Pole piece insulation treatment method and pole piece manufacturing equipment

By cutting the pole sheet into sub-pole sheets and forming an insulating layer on its edges, the problem of pole sheet burrs piercing the isolation film is solved, and the reliability and stability of the battery are improved.

CN119069614AActive Publication Date: 2024-12-03CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310627352.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

During the battery manufacturing process, the burrs generated after the pole slicing are prone to pierce the isolation film, resulting in short circuits inside the battery cell and reducing the reliability of the battery.

Method used

Cut the pole sheet into multiple sub-pole sheets, wind it up to form the pole sheet roll, and transfer the insulating coating to the slicing edge of the sub-pole sheet to form an insulating layer to cover the burrs generated after the current collector is cut, Reduce the risk of burrs piercing the isolation membrane.

Benefits of technology

The reliability of the battery is improved, and the risk of burrs piercing the isolation film is reduced through the insulation effect of the insulating layer, thereby enhancing the stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069614A_ABST
    Figure CN119069614A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a pole piece insulation treatment method and pole piece manufacturing equipment. The pole piece insulation treatment method comprises the following steps: slitting a pole piece into a plurality of sub pole pieces; the sub-pole pieces are wound to form a pole piece coiled material, and the pole piece coiled material comprises a first end face formed by the slitting edges of the sub-pole pieces; and transferring an insulating coating to the first end surface to form an insulating layer which at least covers the current collector of the sub-pole piece and burrs generated after the current collector is cut. The pole piece manufactured according to the technical scheme provided by the embodiment of the invention can improve the reliability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a pole piece insulation processing method and pole piece manufacturing equipment. Background Art

[0002] Energy conservation and emission reduction are the key to the sustainable development of the automobile industry. Electric vehicles have become an important part of the sustainable development of the automobile industry due to their advantages in energy conservation and environmental protection. For electric vehicles, battery technology is an important factor in their development.

[0003] During the manufacturing process of batteries, the reliability of batteries is an issue that cannot be ignored. Therefore, how to improve the reliability of batteries is a technical problem that needs to be solved urgently in battery technology. Summary of the invention

[0004] The present application provides a pole piece insulation processing method and a pole piece manufacturing device, and the manufactured pole piece can improve the reliability of the battery.

[0005] This application is achieved through the following technical solutions:

[0006] In a first aspect, an embodiment of the present application provides a method for insulating a pole piece, comprising: cutting a pole piece into a plurality of sub-pole pieces; rolling up the sub-pole pieces to form a pole piece roll, wherein the pole piece roll comprises a first end face formed by the cut edges of the sub-pole pieces; transferring an insulating coating to the first end face to form an insulating layer that at least covers the current collector of the sub-pole pieces and burrs generated after the current collector is cut.

[0007] According to the electrode sheet insulation processing method of the embodiment of the present application, after the electrode sheet is cut into a plurality of sub-electrode sheets, the sub-electrode sheets are wound to form a electrode sheet coil, and the insulating coating is transferred to the first end surface formed after the sub-electrode sheets are cut, so that an insulating layer is formed on the first end surface. The operation is simple, and the insulation processing efficiency of the cut edge of the sub-electrode sheet is high. At the same time, the insulating layer can at least cover the current collector and the burrs generated after the current collector is cut, that is, the insulating layer covers the current collector and part of the active material layer, so that the burrs are blocked. Since the insulating layer has an insulating effect, the insulating layer can block the burrs while reducing the risk of the burrs piercing the isolation membrane and causing an internal short circuit, so that the battery can have a higher reliability.

[0008] According to some embodiments of the present application, transferring the insulating coating to the first end face includes: rotating the pole piece coil, and transferring the insulating coating to the first end face by rotating a coating roller.

[0009] In the above scheme, the insulating coating is transferred to the first end surface by rotating the coating roller, which can improve the coating efficiency and is simple to operate.

[0010] According to some embodiments of the present application, the coating roller rotates in the same direction as the pole piece coil.

[0011] In the above scheme, the coating roller and the pole piece coil rotate in the same direction, so that the friction between the coating roller and the first end surface is small, so that the insulating coating on the coating roller can adhere to the first end surface.

[0012] According to some embodiments of the present application, the rotation speed of the coating roller is the same as the rotation speed of the pole piece coil.

[0013] In the above scheme, the rotation speed of the coating roller is the same as the rotation speed of the pole piece coil, and the coating roller and the first end surface are relatively stationary, which reduces friction, extends the service life of the coating roller, reduces damage to the first end surface, and enables the insulating coating to cover the first end surface evenly.

[0014] According to some embodiments of the present application, before rotating the pole piece coil, the pole piece insulation processing method further includes: the first end surface is arranged along a vertical direction.

[0015] In the above scheme, the first end face is arranged in the vertical direction, and the pole piece coil occupies a smaller space in the horizontal direction, reducing the risk of interference between the pole piece coil and other components (such as a glue coating device, a container for insulating coating, etc.).

[0016] According to some embodiments of the present application, the coating roller is a tapered roller, and the angle between the generatrix of the coating roller and the central axis of the coating roller is α, satisfying 30°≤α≤60°.

[0017] In the above scheme, the angle α between the busbar of the coating roller and the central axis of the coating roller satisfies the above relationship (30°≤α≤60°), which is convenient for the reasonable arrangement of the pole piece coil. The pole piece coil is not easy to interfere with other components (such as the gluing device, the container for the insulating coating, etc.), so as to facilitate the transfer of the insulating coating to the first end face.

[0018] According to some embodiments of the present application, α=45°.

[0019] In the above scheme, when α=45°, the pole piece coil 111 occupies a smaller space in the horizontal direction, reducing the risk of interference between the pole piece coil 111 and other components (such as a glue coating device, a container for insulating coating, etc.).

[0020] According to some embodiments of the present application, rotating the pole piece coil to transfer the insulating coating to the first end face by rotating a coating roller includes: before transferring the insulating coating to the first end face by rotating the coating roller, scraping off excess insulating coating by a scraper.

[0021] In the above scheme, by scraping off excess insulating coating with a scraper, the thickness of the insulating coating attached to the roller surface of the coating roller can be controlled, thereby controlling the thickness of the insulating coating attached to the first end surface, and further achieving control of the thickness of the insulating layer.

[0022] According to some embodiments of the present application, before rotating the pole piece coil and transferring the insulating coating to the first end face by rotating a coating roller, the pole piece insulation processing method further includes: adjusting the gap between the scraper and the coating roller to control the thickness of the insulating coating attached to the coating roller.

[0023] In the above scheme, by adjusting the gap between the scraper and the coating roller, the thickness of the insulating coating attached to the coating roller can be controlled according to different coating requirements, so as to control the thickness of the insulating layer attached to the first end face.

[0024] According to some embodiments of the present application, the solid content of the insulating coating is 10% to 30%.

[0025] In the above scheme, the solid content of the insulating coating satisfies the above relationship. On the one hand, it is easy to adhere to the first end face, and the thickness of the insulating layer after drying is thicker, which has a better insulation effect; on the other hand, the insulating layer is not easy to accumulate on the first end face, reducing the risk of the insulating layer adhering to the two adjacent circles of pole pieces. If the solid content of the insulating coating is small (such as less than 10%), the thickness of the insulating layer after drying is small, and the insulation effect is poor; if the solid content of the insulating coating is large (such as greater than 30%), the insulating layer is easy to accumulate on the first end face, which easily causes the insulating layer to adhere to the two adjacent circles of pole pieces.

[0026] According to some embodiments of the present application, the solid content of the insulating coating is 12% to 18%.

[0027] In the above scheme, compared with the solid content of the insulating coating being less than 12%, when the solid content of the insulating coating is greater than or equal to 12%, the thickness of the insulating layer attached to the first surface is thicker and has a better insulation effect; compared with the solid content of the insulating coating being greater than 18%, when the solid content of the insulating coating is less than or equal to 18%, the insulating coating is not easy to accumulate on the first end face, reducing the risk of the insulating layer adhering to the two adjacent circles of pole pieces.

[0028] In the second aspect, the embodiment of the present application also provides a pole piece manufacturing device, including a slitting device, a winding device, a driving device and a coating device. The slitting device is used to slit the pole piece into a plurality of sub-pole pieces; the winding device is used to wind up the sub-pole piece to form a pole piece coil, the pole piece coil includes a first end face formed by the slitting edge of the sub-pole piece; the coating device is used to transfer the insulating coating to the first end face to form an insulating layer that at least covers the current collector of the sub-pole piece and the burrs generated after the current collector is cut.

[0029] According to the pole piece manufacturing equipment of the embodiment of the present application, the pole piece is cut into a plurality of sub-pole pieces by a cutting device, which can improve the pole piece manufacturing efficiency; the sub-pole pieces are rolled up by a collecting device, and the insulating coating is transferred to the first end face by a coating device, so that the insulating coating can be coated on all the cut edges of the sub-pole pieces to form an insulating layer on the first end face. The pole piece prepared by the pole piece manufacturing equipment has an insulating layer formed on the first end face of the cut edge, and the insulating layer can cover the current collector and the burrs generated after the current collector is cut. After forming a battery cell, the insulating layer can reduce the risk of burrs piercing the isolation membrane and causing an internal short circuit in the battery cell, so that the battery cell has a higher reliability.

[0030] According to some embodiments of the present application, the pole piece manufacturing equipment further includes a driving device, which is used to drive the pole piece coil to rotate.

[0031] In the above scheme, the pole piece coil is driven to rotate by a driving device so that the insulating coating can be evenly coated on the first end surface.

[0032] According to some embodiments of the present application, the pole piece manufacturing equipment also includes a first container, the first container is used to contain the insulating coating, the coating device includes a coating roller and a coating roller driving member, the coating roller is transmission-connected to the coating roller driving member, and the coating roller driving member is used to drive the coating roller to rotate so as to transfer the insulating coating in the first container to the first end face.

[0033] In the above scheme, the insulating coating in the first container is transferred to the first end surface by the rotation of the coating roller, so that the coating efficiency is high and the operation is simple.

[0034] According to some embodiments of the present application, the coating roller is a tapered roller, and the angle between the generatrix of the coating roller and the central axis of the coating roller is α, satisfying 30°≤α≤60°.

[0035] In the above scheme, the coating roller is a tapered roller, and α satisfies the above relationship, which is convenient for reasonably arranging the pole piece coil, the pole piece coil occupies a small space, and the pole piece coil is not easy to interfere with other components (such as a coating device, a container for containing insulating paint, etc.), so as to facilitate the transfer of the insulating paint in the first container to the first end face. If α is small (such as less than 60°) or α is large (such as greater than 120°), the pole piece coil is easy to interfere with other components (such as a coating device, a container for containing insulating paint, etc.).

[0036] According to some embodiments of the present application, α=45°.

[0037] In the above scheme, when α=45°, the first end face can be set in the vertical direction, and the coating roller can apply the insulating coating in a horizontal state to the vertically set first end face. The pole piece coil occupies a smaller space in the horizontal direction, reducing the risk of interference between the pole piece coil and other components (such as a gluing device, a container for containing insulating coating, etc.).

[0038] According to some embodiments of the present application, the pole piece manufacturing equipment also includes a scraper, which is arranged in the first container, and the scraper and the coating roller are spaced apart, and the gap between the scraper and the coating roller is adjustable to control the thickness of the insulating coating attached to the coating roller.

[0039] In the above scheme, the scraper and the coating roller are spaced apart, and the gap between the scraper and the coating roller is adjustable to control the thickness of the insulating coating attached to the coating roller, thereby controlling the thickness of the insulating layer on the first end face to meet the coating requirements.

[0040] According to some embodiments of the present application, the scraper is arranged parallel to the roller surface of the coating roller.

[0041] In the above scheme, the scraper is arranged parallel to the roller surface of the coating roller so that the gap between the scraper and the roller surface of the coating roller at any position along the extension direction of the scraper is the same, that is, the thickness of the insulating coating attached at any position of the coating roller is the same, so that the thickness of the insulating coating on the roller surface of the coating roller is highly consistent.

[0042] According to some embodiments of the present application, the pole piece manufacturing equipment further includes: a stirring device for stirring the insulating coating located in the first container.

[0043] In the above solution, the provision of the stirring device can make the components of the insulating coating mixed evenly, so that the thickness of the insulating layer formed on the first end surface is uniform.

[0044] According to some embodiments of the present application, the pole piece manufacturing equipment also includes: a circulation device, including a second container, a pipeline and a circulation pump, the second container is connected to the first container through the pipeline, and the circulation pump is used to drive the insulating coating to circulate between the first container and the second container.

[0045] In the above scheme, the insulating coating is driven to circulate between the first container and the second container by a circulation pump, so that the components of the insulating coating are evenly mixed, and the thickness of the insulating layer formed on the first end surface is uniform.

[0046] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0048] Figure 1 A schematic flow chart of a pole piece insulation treatment method provided in some embodiments of the present application;

[0049] Figure 2 A schematic diagram of a pole piece cutting process provided in some embodiments of the present application;

[0050] Figure 3 A schematic diagram of a coating device provided in some embodiments of the present application coating an insulating coating on a first end surface;

[0051] Figure 4 A schematic flow chart of the step of "transferring the insulating coating to the first end surface" provided in some embodiments of the present application;

[0052] Figure 5 A schematic flowchart of a pole piece insulation treatment method provided in some other embodiments of the present application;

[0053] Figure 6 A schematic block diagram of the structure of a pole piece manufacturing device provided in some embodiments of the present application;

[0054] Figure 7 A partial structural schematic diagram of a pole piece manufacturing device provided in some embodiments of the present application;

[0055] Figure 8 A schematic diagram of the structure of a stirring device provided in some embodiments of the present application;

[0056] Fig. 9 A schematic diagram of the structure of a circulation device provided in some embodiments of the present application.

[0057] Icons: 100-slitting device; 10-pole piece; 11-sub-pole piece; 111-pole piece coil; 112-first end face; 200-winding device; 21-winding roller; 300-coating device; 31-coating roller; 32-coating roller drive; 400-drive device; 500-first container; 600-scraper; 700-stirring device; 71-stirring paddle; 72-stirring drive; 800-circulation device; 81-second container; 82-pipeline; 83-circulation pump. DETAILED DESCRIPTION

[0058] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0059] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by technicians in the technical field of this application; the terms used in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned drawings and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", etc. in the specification and claims of this application or the above-mentioned drawings are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship.

[0060] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this application may be combined with other embodiments.

[0061] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", and "attached" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0062] The term "and / or" in this application is only a description of the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this application generally indicates that the associated objects before and after are in an "or" relationship.

[0063] The term "multiple" as used in the present application refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple sheets" refers to more than two sheets (including two sheets).

[0064] In some embodiments, the battery may be a battery module. When there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module.

[0065] In some embodiments, the battery may be a battery pack, which includes a case and battery cells, wherein the battery cells or battery modules are accommodated in the case.

[0066] In some embodiments, the box body can be used as a part of the chassis structure of the vehicle. For example, part of the box body can become at least a part of the floor of the vehicle, or part of the box body can become at least a part of the cross beam and longitudinal beam of the vehicle.

[0067] In some embodiments, the battery may be an energy storage device, which includes an energy storage container, an energy storage cabinet, and the like.

[0068] In the embodiment of the present application, the battery cell may be a secondary battery. A secondary battery refers to a battery cell that can be continuously used by activating active materials by charging after the battery cell is discharged.

[0069] The battery cells may be, but are not limited to, lithium ion batteries, sodium ion batteries, sodium lithium ion batteries, lithium metal batteries, sodium metal batteries, lithium sulfur batteries, magnesium ion batteries, nickel hydrogen batteries, nickel cadmium batteries, lead storage batteries, etc.

[0070] A battery cell generally includes an electrode assembly. The electrode assembly includes a positive electrode, a negative electrode, and a separator. During the charge and discharge process of the battery cell, active ions (such as lithium ions) are embedded and removed between the positive electrode and the negative electrode. The separator is set between the positive electrode and the negative electrode to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through.

[0071] In some embodiments, the positive electrode may be a positive electrode sheet, and the positive electrode sheet may include a positive electrode current collector and a positive electrode active material disposed on at least one surface of the positive electrode current collector.

[0072] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material is disposed on either or both of the two facing surfaces of the positive electrode current collector.

[0073] As an example, the positive electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum with a silver-plated surface, stainless steel with a silver-plated surface, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc., may be used. The composite current collector may include a polymer material base and a metal layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).

[0074] As an example, the positive electrode active material may include at least one of the following materials: lithium-containing phosphates, lithium transition metal oxides, and their respective modified compounds. However, the present application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used.

[0075] In some embodiments, the negative electrode may be a negative electrode sheet, and the negative electrode sheet may include a negative electrode current collector.

[0076] As an example, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, aluminum with a silver-plated surface, stainless steel with a silver-plated surface, stainless steel, copper, aluminum, nickel, carbon electrode, carbon, nickel or titanium, etc. may be used.

[0077] In some embodiments, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode active material is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0078] As an example, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0079] In some embodiments, the separator is a separator. The present application has no particular limitation on the type of separator, and any known separator with a porous structure having good chemical stability and mechanical stability can be selected.

[0080] As an example, the main material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, polyvinylidene fluoride, and ceramic. The separator can be a single-layer film or a multi-layer composite film, without special restrictions. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions. The separator can be a separate component located between the positive and negative electrodes, or it can be attached to the surface of the positive and negative electrodes.

[0081] In some embodiments, the electrode assembly is a wound structure, wherein the positive electrode sheet and the negative electrode sheet are wound into the wound structure.

[0082] In some embodiments, the electrode assembly is a laminate structure.

[0083] As an example, the battery cell can be a cylindrical battery cell, a prismatic battery cell, a soft-pack battery cell or a battery cell of other shapes. The prismatic battery cell includes a square shell battery cell, a blade-shaped battery cell, a polygonal prismatic battery, such as a hexagonal prismatic battery, etc. There is no particular limitation in the embodiments of the present application.

[0084] The development of battery technology must take into account many design factors at the same time, such as energy density, discharge capacity, charge and discharge rate and other performance parameters. In addition, battery reliability must also be considered.

[0085] During the battery production process, the pole piece production process includes a slitting process, in which the pole piece is cut into multiple sub-pole pieces. The pole piece is usually cut by a rolling cutter, which includes an upper cutter and a lower cutter. The upper cutter and the lower cutter are staggered and bite close to each other. The upper cutter and the lower cutter rotate synchronously in opposite directions, and the pole piece is sheared apart by the staggered bite of the upper cutter and the lower cutter. Since the upper cutter and the lower cutter are staggered and bite close to each other, the bite part is worn and consumed, resulting in blade blunting and chipping. In the manufacturing process of battery cells, it is necessary to deal with different material formulations and process requirements. The different working conditions of the pole piece tending to be thickly coated or thinly coated will cause metal burrs to form on the cutting edge, that is, burrs are generated after the current collector is cut. After the battery cell is formed, the oversized burrs are easy to pierce the isolation membrane, causing internal short circuits in the battery cell, and even fire and explosion, making the reliability of the battery cell low.

[0086] In view of this, in order to solve the problem of burrs piercing the isolation membrane and causing low reliability of the battery cell, an embodiment of the present application provides a technical solution, in which the pole piece is cut into a plurality of sub-pole pieces, and the sub-pole pieces are wound to form a pole piece coil, and the pole piece coil includes a first end face formed by the cut edges of the sub-pole pieces, and the insulating coating is transferred to the first end face to form an insulating layer on the first end face. The insulating layer can cover the burrs generated after the current collector is cut, thereby reducing the risk of burrs piercing the isolation membrane and improving the reliability of the battery cell.

[0087] The pole piece prepared by the above-mentioned pole piece insulation treatment method transfers the insulating coating to the first end face formed after the sub-pole piece is cut, so that an insulating layer is formed on the first end face, and the insulating layer can at least cover the current collector and the burrs generated after the current collector is cut, that is, the insulating layer covers the current collector and part of the active material layer, so that the burrs are blocked. Since the insulating layer has an insulating effect, the insulating layer can block the burrs while reducing the risk of the burrs piercing the isolation membrane and causing an internal short circuit, so that the battery can have higher reliability.

[0088] Please refer to Figures 1 to 3 , Figure 1 A schematic flow chart of a pole piece insulation treatment method provided in some embodiments of the present application; Figure 2A schematic diagram of a pole piece cutting process provided in some embodiments of the present application;

[0089] Figure 3 A schematic diagram of a coating device provided in some embodiments of the present application coating an insulating coating on a first end surface. According to some embodiments of the present application, an embodiment of the present application provides a method for insulating a pole piece, comprising:

[0090] S110, cutting the pole piece 10 into a plurality of sub-pole pieces 11;

[0091] S120, rolling up the sub-pole sheet 11 to form a pole sheet coil 111, wherein the pole sheet coil 111 includes a first end surface 112 formed by the cut edges of the sub-pole sheet 11;

[0092] S130, transferring the insulating coating to the first end surface 112 to form an insulating layer that at least covers the current collector of the sub-pole sheet 11 and burrs generated after the current collector is cut.

[0093] During the manufacturing process of the pole piece 10, the pole piece 10 is a continuous strip structure, and the pole piece 10 has a certain width. The pole piece 10 can be cut into a plurality of sub-pole pieces 11 to improve the manufacturing efficiency of the pole piece 10. For example, the pole piece 10 can be cut into two sub-pole pieces 11, three sub-pole pieces 11, or more than three sub-pole pieces 11. In some embodiments, the sub-pole piece 11 can be called the pole piece 10.

[0094] The sub-pole sheet 11 is rolled up on the winding roller 21 to form a pole sheet coil 111. The first end face 112 is formed by the cut edge of the sub-pole sheet 11. The first end face 112 as a whole can be annular, and the first end face 112 has an inner circle and an outer circle. The inner circle of the first end face 112 can be wound around the roller surface of the winding roller 21.

[0095] Since the sub-pole sheet 11 is a strip-shaped continuous structure, burrs are formed on the cut edges of the sub-pole sheet 11. The sub-pole sheet 11 is rolled up to form a pole sheet coil 111, so that insulating paint can be applied to the cut edges of the sub-pole sheet 11, so that the insulating paint can be attached to all the cut edges.

[0096] In step “ S130 , transferring the insulating coating to the first end surface 112 ”, the insulating coating may be applied to the first end surface 112 manually, or by a coating roller 31 of a coating device 300 .

[0097] When observed in a direction perpendicular to the first end face 112, the burrs generated after the current collector is cut partially overlap with the active material layer. When the insulating coating is transferred to the first end face 112, the insulating layer covers the current collector and at least part of the active material layer, that is, the insulating layer partially overlaps with the active material layer in the thickness direction of the sub-pole sheet 11, so that the insulating layer at least covers the current collector of the sub-pole sheet 11 and the burrs generated after the current collector is cut.

[0098] The insulating coating may include a solid insulating material, a binder and a solvent. The solid insulating material may be selected from BaSO 4 、CaSiO 3 ,γ-AlOOH,CaSiO 4 , polytetrafluoroethylene. The binder is selected from at least one of polyvinylidene fluoride binder, styrene-butadiene rubber binder, polyetherimide binder, sodium polyacrylate binder, polytetrafluoroethylene binder, acrylate binder, and carboxymethyl cellulose binder. The solvent is selected according to the properties of the binder. When the binder is a water-based binder, a water-based solvent (such as distilled water, etc.) can be selected; when the binder is an oily binder, an oily solvent (such as N-methylpyrrolidone, etc.) can be selected.

[0099] According to the electrode sheet insulation processing method of the embodiment of the present application, after the electrode sheet 10 is cut into a plurality of sub-electrode sheets 11, the sub-electrode sheets 11 are wound to form a electrode sheet coil 111, and the electrode sheet coil 111 is rotated to transfer the insulating coating to the first end face 112 formed after the sub-electrode sheet 11 is cut, so that an insulating layer is formed on the first end face 112. The operation is simple, and the insulation processing efficiency of the cut edge of the sub-electrode sheet 11 is high. At the same time, the insulating layer can at least cover the burrs generated after the current collector and the current collector are cut, that is, the insulating layer covers the current collector and part of the active material layer, so that the burrs are blocked. Since the insulating layer has an insulating effect, the insulating layer can block the burrs while reducing the risk of the burrs piercing the isolation membrane and causing an internal short circuit, so that the battery can have a higher reliability.

[0100] Please refer to Figure 4 , Figure 4 A schematic flow chart of the step "transferring the insulating coating to the first end face" provided for some embodiments of the present application. According to some embodiments of the present application, transferring the insulating coating to the first end face 112 includes:

[0101] S131 , rotating the pole piece coil 111 , and transferring the insulating coating to the first end surface 112 by rotating the coating roller 31 .

[0102] The pole piece coil 111 is rotated so that the insulating coating covers the inner circle and the outer circle of the first end surface 112 , thereby improving the thickness uniformity of the insulating coating attached to the first end surface 112 .

[0103] During the rotation of the coating roller 31 , the insulating coating material adheres to the roller surface of the coating roller 31 . As the coating roller 31 rotates, the coating roller 31 transfers the insulating coating material to the first end surface 112 to form an insulating layer on the first end surface 112 .

[0104] For example, when the coating roller 31 rotates, it first rotates to the container containing the insulating coating, the roller surface of the coating roller 31 is soaked with the insulating coating, and the insulating coating adheres to the roller surface of the coating roller 31. As the coating roller 31 rotates, the insulating coating on the roller surface contacts the first end face 112, and the insulating coating adheres to the first end face 112, thereby forming an insulating layer.

[0105] When the coating roller 31 is coating the insulating coating, the pole piece coil 111 is also rotated, so that the insulating coating can be coated on the inner circle and the outer circle of the first end surface 112 .

[0106] In the above solution, the insulating coating is transferred to the first end surface 112 by rotating the coating roller 31, which can improve the coating efficiency and is simple to operate.

[0107] Please refer to Figure 3 According to some embodiments of the present application, the coating roller 31 rotates in the same direction as the pole piece coil 111 .

[0108] The coating roller 31 rotates in the same direction as the pole piece coil 111 , so that the friction between the coating roller 31 and the first end surface 112 is small, so that the insulating paint on the coating roller 31 adheres to the first end surface 112 .

[0109] Please refer to Figure 3 According to some embodiments of the present application, the rotation speed of the coating roller 31 is the same as the rotation speed of the pole piece coil 111 .

[0110] The rotation speed of the coating roller 31 is the same as the rotation speed of the pole piece coil 111, that is, the ratio of the rotation speed of the coating roller 31 to the rotation speed of the pole piece coil 111 is 1:1. Combined with the coating roller 31 and the pole piece coil 111 rotating in the same direction, the coating roller 31 and the first end face 112 are relatively stationary, which reduces friction, extends the service life of the coating roller 31, reduces damage to the first end face 112, and enables the insulating coating to cover the first end face 112 evenly.

[0111] Please refer to Figure 5 , Figure 5 A schematic flow chart of a method for insulating a pole piece provided in some other embodiments of the present application. According to some embodiments of the present application, before rotating the pole piece coil 111, the method for insulating a pole piece further includes:

[0112] S130a, the first end surface 112 is arranged along the vertical direction.

[0113] If the first end face 112 is arranged in the horizontal direction, the coating roller 31 applies the insulating coating above or below the first end face 112. When the coating roller 31 applies the insulating coating above the first end face 112, the insulating coating is easy to drip onto the first end face 112, making the thickness of the insulating layer formed on the first end face 112 uneven. When the coating roller 31 applies the insulating coating below the first end face 112, the pole sheet coil 111 is rotated, and the pole sheet coil 111 is easy to detach from the winding roller 21, that is, the pole sheet coil 111 is easy to fall off, resulting in damage to the pole sheet coil 111.

[0114] In some embodiments, the first end surface 112 may also be arranged to be inclined relative to the vertical direction. For example, the first end surface 112 is arranged to be inclined downward, or the first end surface 112 is arranged to be inclined upward.

[0115] In the above solution, the first end face 112 is arranged in the vertical direction, and the pole piece coil 111 occupies a smaller space, reducing the risk of interference between the pole piece coil 111 and other components (such as a glue coating device, a container for containing insulating paint, etc.).

[0116] Please refer to Figure 3 and Figure 7 According to some embodiments of the present application, the coating roller 31 is a tapered roller, and the angle between the generatrix of the coating roller 31 and the central axis P1 of the coating roller 31 is α, satisfying 30°≤α≤60°.

[0117] The coating roller 31 is a tapered roller, and along the extension direction of the central axis P1 of the coating roller 31, the coating roller 31 has a large diameter end and a small diameter end. When the coating roller 31 cooperates with the first end face 112, the small diameter end of the coating roller 31 can correspond to the inner ring of the first end face 112, and the large diameter end of the coating roller 31 can correspond to the outer ring of the first end face 112, so that when the coating roller 31 rotates, the insulating coating attached to the roller surface of the coating roller 31 can cover the inner ring and the outer ring of the first end face 112.

[0118] When the insulating coating is transferred to the first end face 112 by the coating roller 31, since the liquid level of the insulating coating is parallel to the horizontal plane, in order to make the thickness of the insulating coating adhered to the roller surface of the coating roller 31 consistent, the roller surface of the coating roller 31 needs to be parallel to the liquid level of the insulating coating, and the roller surface of the coating roller 31 that cooperates with the first end face 112 needs to be parallel to the first end face 112. Therefore, the angle between the busbar of the coating roller 31 and the center axis P1 of the coating roller 31 can determine the setting direction of the first end face 112.

[0119] Optionally, α may be, but is not limited to, 30°, 35°, 40°, 45°, 50°, 55°, 60°, etc.

[0120] If the taper of the coating roller 31 is small (such as less than 60°) or the taper of the coating roller 31 is large (such as greater than 120°), the pole piece coil 111 occupies a larger space in the horizontal direction, making it easy for the pole piece coil 111 to interfere with other components (such as a glue coating device, a container for insulating coating, etc.).

[0121] The angle α between the busbar of the coating roller 31 and the central axis P1 of the coating roller 31 satisfies the above relationship (30°≤α≤60°), which is convenient for the reasonable setting of the pole piece coil 111. The pole piece coil 111 is not easy to interfere with other components (such as a gluing device, a container for insulating coating, etc.), so as to facilitate the transfer of the insulating coating to the first end face 112.

[0122] According to some embodiments of the present application, α=45°.

[0123] When α=45°, the roller surface of the coating roller 31 located on one side of the central axis P1 of the coating roller 31 can be arranged in a horizontal direction, and the roller surface of the coating roller 31 located on the other side of the central axis P1 of the coating roller 31 can be arranged in a vertical direction. At this time, the first end surface 112 can be arranged in a vertical direction, so that the insulating paint in the first container 500 can be transferred to the first end surface 112 through the coating roller 31. The coating roller 31 can have a good contact effect with the first end surface 112, so that the insulating paint is evenly coated on the first end surface 112.

[0124] When α=45°, the pole piece coil 111 occupies a smaller space in the horizontal direction, reducing the risk of interference between the pole piece coil 111 and other components (such as a glue coating device, a container for containing insulating paint, etc.).

[0125] According to some embodiments of the present application, the pole piece coil 111 is rotated, and the insulating coating is transferred to the first end face 112 by rotating the coating roller 31, including: before transferring the insulating coating to the first end face 112 by rotating the coating roller 31, scraping off excess insulating coating by a scraper 600.

[0126] In the above scheme, by scraping off excess insulating coating with the scraper 600, the thickness of the insulating coating attached to the roller surface of the coating roller 31 can be controlled, thereby controlling the thickness of the insulating coating attached to the first end surface 112, and further achieving control of the thickness of the insulating layer.

[0127] According to some embodiments of the present application, before the pole piece coil 111 is rotated and the insulating coating is transferred to the first end surface 112 by rotating the coating roller 31, the pole piece insulation processing method also includes: adjusting the gap between the scraper 600 and the coating roller 31 to control the thickness of the insulating coating attached to the coating roller 31.

[0128] In the above solution, by adjusting the gap between the scraper 600 and the coating roller 31 , the thickness of the insulating coating attached to the coating roller 31 can be controlled according to different coating requirements, so as to control the thickness of the insulating layer attached to the first end surface 112 .

[0129] According to some embodiments of the present application, the solid content of the insulating coating is 10% to 30%.

[0130] The solid content of insulating coating refers to the proportion of solid mass in the insulating coating to the total mass. The solid content of insulating coating can be tested using a solid content tester.

[0131] The insulating coating may be a diluted slurry with a solid content of 10% to 30%.

[0132] Optionally, the solid content of the insulating coating may be, but is not limited to, 10%, 12%, 15%, 17%, 20%, 22%, 25%, 27%, 30%, etc.

[0133] If the solid content of the insulating coating is small (e.g., less than 10%), the thickness of the insulating layer after drying is small, and the insulating effect is poor. If the solid content of the insulating coating is large (e.g., greater than 30%), the insulating layer is easily accumulated on the first end surface 112, which easily causes the insulating layer to adhere to the two adjacent circles of pole pieces 11.

[0134] The solid content of the insulating coating satisfies the above relationship (10% to 30%). On the one hand, it is easy to adhere to the first end face 112, and the thickness of the insulating layer after drying is thicker, which has a better insulating effect; on the other hand, the insulating layer is not easy to accumulate on the first end face 112, reducing the risk of the insulating layer adhering to the two adjacent circles of pole pieces 11.

[0135] According to some embodiments of the present application, the solid content of the insulating coating is 12% to 18%.

[0136] Optionally, the solid content of the insulating coating may be, but is not limited to, 12%, 13%, 14%, 15%, 16%, 17%, 18%, etc.

[0137] Compared with the insulating coating having a solid content of less than 12%, when the solid content of the insulating coating is greater than or equal to 12%, the thickness of the insulating layer attached to the first surface is thicker and has a better insulating effect; compared with the insulating coating having a solid content of greater than 18%, when the solid content of the insulating coating is less than or equal to 18%, the insulating coating is not easy to accumulate on the first end surface 112, thereby reducing the risk of the insulating layer adhering to the two adjacent circles of pole pieces 11.

[0138] According to some embodiments of the present application, the thickness of the insulating layer is 10 μm to 200 μm.

[0139] The thickness of the insulating layer can be the thickness of the insulating coating solidified after being attached to the first end face 112. The pole piece coil 111 can be unfolded, and the distance between the first end face 112 and the surface of the insulating layer away from the first end face 112 can be measured in a direction perpendicular to the first end face 112 to obtain the thickness of the insulating layer.

[0140] Optionally, the thickness of the insulating layer may be, but is not limited to, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 100 μm, 150 μm, 200 μm, etc.

[0141] In the above solution, the thickness of the insulating layer satisfies the above relationship (10 μm to 200 μm), which has a good insulating effect on one hand, and is not easy to accumulate on the first end surface 112 on the other hand.

[0142] If the thickness of the insulating layer is thin (e.g., less than 10 μm), the insulating effect of the insulating layer is poor, and burrs are easy to pierce the insulating layer. If the thickness of the insulating layer is thick (e.g., greater than 200 μm), the insulating coating is easy to flow into the gap between the two adjacent layers of sub-pole pieces 11 after being attached to the first end face 112, thereby adhering the two adjacent circles of pole pieces 11. After the insulating layer solidifies, when the sub-pole piece 11 is unfolded, it is easy to cause the insulating layer to separate from the sub-pole piece 11.

[0143] According to some embodiments of the present application, the thickness of the insulating layer is 20 μm to 60 μm.

[0144] Optionally, the thickness of the insulating layer may be, but is not limited to, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, etc.

[0145] Compared with the thickness of the insulating layer being less than 20 μm, when the thickness of the insulating layer is greater than or equal to 20 μm, the thickness of the insulating layer is thicker and has a better insulation effect. Compared with the thickness of the insulating layer being greater than 60 μm, when the thickness of the insulating layer is less than or equal to 60 μm, the insulating layer is not easily deposited on the first end surface 112, reducing the risk of the insulating layer adhering to the two adjacent circles of pole pieces 11.

[0146] In the above-mentioned embodiment, the thickness of the insulating layer can be determined by the thickness of the insulating coating attached to the coating roller 31 . For example, the thickness of the insulating coating on the coating roller 31 can be controlled by adjusting the gap between the scraper and the coating roller 31 .

[0147] Please refer to Figure 2 and Figure 3 , and further refer to Figure 6 and Figure 7 , Figure 6 A schematic block diagram of the structure of a pole piece manufacturing device provided in some embodiments of the present application, Figure 7A partial structural schematic diagram of a pole piece manufacturing device provided for some embodiments of the present application. According to some embodiments of the present application, the embodiments of the present application also provide a pole piece manufacturing device, which can manufacture a pole piece 10 using the pole piece insulation treatment method provided in any of the above embodiments. The pole piece manufacturing device includes a slitting device 100, a winding device 200 and a coating device 300. The slitting device 100 is used to slit the pole piece 10 into a plurality of sub-pole pieces 11; the winding device 200 is used to wind up the sub-pole piece 11 to form a pole piece coil 111, and the pole piece coil 111 includes a first end face 112 formed by the slitting edge of the sub-pole piece 11; the coating device 300 is used to transfer the insulating coating to the first end face 112 to form an insulating layer that at least covers the current collector of the sub-pole piece 11 and the burrs generated after the current collector is cut.

[0148] The slitting device 100 is a device for slitting the pole piece 10 into a plurality of sub-pole pieces 11. The slitting device 100 may include an upper cutter and a lower cutter, and the pole piece 10 is slitting by the engagement of the upper cutter and the lower cutter.

[0149] The winding device 200 is a device for winding the sub-pole sheet 11. The winding device 200 may include a winding roller 21 and a winding drive, and the winding drive drives the winding roller 21 to rotate so as to wind the sub-pole sheet 11 on the winding roller 21. After the sub-pole sheet 11 is wound on the winding roller 21, a pole sheet coil 111 is formed, and the winding roller 21 moves with the pole sheet coil 111 between subsequent processes.

[0150] The coating device 300 is a device for transferring the insulating coating to the first end surface 112. The coating device 300 may include a coating roller 31, and the insulating coating is transferred to the first end surface 112 by the coating roller 31. For example, an operator may hold the coating roller 31 and manually transfer the insulating coating to the first end surface 112; or, the coating roller 31 may transfer the insulating coating to the first end surface 112 under the drive of a driving member (such as a motor).

[0151] The pole piece 10 is cut into a plurality of sub-pole pieces 11 by the cutting device 100 , so that the manufacturing efficiency of the pole piece 10 can be improved; the sub-pole piece 11 is rolled up by the collecting device and the insulating coating is transferred to the first end face 112 by the coating device 300 , so that all the cut edges of the sub-pole piece 11 can be coated with the insulating coating to form an insulating layer on the first end face 112 .

[0152] The pole piece 10 prepared by the pole piece manufacturing equipment has an insulating layer formed on the first end face 112 of the cutting edge, and the insulating layer can cover the current collector and the burrs generated after the current collector is cut. After forming a battery cell, the insulating layer can reduce the risk of burrs piercing the isolation membrane and causing an internal short circuit in the battery cell, so that the battery cell has higher reliability.

[0153] Please refer to Figure 7 According to some embodiments of the present application, the pole piece manufacturing equipment further includes a driving device 400, and the driving device 400 is used to drive the pole piece coil 111 to rotate.

[0154] The driving device 400 is a device for driving the pole piece coil 111 to rotate. The driving device 400 may include a driving motor, and the winding roller 21 of the pole piece coil 111 is drivingly connected to the output end of the driving motor, and the pole piece coil 111 is driven to rotate by the driving motor.

[0155] In the above solution, the pole piece coil 111 is driven to rotate by the driving device 400 so that the insulating coating covers the inner and outer circles of the first end surface 112 , thereby improving the thickness uniformity of the insulating coating attached to the first end surface 112 .

[0156] Please refer to Figure 3 and Figure 7 According to some embodiments of the present application, the pole piece manufacturing equipment also includes a first container 500, the first container 500 is used to contain the insulating coating, the coating device 300 includes a coating roller 31 and a coating roller driving member 32, the coating roller 31 is transmission-connected to the coating roller driving member 32, and the coating roller driving member 32 is used to drive the coating roller 31 to rotate so as to transfer the insulating coating in the first container 500 to the first end surface 112.

[0157] The first container 500 is a container for storing insulating coating, and the first container 500 can be disposed adjacent to the electrode coil 111, so that the coating roller 31 can transfer the insulating coating to the first end surface 112. The first container 500 can be a plastic barrel with a certain capacity.

[0158] In some embodiments, a residual amount detection device is provided in the first container 500, for detecting the residual amount of the insulating coating in the first container 500. For example, the residual amount detection device may be a liquid level meter, for detecting the liquid level of the insulating coating in the first container 500.

[0159] The coating roller 31 can rotate relative to the first container 500. The coating roller 31 rotates under the drive of the coating roller driving member 32. The coating roller 31 first contacts the insulating coating in the first container 500, and the insulating coating adheres to the roller surface of the coating roller 31. Then, the coating roller 31 transfers the insulating coating to the first end face 112.

[0160] In some embodiments, the coating roller 31 and the coating roller driving member 32 are disposed at the opening above the first container 500 , and the coating roller 31 contacts the insulating coating in the first container 500 so that the coating roller 31 transfers the insulating coating to the first end surface 112 .

[0161] In some embodiments, the coating roller 31 and the coating roller driving member 32 are arranged on a robot, and the coating roller 31 is transferred to the opening of the first container 500 by the robot, so that the coating roller 31 can contact the insulating coating in the first container 500 when rotating, thereby transferring the insulating coating to the first end surface 112.

[0162] In the above solution, the coating roller 31 transfers the insulating coating in the first container 500 to the first end surface 112, so that the coating efficiency is high.

[0163] In some embodiments, the roller surface of the coating roller 31 may include a brush-like flexible structure capable of absorbing the insulating coating so that the insulating coating is attached to the first end surface 112 when the coating roller 31 contacts the first end surface 112 .

[0164] Please refer to Figure 3 and Figure 7 According to some embodiments of the present application, the coating roller 31 is a tapered roller, and the angle between the generatrix of the coating roller 31 and the central axis P1 of the coating roller 31 is α, satisfying 30°≤α≤60°.

[0165] The coating roller 31 is a tapered roller, and along the extension direction of the central axis P1 of the coating roller 31, the coating roller 31 has a large diameter end and a small diameter end. When the coating roller 31 cooperates with the first end face 112, the small diameter end of the coating roller 31 can correspond to the inner ring of the first end face 112, and the large diameter end of the coating roller 31 can correspond to the outer ring of the first end face 112, so that when the coating roller 31 rotates, the insulating coating can cover the inner ring and the outer ring of the first end face 112.

[0166] Since the liquid level of the insulating coating in the first container 500 is parallel to the horizontal plane, in order to make the thickness of the insulating coating adhered to the roller surface of the coating roller 31 consistent, the roller surface of the coating roller 31 located in the first container 500 needs to be parallel to the liquid level of the insulating coating, and the roller surface of the coating roller 31 that cooperates with the first end face 112 needs to be parallel to the first end face 112. Then, the angle between the busbar of the coating roller 31 and the center axis P1 of the coating roller 31 can determine the setting direction of the first end face 112.

[0167] Optionally, α may be, but is not limited to, 30°, 35°, 40°, 45°, 50°, 55°, 60°, etc.

[0168] The angle α between the generatrix of the coating roller 31 and the central axis P1 of the coating roller 31 satisfies the above relationship, which is convenient for reasonably setting the pole piece coil 111, and the pole piece coil 111 is not easy to interfere with other components (such as a coating device, a container for containing insulating paint, etc.), so as to facilitate the transfer of the insulating paint in the first container 500 to the first end surface 112. If the taper of the coating roller 31 is small (such as less than 60°) or the taper of the coating roller 31 is large (such as greater than 120°), the pole piece coil 111 occupies a large space in the horizontal direction, making it easy for the pole piece coil 111 to interfere with other components (such as a coating device, a container for containing insulating paint, etc.).

[0169] According to some embodiments of the present application, α=45°.

[0170] When α=45°, the roller surface of the coating roller 31 located on one side of the central axis P1 of the coating roller 31 can be arranged in a horizontal direction, and the roller surface of the coating roller 31 located on the other side of the central axis P1 of the coating roller 31 can be arranged in a vertical direction. At this time, the first end surface 112 can be arranged in a vertical direction, so that the insulating paint in the first container 500 can be transferred to the first end surface 112 through the coating roller 31. The coating roller 31 can have a good contact effect with the first end surface 112, so that the insulating paint is evenly coated on the first end surface 112.

[0171] In the above scheme, when α=45°, the first end face 112 can be set in the vertical direction, and the coating roller 31 can apply the insulating coating in a horizontal state to the vertically set first end face 112. The pole piece coil 111 occupies a smaller space in the horizontal direction, reducing the risk of interference between the pole piece coil 111 and other components (such as a gluing device, a container for containing insulating coating, etc.).

[0172] Please refer to Figure 3 and Figure 7 According to some embodiments of the present application, the pole piece manufacturing equipment also includes a scraper 600, which is arranged in the first container 500, and the scraper 600 is spaced apart from the coating roller 31. The gap between the scraper 600 and the coating roller 31 is adjustable to control the thickness of the insulating coating attached to the coating roller 31.

[0173] The scraper 600 may be disposed at the opening of the first container 500 , and the gap between the scraper 600 and the coating roller 31 determines the thickness of the insulating coating attached to the coating roller 31 .

[0174] When the coating roller 31 is soaked in the insulating coating, when the roller surface with the insulating coating rotates to the scraper 600, the scraper 600 scrapes off the excess insulating coating on the roller surface, leaving an appropriate amount of insulating coating on the roller surface. As the coating roller 31 rotates, when the roller surface contacts the first end face 112, the insulating coating contacts the first end face 112 to complete the coating.

[0175] When the gap between the scraper 600 and the coating roller 31 is small, the thickness of the insulating coating attached to the coating roller 31 is thin; when the gap between the scraper 600 and the coating roller 31 is large, the thickness of the insulating coating attached to the coating roller 31 is thick.

[0176] The connection position of the scraper 600 and the first container 500 is adjustable, so as to change the gap between the scraper 600 and the coating roller 31. For example, a slide groove is provided on the first container 500, a through hole is provided on the scraper 600, and the scraper 600 and the first container 500 are connected by a locking bolt passing through the through hole and the slide groove. When it is necessary to adjust the gap between the scraper 600 and the coating roller 31, the position of the locking bolt in the slide groove can be adjusted to change the connection position of the scraper 600 on the first container 500, so as to achieve the gap adjustment between the scraper 600 and the coating roller 31.

[0177] In the above scheme, the scraper 600 is spaced apart from the coating roller 31, and the gap between the scraper 600 and the coating roller 31 is adjustable to control the thickness of the insulating coating attached to the coating roller 31, thereby controlling the thickness of the insulating layer on the first end face 112 to meet the coating requirements.

[0178] According to some embodiments of the present application, the scraper 600 is arranged parallel to the roller surface of the coating roller 31 .

[0179] The scraper 600 is arranged parallel to the roller surface of the coating roller 31 so that the gap between the scraper 600 and the roller surface of the coating roller 31 at any position along the extension direction of the scraper 600 is the same, that is, the thickness of the insulating coating attached to any position of the coating roller 31 is the same, so that the thickness of the insulating coating on the roller surface of the coating roller 31 is highly consistent.

[0180] Please refer to Figure 8 , Figure 8 A schematic diagram of the structure of a stirring device provided in some embodiments of the present application. According to some embodiments of the present application, the pole piece manufacturing equipment further includes a stirring device 700 , and the stirring device 700 is used to stir the insulating coating in the first container 500 .

[0181] The stirring device 700 may include a stirring paddle 71 and a stirring driving member 72. The stirring paddle 71 may be disposed in the first container 500. The stirring paddle 71 is in transmission connection with the stirring driving member 72. The stirring driving member 72 is used to drive the stirring paddle 71 to rotate so as to stir the insulating coating in the first container 500. For example, the stirring driving member 72 may include a motor, and the stirring paddle 71 may be driven to rotate by the motor.

[0182] In the above solution, the provision of the stirring device 700 can make the components of the insulating coating material mixed evenly, so that the thickness of the insulating layer formed on the first end surface 112 is uniform.

[0183] Please refer to Fig. 9 , Fig. 9 A schematic diagram of a circulation device provided for some embodiments of the present application. According to some embodiments of the present application, the pole piece manufacturing equipment further includes a circulation device 800, the circulation device 800 includes a second container 81, a pipeline 82 and a circulation pump 83, the second container 81 is connected to the first container 500 through the pipeline 82, and the circulation pump 83 is used to drive the insulating coating to circulate between the first container 500 and the second container 81.

[0184] The second container 81, the pipeline 82, the first container 500 and the circulation pump 83 form a circulation loop. The circulation pump 83 drives the insulating paint to flow in the circulation loop, so that the insulating paint circulates between the second container 81 and the first container 500, so that the insulating paint in the first container 500 is evenly mixed, reducing the risk of precipitation of components in the insulating paint.

[0185] In some embodiments, the circulation pump 83 may include an air-operated diaphragm pump or a screw pump.

[0186] In the above solution, the insulating coating is driven to circulate between the first container 500 and the second container 81 by the circulation pump 83, so that the components of the insulating coating are evenly mixed, and the thickness of the insulating layer formed on the first end surface 112 is uniform.

[0187] Please refer to Figure 2 , Figure 3 , Figure 7 and Fig. 9According to some embodiments of the present application, the embodiments of the present application provide a pole piece manufacturing device, which includes a slitting device 100, a winding device 200, a driving device 400, a coating device 300, a first container 500, a scraper 600 and a circulation device 800. The slitting device 100 includes an upper cutter and a lower cutter, and the upper cutter and the lower cutter cooperate with each other to cut the pole piece 10, and cut the pole piece 10 into a plurality of sub-pole pieces 11. The winding device 200 includes a winding roller 21 and a winding drive member, which is transmission-connected to the winding roller 21, and the winding drive member is used to drive the winding roller 21 to rotate, so as to wind the sub-pole piece 11 on the winding roller 21. The driving device 400 includes a driving motor, and the driving motor is used to drive the pole piece coil 111 to rotate. The first container 500 is used to contain insulating coating. The coating device 300 includes a coating roller 31 and a coating roller driving member 32, wherein the coating roller 31 is in transmission connection with the coating roller driving member 32, and the coating roller driving member 32 is used to drive the coating roller 31 to rotate so as to transfer the insulating coating in the first container 500 to the first end surface 112. The coating roller 31 is a tapered roller, and the angle between the generatrix of the coating roller 31 and the central axis P1 of the coating roller 31 is 45°, and the first end surface 112 can be arranged in the vertical direction. The scraper 600 is arranged at the opening of the first container 500, and the scraper 600 is arranged at a distance from the coating roller 31, and the gap between the scraper 600 and the coating roller 31 is adjustable to control the thickness of the insulating coating attached to the coating roller 31. The circulation device 800 includes a second container 81, a pipeline 82 and a circulation pump 83. The second container 81 is connected to the first container 500 through the pipeline 82. The second container 81, the first container 500, the pipeline 82 and the circulation pump 83 constitute a circulation loop. The circulation pump 83 is used to drive the insulating coating to circulate between the first container 500 and the second container 81.

[0188] According to some embodiments of the present application, an embodiment of the present application provides a pole piece insulation processing method, and the pole piece insulation processing method is performed using a pole piece manufacturing device provided in any of the above embodiments. The pole piece insulation processing method includes:

[0189] like Figure 2 As shown, the pole piece 10 is cut into a plurality of sub-pole pieces 11;

[0190] Rolling up the sub-pole sheet 11 to form a pole sheet coil 111, wherein the pole sheet coil 111 includes a first end surface 112 formed by the cut edge of the sub-pole sheet 11;

[0191] like Figure 7 As shown, the first end surface 112 is arranged along the vertical direction;

[0192] like Figure 3 As shown, the pole sheet coil 111 is rotated, and the insulating coating is transferred to the first end surface 112 by rotating the coating roller 31 to form an insulating layer that at least covers the current collector of the sub-pole sheet 11 and the burrs generated after the current collector is cut.

[0193] Among them, Figure 3 and Figure 7 As shown, the coating roller 31 is a tapered roller, and the angle α between the generatrix of the coating roller 31 and the central axis P1 of the coating roller 31 is 45°; the coating roller 31 rotates in the same direction as the pole piece coil 111, and the rotation speed of the coating roller 31 is the same as the rotation speed of the pole piece coil 111.

[0194] Before the insulating coating is transferred to the first end surface 112 by the rotation of the coating roller 31 , the thickness of the insulating coating attached to the coating roller 31 can be controlled by adjusting the gap between the scraper 600 and the coating roller 31 .

[0195] According to the technical solution provided in the present application, in the prepared pole piece 10, the first end face 112 of the cutting edge is attached with an insulating layer, and the insulating layer covers the current collector and part of the active material layer, so that the insulating layer blocks the burrs generated after the current collector is cut. The insulating layer has a good insulating effect. When the pole piece 10 constitutes a battery cell, it can reduce the risk of burrs piercing the isolation membrane and causing an internal short circuit in the battery cell, so that the battery cell can have higher reliability.

[0196] Although the present application has been described with reference to preferred embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.

Claims

1. A method for insulating a pole piece, characterized in that: include: Cutting the pole piece into a plurality of sub-pole pieces; Rolling up the sub-pole sheet to form a pole sheet coil, wherein the pole sheet coil includes a first end surface formed by a cut edge of the sub-pole sheet; The insulating coating is transferred to the first end surface to form an insulating layer that at least covers the current collector of the sub-electrode sheet and burrs generated after the current collector is cut.

2. The electrode insulation processing method according to claim 1, characterized in that: The step of transferring the insulating coating to the first end surface comprises: The pole piece coil is rotated, and the insulating coating is transferred to the first end surface by rotating the coating roller.

3. The pole piece insulation processing method according to claim 2, characterized in that: The coating roller rotates in the same direction as the pole piece coil.

4. The pole piece insulation processing method according to claim 3, characterized in that: The rotation speed of the coating roller is the same as the rotation speed of the pole piece coil.

5. The pole piece insulation processing method according to claim 2, characterized in that: Before rotating the pole piece coil, the pole piece insulation treatment method further includes: The first end surface is arranged along the vertical direction.

6. The pole piece insulation processing method according to claim 2, characterized in that: The coating roller is a tapered roller, and the angle between the generatrix of the coating roller and the central axis of the coating roller is α, which satisfies 30°≤α≤60°.

7. The pole piece insulation processing method according to claim 6, characterized in that: α=45°。 8. The pole piece insulation processing method according to claim 2, characterized in that: The step of rotating the pole piece coil and transferring the insulating coating to the first end surface by rotating the coating roller includes: Before the insulating coating is transferred to the first end surface by rotating the coating roller, the excess insulating coating is scraped off by a scraper.

9. The pole piece insulation processing method according to claim 8, characterized in that: Before rotating the pole piece coil and transferring the insulating coating to the first end surface by rotating the coating roller, the pole piece insulation treatment method further includes: The gap between the scraper and the coating roller is adjusted to control the thickness of the insulating coating attached to the coating roller.

10. The pole piece insulation processing method according to claim 1, characterized in that: The solid content of the insulating coating is 10% to 30%.

11. The pole piece insulation processing method according to claim 10, characterized in that: The solid content of the insulating coating is 12% to 18%.

12. A pole piece manufacturing device, characterized in that: include: A slitting device, used for slitting a pole piece into a plurality of sub-pole pieces; A winding device, used for winding the sub-pole sheet to form a pole sheet coil, wherein the pole sheet coil includes a first end surface formed by a cut edge of the sub-pole sheet; The coating device is used to transfer the insulating coating to the first end surface to form an insulating layer that at least covers the current collector of the sub-pole sheet and the burrs generated after the current collector is cut.

13. The pole piece manufacturing equipment according to claim 12, characterized in that: The pole piece manufacturing equipment also includes a driving device for driving the pole piece coil to rotate.

14. The pole piece manufacturing equipment according to claim 12, characterized in that: The pole piece manufacturing equipment also includes a first container, which is used to contain insulating paint. The coating device includes a coating roller and a coating roller driving member. The coating roller is transmission-connected to the coating roller driving member, and the coating roller driving member is used to drive the coating roller to rotate so as to transfer the insulating paint in the first container to the first end face.

15. The pole piece manufacturing equipment according to claim 14, characterized in that: The coating roller is a tapered roller, and the angle between the generatrix of the coating roller and the central axis of the coating roller is α, which satisfies 30°≤α≤60°.

16. The pole piece manufacturing equipment according to claim 15, characterized in that: α=45°。 17. The pole piece manufacturing equipment according to claim 14, characterized in that: The pole piece manufacturing equipment also includes: A scraper is arranged in the first container, the scraper and the coating roller are arranged at a distance, and the gap between the scraper and the coating roller is adjustable to control the thickness of the insulating coating attached to the coating roller.

18. The pole piece manufacturing equipment according to claim 17, characterized in that: The scraper is arranged parallel to the roller surface of the coating roller.

19. The pole piece manufacturing equipment according to claim 14, characterized in that: The pole piece manufacturing equipment also includes: A stirring device is used to stir the insulating coating in the first container.

20. The pole piece manufacturing equipment according to claim 14, characterized in that: The pole piece manufacturing equipment also includes: The circulation device comprises a second container, a pipeline and a circulation pump, wherein the second container is connected to the first container through the pipeline, and the circulation pump is used to drive the insulating coating to circulate between the first container and the second container.

Citation Information

Patent Citations

  • Lithium ion battery anode baking process

    CN111687019A

  • Coating roller

    CN115515725A

  • Battery cell pole piece manufacturing method, battery cell manufacturing method, battery cell and battery

    CN115911277A

  • Modified waterproof roll oil presoaking system

    CN209318038U

  • Method and device for coating

    JP1994020272A