction with the accompanying drawings. However, these exemplary embodiments can be implemented in a variety of different forms and should be interpreted as being limited to the embodiments described herein. It should be understood that these embodiments are provided to make the disclosure of the present application thorough and complete, and to fully convey the concepts of these exemplary embodiments to those of ordinary skill in the art.

[0066] First, if Figure 3 As shown, step S101 is performed: providing a substrate 10 .

[0067] Specifically, the materials of the substrate 10 include silicon carbide, silicon, gallium nitride, gallium oxide, aluminum oxide, aluminum nitride and the like. Personnel skilled in the art may make reasonable selections based on actual needs, and no specific limitation is imposed on the application.

[0068] Exemplarily, the substrate includes a doped SiC substrate having a resistivity of 0.016 Ωcm to 0.024 Ωcm to form a high-power MOS device.

[0069] After providing the substrate, as Figure 3 As shown, step S102 is performed: a drift layer 20 is formed on the substrate 10 .

[0070] Specifically, the drift layer 20 may be an epitaxial layer having the same doping type as the substrate 10, or may be made of the same semiconductor material as the substrate. The doping concentration of the drift layer 20 is 1.0×10 15 cm -3 ~1.0×10 16 cm -3 , and the doping concentration of the drift layer 20 is lower than the doping concentration of the substrate, and bears the main breakdown voltage in the MOS device. In addition, those skilled in the art can adjust the thickness of the drift layer 20 to meet the breakdown voltage of the product. For example, when the thickness of the drift layer 20 is 9μm~11μm, the breakdown voltage of the MOS device is 1200V, and when the thickness of the drift layer 20 is 5μm~7μm, the breakdown voltage of the MOS device is reduced to 650V.

[0071] In some optional embodiments, the process of forming a drift layer includes but is not limited to a deposition process and an epitaxial growth process. In the epitaxial growth process, the doping concentration of impurities is relatively easy to control and the activation rate is relatively fixed, so it is easy to achieve the target doping distribution. It is not only suitable for silicon-based power devices, but also can avoid the difficulty of injection doping of silicon carbide power devices and improve the efficiency of its terminal structure. The deposition process is relatively mature, simple to operate and has low cost. The deposition process includes but is not limited to physical vapor deposition (PVD), chemical vapor deposition (CVD) and atomic layer deposition (ALD). Physical vapor deposition (PVD) includes but is not limited to magnetron sputtering process, reactive sputtering process, DC sputtering process, AC sputtering process, vacuum coating process, arc evaporation process, and chemical vapor deposition (CVD) includes but is not limited to plasma enhanced chemical vapor deposition (PECVD), metal-organic chemical vapor deposition (MOCVD), and laser-induced chemical vapor deposition (LCVD). Those skilled in the art can make reasonable selections according to actual needs, and no specific limitation is made without application.

[0072] Then, after forming the drift layer, step S103 is performed to form a source region structure.

[0073] The steps of forming the source region structure include: first, Figure 4 and Figure 5As shown, a first material layer 3031 is formed on the drift layer 20 by a deposition process; then, as shown in FIG. Figure 6 As shown, ions are implanted into the first material layer 3031 by an ion implantation process to form a first body region 303; then, as shown in FIG. Figure 7 As shown, ion implantation process is used to implant ions of different doping types into the first body region 303 to form a first heavily doped region 301 and a second heavily doped region 302 .

[0074] More specifically, the steps of forming the first source region structure and the second source region structure include: before forming the source region structure, first, as Figure 4 As shown, a first trench 33 is formed in the drift layer 20 by an etching process; then, as shown in FIG. Figure 5 As shown, a first material layer 3031 is formed on the bottom of the first trench and the preliminary drift layer 21 by a deposition process, wherein the preliminary drift layer 21 is a portion of the drift layer 20 located on the side of the first material layer 3031 away from the first trench; then, as shown Figure 6 As shown, ions are implanted into the first material layer 3031 by an ion implantation process to form a first body region 303; then, as shown in FIG. Figure 7 As shown, ion implantation of different doping types is performed in the first body region 303 by ion implantation to form a first heavily doped region 301 and a second heavily doped region 302. The first source region structure 31 or the second source region structure 32 includes a first heavily doped region 301, a second heavily doped region 302 and a first body region 303.

[0075] In other embodiments, Figure 8 As shown, the preparation method further includes forming a second body region 304, the second body region 304 is located on the side of the first body region 303 close to the substrate 10 and in contact with the first body region 303, and the steps of preparing the second body region 304 include: Figure 8 As shown, in the process of forming the first body region by ion implantation into the first material layer, the ion implantation depth is deepened so that the second material layer 3032 located below the first material layer is also implanted with ions, wherein the second material layer 3032 is a portion of the drift layer 20 located in the drift layer 20 and in contact with the first material layer 3031, so as to form the second body region 304; then, as shown in Fig. 9 As shown, ion implantation of different doping types is performed in the first body region 303 by an ion implantation process to form a first heavily doped region 301 and a second heavily doped region 302. The first heavily doped region 301, the second heavily doped region 302, the first body region 303 and the second body region 304 located in the trench constitute a first source region structure 31; the first heavily doped region 301, the second heavily doped region 302, the first body region 303 and the second body region 304 located on the drift layer 20 constitute a second source region structure 32.

[0076] Wherein, ions are injected into the first material layer and the second material layer, the first material layer forms a first body region, and the second material layer forms a second body region, wherein the second material layer is a portion of the drift layer located in the drift layer and in contact with the first material layer, and the ratio of the depth of ion injection in the first material layer and the second material layer in the second direction is 1:2~1:6, and the second direction is perpendicular to the first surface.

[0077] For example, the first material layer has a first doping type and a doping concentration of 1.0×10 15 cm -3 ~1.0×10 16 cm -3 , the thickness is 0.4μm-0.5μm, the total thickness of the first material layer and the second material layer is 0.7μm~0.8μm; the first body region has a first doping type and a doping concentration of 5.0×10 16 cm -3 ~1.5×10 17 cm -3 , the second body region has the first doping type and the doping concentration is 5.0×10 16 cm -3 ~1.5×10 17 cm -3 The first heavily doped region has a first doping type and a doping concentration of 5.0×10 18 cm -3 ~1.5×10 19 cm -3 , with a thickness of 0.2 μm-0.3 μm; the second heavily doped region has a second doping type and a doping concentration of 5.0×10 18 cm -3 ~1.5×10 19 cm -3 The thickness is 0.2μm-0.3μm. People skilled in the art can make a reasonable selection according to actual needs, and no specific limitation is made without application.

[0078] In some other embodiments, the method for preparing a MOS device further includes, after step S103 , step S1031 : forming a current extension region.

[0079] Specifically, the steps of forming the current extension region include: Fig.10 As shown, an ion implantation process is performed in the drift layer 20 remaining at the bottom of the first trench to form a current extension region 50 having a second doping type.

[0080] The doping concentration of the current extension region is 1.0×10 19 cm -3 ~1.0×1020 cm -3 , the doping concentration of the drift layer is 1.0×10 15 cm -3 ~1.0×10 16 cm -3 , and the doping concentration of the current extension region is 100 to 1000 times that of the drift layer. Under the same level of other conditions, its carrier mobility can be increased by more than 100 times, and the corresponding JFET resistance can be reduced to more than 1 / 100 of it.

[0081] Specifically, the process of forming the first body region, the second body region, the first heavily doped region, the second heavily doped region and the current extension region includes but is not limited to an ion implantation process and a diffusion process, wherein the ion implantation process is to inject a high-energy ion beam into a semiconductor material, and is a process in which ions collide with semiconductor atoms and embed ions into semiconductor crystals. The ion implantation process can accurately control the concentration and depth, and ion doping can be achieved at a lower temperature. The ion implantation equipment is expensive and the cost is high. The diffusion process is a process in which impurity atoms are allowed to diffuse freely along the thermal gradient of the crystal while maintaining thermal equilibrium in the semiconductor through high temperature or chemical reaction to achieve doping. The diffusion process does not require expensive equipment, requires higher control temperature and time conditions, and cannot accurately control the distribution and concentration of impurity atoms. Those skilled in the art can make reasonable selections based on actual needs, and no specific restrictions are made without application.

[0082] In the above embodiment, if Fig.10 As shown, the first source region structure 31 is formed in the first trench, and the second source region structure 32 is formed on the side of the drift layer 20 away from the substrate 10, so that the MOS device has the characteristics of a planar MOS device and a trench MOS device. The body region (including the first body region and the second body region) of the first source region structure forms a vertical channel, and the body region (including the first body region and the second body region) of the second source region structure forms a planar channel, which not only makes the MOS device have a smaller on-resistance, but also can better balance the electric field distribution, so that the electric field originally concentrated in the oxide layer below the gate area and the trench corner is dispersed, reducing the risk of premature gate breakdown.

[0083] Then, step S104: forming a gate structure.

[0084] Specifically, the steps of forming the gate structure include: Fig.11As shown, an oxidation process is used to form a first sub-gate dielectric layer 4021 and a second sub-gate dielectric layer 4022 connected to each other on at least a portion of the first source region structure 31 and the first side surface 321 of the second source region structure 32, wherein the first sub-gate dielectric layer 4021 contacts a portion of the first source region structure 31, the second sub-gate dielectric layer 4022 contacts the second source region structure 32, and the first sub-gate dielectric layer 4021 and the second sub-gate dielectric layer 4022 constitute a first gate dielectric 402; then, as shown in FIG. Fig.12 As shown, the gate 401 is formed by a deposition process on a side of the first sub-gate dielectric layer 4021 facing away from the substrate 10 and a side of the second sub-gate dielectric layer 4022 facing away from the second source region structure 32 .

[0085] The gate material may include doped polysilicon material, which has good stability and compatibility and can improve the conductivity and stability of the MOS device. The thickness of the first sub-gate dielectric perpendicular to the first surface is 400A~800A, and the thickness of the first sub-gate dielectric parallel to the first surface is 400A~800A.

[0086] In some optional embodiments, after performing step S104, the preparation method further includes step S1041: Fig.13 As shown, a second gate dielectric 70 is formed by a deposition process, wherein the second gate dielectric 70 is at least located on a third side surface 4012 and a top surface of the gate 401 opposite to the second side surface 4011 , and the second gate dielectric is respectively in contact with the gate, the first gate dielectric and a portion of the source region structure.

[0087] Specifically, the material of the second gate dielectric may include, but is not limited to, SIO2, Al2O3, AlN, HfO2, and Si3N4, which are not specifically limited in this application. Fig.13The method shown in FIG. 1 may include step S10411: first, a first low-pressure epoxy alkyl silicone oil layer 711 (LPTEOS layer) is formed at least on the third side surface 4012 of the gate 401 by a deposition process, and a second low-pressure epoxy alkyl silicone oil layer 712 is formed at least on the top surface of the gate 401, wherein the first low-pressure epoxy alkyl silicone oil layer 711 is in contact with the first source region structure 31, the first sub-gate dielectric layer 4021 and the gate 401, respectively, and the second low-pressure epoxy alkyl silicone oil layer 712 is in contact with the second source region structure 32, the second sub-gate dielectric layer 4022 and the gate 401; then, A first PETEOS layer 721 (PETEOS layer) is formed on the side of the first low-pressure epoxyalkyl silicone oil layer 711 away from the gate 401 by a deposition process, and a second PETEOS layer 722 is formed on the side of the second low-pressure epoxyalkyl silicone oil layer 712 away from the substrate 10, wherein the first low-pressure epoxyalkyl silicone oil layer 711 and the first PETEOS layer 721 constitute a third sub-gate dielectric 71, the second low-pressure epoxyalkyl silicone oil layer 712 and the second PETEOS layer 722 constitute a fourth sub-gate dielectric 72, and the third sub-gate dielectric 71 and the fourth sub-gate dielectric 72 constitute a second gate dielectric 70.

[0088] Among them, the thicknesses of the first low-pressure epoxy alkyl silicone oil layer 711 and the first tetraethyl orthosilicate layer 721 in a direction parallel to the first surface are 1000A~4000A and 5000~8000A respectively, the thicknesses of the second low-pressure epoxy alkyl silicone oil layer 712 and the second tetraethyl orthosilicate layer 722 in a direction perpendicular to the first surface are 1000A~4000A and 5000~8000A respectively, and the thickness of the third sub-gate dielectric 71 in a direction parallel to the first surface is 6000A-12000A, and the thickness of the fourth sub-gate dielectric 72 in a direction perpendicular to the first surface is 6000A~12000A.

[0089] The above method is used to form the LPTEOS layer and the PETEOS layer in a two-step deposition process, which can not only reduce the preparation cost but also make the MOS device have better voltage resistance performance.

[0090] In some other optional embodiments, the above preparation method further includes step S1042: Fig.14 As shown, a first conductive layer 61 is formed.

[0091] Specifically, the first conductive layer 61 is located on the side of the first heavily doped region 301 and part of the second heavily doped region 302 away from the substrate 10, and the first conductive layer 61 forms an ohmic contact with the first source region structure 31 and the second source region structure 32 respectively. The material of the first conductive layer 61 includes but is not limited to Ni and Ti, and the thickness is 200nm~400nm. The first conductive layer contacts the first heavily doped region 301 and the second heavily doped region 302, forming an ohmic contact, thereby reducing the on-resistance of the MOS device.

[0092] Exemplarily, a first conductive layer is formed using metal Ni, and a method for preparing the first conductive layer includes: first, forming NiSi with a thickness of about 200nm~400nm on the surface of the first heavily doped region and the second heavily doped region at 600℃~800℃, then stripping off unreacted Ni with a Ni etching solution, and performing high-temperature annealing at 900℃~1000℃ to form a first conductive layer of metal Ni.

[0093] In the above embodiment, the above preparation method further includes step S1043: Fig.15 As shown, a second conductive layer 62 and a third conductive layer 63 are formed.

[0094] Specifically, the second conductive layer 62 is located on the side of the first conductive layer 61, the gate structure 40, the second gate dielectric 70, the first source region structure 31 and the second source region structure 32 away from the substrate 10, and the second conductive layer 62 is respectively in contact with the first conductive layer 61, the second gate dielectric 70 and part of the first source region structure 31 and part of the second source region structure 32; the third conductive layer 63 is located on the side of the substrate 10 away from the drift layer 20, wherein the second conductive layer 62 and the third conductive layer 63 respectively serve as the source electrode and the drain electrode of the MOS device, playing the role of current input and output of the MOS device.

[0095] Among them, the materials of the second conductive layer and the third conductive layer include but are not limited to alloy materials composed of any one or more of Ag, Cu, Al, Au, Ti, Ni, Pt and Pb metals. Technical personnel in this field can make reasonable selections according to actual needs, and no specific limitations are made without application.

[0096] Exemplarily, the material of the second conductive layer includes AlCu with a thickness of 2 μm to 6 μm, and the material of the third conductive layer includes TiNiAg with a thickness of 200 nm to 400 nm. Both AlCu and TiNiAg have good conductivity, which improves the conductivity of the device.

[0097] It should be noted that the above-mentioned steps S1031: forming a current extension region, step S104: forming a gate structure, step S1041: forming a second gate dielectric, step S1042: forming a first conductive layer, step S1043: forming a second conductive layer and a third conductive layer are also applicable to the following steps: Figure 7 In the structure shown, the preparation method is the same as Fig. 9 The structures shown are the same and have the same technical effects, so they will not be described in detail here.

[0098] The MOS device formed by the MOS device preparation method of the present application will be described below in conjunction with an embodiment.

[0099] Example:

[0100] The method for preparing a MOS device provided in this embodiment comprises the following steps:

[0101] Provide an N-type SiC substrate 10, whose resistivity is 0.02Ωcm, such as Figure 3 As shown;

[0102] An N-type SiC drift layer 20 is formed on the N-type SiC substrate 10 by using an epitaxial growth process. The doping concentration of the N-type SiC drift layer 20 is 1.0×10 15 cm -3 ,like Figure 3 As shown;

[0103] A first trench 33 is formed on the N-type SiC drift layer 20 by an etching process. Figure 4 As shown;

[0104] A P-type Si layer is formed on the bottom of the first trench and the preliminary drift layer 21 by a deposition process to form a first material layer 3031, wherein the preliminary drift layer 21 is a portion of the drift layer 20 located on the side of the first trench away from the first material layer 3031, such as Figure 5 As shown;

[0105] The first material layer 3031 of N-type Si and the drift layer 20 below the first material layer 3031 are also implanted with Al ions by an ion implantation process, so that the first material layer 3031 forms a P-type Si first body region 303 and a P-type SiC second body region 304, wherein the doping concentrations of the P-type Si first body region 303 and the P-type SiC second body region 304 are both 1.0×10 17 cm -3 ,like Figure 8 As shown;

[0106] The first body region 303 is doped with Al ions and N ions respectively by ion implantation to form a P-type first heavily doped region 301 and an N-type second heavily doped region 302. The doping concentration of the first heavily doped region 301 is 1.0×10 19 cm -3 , the doping concentration of the second heavily doped region 302 is 1.0×10 19 cm -3 ,like Fig. 9 As shown;

[0107] An N ion implantation process is performed in the remaining drift layer 20 at the bottom of the first trench to form an N-type current extension region 50. The doping concentration of the current extension region is 1.0×10 19 cm -3 ,like Fig.10 As shown;

[0108] An oxidation process is used to form a first sub-gate dielectric layer 4021 and a second sub-gate dielectric layer 4022 connected to each other on at least a portion of the first source region structure 31 and the first side surface 321 of the second source region structure 32, wherein the materials of the first sub-gate dielectric layer 4021 and the second sub-gate dielectric layer 4022 are both silicon oxide materials, the first sub-gate dielectric layer 4021 and the second sub-gate dielectric layer 4022 constitute the first gate dielectric 402, the second sub-gate dielectric layer 4022 has a thickness of 600A perpendicular to the first surface, and the first sub-gate dielectric has a thickness of 600A parallel to the first surface, such as Fig.11 As shown;

[0109] Polysilicon material is deposited on the side of the first sub-gate dielectric layer 4021 facing away from the substrate 10 and the side of the second sub-gate dielectric layer 4022 facing away from the second source region structure 32 by a deposition process to form the gate 401. Fig.12 As shown;

[0110] A first low-pressure epoxy alkyl silicone oil layer 711 (LPTEOS layer) is formed at least on the third side surface 4012 of the gate 401 by a deposition process, and a second low-pressure epoxy alkyl silicone oil layer 712 is formed at least on the top surface of the gate 401, wherein the first low-pressure epoxy alkyl silicone oil layer 711 is in contact with the first source region structure 31, the first sub-gate dielectric layer 4021 and the gate 401, respectively, and the second low-pressure epoxy alkyl silicone oil layer 712 is in contact with the second source region structure 32, the second sub-gate dielectric layer 4022 and the gate 401, as shown in FIG. Fig.13 As shown;

[0111] A first PETEOS layer 721 (PETEOS layer) is formed on a side of the first low-pressure epoxyalkyl silicone oil layer 711 away from the gate 401 by a deposition process, and a second PETEOS layer 722 is formed on a side of the second low-pressure epoxyalkyl silicone oil layer 712 away from the substrate 10, wherein the first low-pressure epoxyalkyl silicone oil layer 711 and the first PETEOS layer 721 constitute a third sub-gate dielectric 71, and the second low-pressure epoxyalkyl silicone oil layer 712 and the second PETEOS layer 722 constitute a fourth sub-gate dielectric 72. The third sub-gate dielectric 71 and the fourth sub-gate dielectric 72 are both treated at 100° C. to form SiO2 to form a second gate dielectric 70, as shown in FIG. Fig.13 As shown;

[0112] NiSi is formed on the surface of the P-type first heavily doped region 301 and the N-type second heavily doped region by a deposition process at 700° C., and then unreacted Ni is stripped off by a Ni etching solution, and a high-temperature annealing treatment is performed at 950° C. to form a first conductive layer 61 of metal Ni. Fig.14 As shown;

[0113] An AlCu layer with a thickness of 4 μm is formed on the side of the first conductive layer 61, the gate structure 40, the second gate dielectric 70, the first source region structure 31 and the second source region structure 32 away from the substrate 10 by a deposition process to form a second conductive layer 62. Fig.15 As shown;

[0114] A TiNiAg alloy layer with a thickness of 300 nm is formed on the side of the substrate 10 away from the drift layer 20 by a deposition process to form a third conductive layer 63. Fig.15 shown.

[0115] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.

[0116] The above are only embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included within the scope of the claims of the present application.

Claims

1. A MOS device, characterized in that: include: A substrate and a drift layer on one side of the substrate, wherein the drift layer has a first surface facing away from the substrate, and the MOS device further comprises: at least one source region structure, the source region structure comprising a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region having a first doping type, the second heavily doped region having a second doping type, the first body region being located at least on a side of the first heavily doped region and the second heavily doped region close to the substrate, and the first body region and the drift layer having different semiconductor materials; A gate structure, the gate structure comprising a gate and a first gate dielectric, the first gate dielectric being at least located between the gate and the source region structure, wherein the first gate dielectric is in contact with at least the first body region and the second heavily doped region.

2. The MOS device according to claim 1, characterized in that: The source region structure further includes: The second body region is located on a side of the first body region close to the substrate and in contact with the first body region. The second body region has the first doping type, and the second body region and the drift layer have the same semiconductor material.

3. The MOS device according to claim 2, characterized in that: The material of the first body region includes silicon material, and the material of the second body region includes silicon carbide material.

4. The MOS device according to any one of claims 1 to 3, characterized in that: The source region structure comprises a first source region structure and a second source region structure, the first source region structure has a second surface away from the substrate, the first source region structure is located in the drift layer and the second surface is located in the first surface, the second source region structure is located on a side of the drift layer away from the substrate, and the first source region structure is not in contact with the second source region structure; The gate structure is located on a side of the drift layer away from the substrate, and the gate structure is in contact with a first side of the second source region structure and a portion of the second surface of the first source region structure respectively, wherein the first side is a side of the second source region structure close to the first source region structure.

5. The MOS device according to claim 4, characterized in that: Also includes: A current extension region is located in the drift layer and contacts the first source region structure. A side of the current extension region facing away from the first source region structure contacts the first side. The current extension region has a second doping type.

6. The MOS device according to claim 5, characterized in that: The doping concentration of the current extension region is 100 to 1000 times the doping concentration of the drift layer.

7. The MOS device according to claim 1, characterized in that: Also includes: A first conductive layer, wherein the first conductive layer is located on a side of the first heavily doped region and a portion of the second heavily doped region away from the substrate, and the first conductive layer forms an ohmic contact with the source region structure.

8. A method for preparing a MOS device, characterized in that: Used to prepare the MOS device according to any one of claims 1 to 7, the preparation method comprising: providing a substrate; forming a drift layer on the substrate, the drift layer having a first surface facing away from the substrate; forming a source region structure, the source region structure comprising a first heavily doped region, a second heavily doped region and a first body region, the first heavily doped region and the first body region having a first doping type, the second heavily doped region having a second doping type, the first body region being at least located on a side of the first heavily doped region and the second heavily doped region close to the substrate, and the first body region and the drift layer having different semiconductor materials; A gate structure is formed, wherein the gate structure includes a gate and a first gate dielectric, wherein the first gate dielectric is at least located between the gate and the source region structure, wherein the first gate dielectric is in contact with at least the first body region and the second heavily doped region.

9. The preparation method according to claim 8, characterized in that: The steps of forming the source region structure include: forming a first material layer on each of the drift layers using a deposition process; Implanting ions into the first material layer respectively by using an ion implantation process to form the first body region; Ion implantation of different doping types is performed in the first body region by adopting an ion implantation process to form the first heavily doped region and the second heavily doped region.

10. The preparation method according to claim 9, characterized in that: The second body region is located on a side of the first body region close to the substrate and in contact with the first body region. The preparation steps include: Ions are injected into the first material layer and the second material layer, the first material layer forms the first body region, and the second material layer forms the second body region, wherein the second material layer is a portion of the drift layer located in contact with the first material layer, and a ratio of ion injection depths of the first material layer and the second material layer in a second direction is 1:2~1:6, and the second direction is perpendicular to the first surface.

Citation Information

Patent Citations

  • Semiconductor device having dual parallel channel structure and method of fabricating the same

    CN103928516A

  • Trench gate VDMOS with heterojunction and preparation method

    CN117423729A

  • Planar VDMOS with heterojunction and preparation method

    CN117438446A

  • Groove type MOSFET and manufacturing method thereof

    CN117613069A

  • Method of fabrication semiconductor device forpreventing residue in moat region

    KR1020050040574A

Cited By

  • Field effect transistor and preparation method thereof

    CN119300426A