Negative plate as well as preparation method and application thereof

By optimizing the porosity and material composition of the negative electrode sheet and meeting the specific relationship, the safety hazards and insufficient energy density of the negative electrode sheet of the secondary battery under high charging current are solved, and the high energy density and excellent rate performance are improved.

CN119069641APending Publication Date: 2024-12-03SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411201370.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The negative electrode sheet of the existing secondary batteries is prone to precipitation of alkali metals under high charging current, forming dendrites and piercing the diaphragm, posing safety hazards, and insufficient energy density and charging capacity.

Method used

By optimizing the porosity, the crystal size and particle size of the negative electrode active material along (100) direction in the negative electrode sheet, the specific relationship 0.7≤(P/La)1/2/(0.1×DV50)≤4 is satisfied, and the combination of hardness is combined with Carbon, soft carbon, graphite and other materials, conductive agents and binders are added to build a negative electrode sheet with high energy density and excellent rate performance.

Benefits of technology

The high energy density and excellent rate performance of the negative electrode sheet are achieved, the electrochemical performance of the secondary battery is improved, safety hazards are reduced, and charging capacity is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069641A_ABST
    Figure CN119069641A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a negative plate as well as a preparation method and application thereof. The negative electrode plate provided by the invention comprises a negative electrode current collector and a negative electrode material layer located on at least one side surface of the negative electrode current collector, and the negative electrode material layer comprises a negative electrode active material; the porosity P of the negative plate, the size La of the crystal of the negative electrode active material along the (100) direction and the corresponding particle size Dv50 when the cumulative volume percentage of the negative electrode active material reaches 50% meet the relation that (P / La) 1 / 2 / (0.1 * Dv50) is greater than or equal to 0.7 and less than or equal to 4. The negative plate disclosed by the invention has excellent energy density and good rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of battery technology, and in particular to a negative electrode sheet and a preparation method and application thereof. Background Art

[0002] In recent years, electric vehicles have developed rapidly. Secondary batteries, as a high-energy-density, memory-free, clean, and recyclable energy storage device, have been widely used in electric vehicles. The charging capacity of secondary batteries is one of the key factors restricting the popularization of electric vehicles. Secondary batteries include negative electrodes and positive electrodes. Among them, the negative electrode is usually composed of a negative electrode current collector and a negative electrode material layer. The electrochemical properties of the negative electrode affect the electrochemical properties of the secondary battery. At present, the higher charging current of secondary batteries will cause alkali metals to precipitate on the surface of the negative electrode, forming dendrites and piercing the diaphragm, posing a safety hazard.

[0003] How to improve the negative electrode sheet so that the secondary battery has high energy density and excellent charging capacity is crucial.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] An object of the present invention is to provide a negative electrode sheet having excellent energy density and rate performance.

[0006] Another object of the present invention is to provide a method for preparing the negative electrode sheet, which is simple and easy to implement and can obtain a negative electrode sheet with high energy density and rate performance.

[0007] An object of the present invention is to provide a secondary battery.

[0008] An object of the present invention is to provide an electrical device.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A negative electrode sheet, comprising a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, wherein the negative electrode material layer contains a negative electrode active material; the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction, and the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4.

[0011] In some embodiments, the porosity P of the negative electrode sheet, the size La of the crystals of the negative electrode active material along the (100) direction, and the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2.

[0012] In some embodiments, the porosity P of the negative electrode sheet is 30% to 70%, the crystal size La of the negative electrode active material along the (100) direction is 1.5 to 2.2 nm; and the particle size Dv50 of the negative electrode active material is 2 to 7 μm.

[0013] In some embodiments, the porosity P of the negative electrode sheet is 40% to 60%, the crystal size La of the negative electrode active material along the (100) direction is 1.6 to 2 nm; and the particle size Dv50 of the negative electrode active material is 3 to 5.5 μm.

[0014] In some embodiments, the negative electrode active material includes at least one of hard carbon, soft carbon, graphite, and a carbon-based composite material.

[0015] In some embodiments, the negative electrode sheet further includes a conductive agent and a binder. The mass content of the conductive agent in the negative electrode material layer is 1% to 3%, and the mass content of the binder in the negative electrode material layer is 1% to 3.5%.

[0016] In some embodiments, the mass content of the hard carbon in the negative electrode active material is greater than 50%.

[0017] The method for preparing the negative electrode sheet as described above comprises the following steps:

[0018] A negative electrode slurry containing a negative electrode active material is applied to at least one side of a negative electrode current collector, wherein the particle size of the negative electrode active material is Dv50, and a negative electrode sheet is obtained after drying; the porosity P of the negative electrode material layer on at least one side of the negative electrode sheet and the size La of the crystal of the negative electrode active material along the (100) direction are tested; and the porosity P, La and the particle size Dv50 satisfy 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4 negative electrode sheet.

[0019] In some embodiments, the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction, and the particle size Dv50 of the negative electrode active material satisfy 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2 negative electrode sheet.

[0020] In some embodiments, the negative electrode slurry further includes a binder, a conductive agent, and optionally a dispersant and a solvent.

[0021] A secondary battery comprises the negative electrode sheet.

[0022] An electrical device comprises the secondary battery.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] (1) In the negative electrode sheet of the present invention, the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction, and the particle size Dv50 of the negative electrode active material satisfy the relationship 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4, and by constructing the relationship between the three, the negative electrode sheet can obtain excellent energy density and excellent rate performance.

[0025] (2) The method for preparing the negative electrode sheet of the present invention is to screen the negative electrode sheet satisfying 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4, so that the negative electrode sheet has excellent energy density and good rate performance.

[0026] (3) The battery of the present invention has a high capacity density and excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 Schematic diagram showing the dimension La along the (100) direction. DETAILED DESCRIPTION

[0029] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0030] According to one aspect of the present invention, the present invention relates to a negative electrode sheet, comprising a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, wherein the negative electrode material layer contains a negative electrode active material; the porosity P (in %) of the negative electrode sheet, the size La (in nm) of the crystal of the negative electrode active material along the (100) direction, and the particle size Dv50 (in μm) corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4.

[0031] When the secondary battery is charged, the active ions use the electrolyte as a medium to reach the negative electrode surface (liquid phase conduction), exchange electrons on the surface of the negative electrode active material, and finally enter the interior of the negative electrode active particles (solid phase conduction). According to the charging reaction mechanism, it can be seen that improving the charging capacity of the battery is mainly to increase the rate of liquid phase conduction, electron exchange and solid phase conduction. Improving the wettability of the electrolyte is an effective way to improve the efficiency of liquid phase conduction. The wettability of the electrolyte is closely related to the porosity of the electrode. The ion diffusion rate of the defective active site is much higher than that of the intercalation. The smaller La is, the more terminal active sites (a type of defect site) there are, and the higher the ion diffusion rate. However, the higher the disorder of the carbon layer of the material, the carbon layer is not easy to slip during the extrusion process, and the compaction density is relatively low, resulting in a decrease in energy density; the larger La is, the capacity of the platform area is improved, and the order of the material is increased, which can effectively improve the charge conduction rate and battery energy density. The particle size of the material also has a crucial influence on the electrical performance. The appropriate particle size can coordinate the energy density and rate performance. In the negative electrode sheet of the present invention, the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction and the particle size Dv50 of the negative electrode active material satisfy the relationship 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4, and by constructing the relationship between the three, the negative electrode sheet can obtain excellent energy density and excellent rate performance.

[0032] In some embodiments, the porosity P of the negative electrode sheet, the size La of the crystals of the negative electrode active material along the (100) direction, and the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2. When p, La and Dv50 meet the above ranges, the negative electrode sheet has more excellent electrochemical properties, which can further improve the energy density and rate performance of the battery.

[0033] In some embodiments, the higher the porosity of the negative electrode sheet, the better the wettability of the electrolyte, but if the porosity is too large, the energy density of the battery will be lost. In some embodiments, the porosity P of the negative electrode sheet is 30% to 70%, including but not limited to 30%, 35%, 40%, 50%, 60%, 65%, 70%, etc., or any range between the two.

[0034] In some embodiments, the size La of the crystal of the negative electrode active material along the (100) direction is 1.5 nm to 2.2 nm, including but not limited to 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm, 2 nm, 2.1 nm or 2.2 nm, or any range between the two. The schematic diagram of the size La along the (100) direction is as follows Figure 1 shown.

[0035] In some embodiments, the particle size of the negative electrode material also has a crucial influence on the electrical performance. The smaller the particle size, the shorter the path of active ions passing through the particles, which is beneficial to improving the rate performance of the battery; the larger the particle size, the higher the capacity of the material, which can effectively improve the energy density of the battery. In some embodiments, the particle size Dv50 of the negative electrode active material is 2 to 7 μm, including but not limited to 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, 6 μm or 7 μm, or any range between the two.

[0036] In some embodiments, the porosity P of the negative electrode sheet is 40% to 60%, the crystal size La of the negative electrode active material along the (100) direction is 1.6 nm to 2 nm; and the particle size Dv50 of the negative electrode active material is 3 to 5.5 μm.

[0037] In some embodiments, the negative electrode active material includes at least one of hard carbon, soft carbon, graphite and carbon-based composite materials. The negative electrode active material of the present invention can be any one of the above, or a combination of several, such as a combination of hard carbon and soft carbon, a combination of graphite and carbon-based composite materials, a combination of hard carbon, soft carbon and graphite, etc.

[0038] In some embodiments, the mass content of the hard carbon in the negative electrode active material is greater than 50%, including but not limited to 51%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, etc.

[0039] In some embodiments, the negative electrode sheet further includes a conductive agent and a binder. The mass content of the conductive agent in the negative electrode material layer is 1% to 3%, such as 1%, 1.5%, 2%, 2.5% or 3%. The mass content of the binder in the negative electrode material layer is 1% to 3.5%, such as 1%, 1.5%, 2%, 2.5% or 3%.

[0040] In some embodiments, the binder includes at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylonitrile, polyacrylic acid, polytetrafluoroethylene, polyimide, and polyethylene oxide.

[0041] In some embodiments, the conductive agent includes at least one of conductive carbon black, carbon fiber, carbon nanotube, acetylene black and Ketjen black.

[0042] According to another aspect of the present invention, the present invention also relates to a method for preparing the negative electrode sheet as described above, comprising the following steps:

[0043] A negative electrode slurry containing a negative electrode active material is applied to at least one side of a negative electrode current collector, wherein the particle size of the negative electrode active material is Dv50, and a negative electrode sheet is obtained after drying; the porosity P of the negative electrode material layer on at least one side of the negative electrode sheet and the size La of the crystal of the negative electrode active material along the (100) direction are tested; and the porosity P, La and the particle size Dv50 satisfy 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4 negative electrode sheet.

[0044] The preparation method of the negative electrode sheet of the present invention is to screen and satisfy 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4, so that the negative electrode sheet has excellent energy density and good rate performance.

[0045] In some embodiments, negative electrode active material, conductive carbon black and binder are prepared, and the mass ratio of negative electrode active material, conductive carbon black and binder is (93.5-97): (1-3): (1-3.5), and the binder is CMC glue (solid content 1%) and SBR, and the mass ratio of CMC and SBR is (2-4): (6-8). When the cumulative volume percentage of the negative electrode active material reaches 50%, the corresponding particle size Dv50 is 2-7 μm. First, 50% of the negative electrode active material is mixed with the conductive agent and CMC glue, and then the remaining 50% of hard carbon and deionized water are added to the above mixed slurry, and stirring is continued. Finally, SBR is added and stirred to obtain a negative electrode slurry, and the solid content is controlled at 42% to 48%. The slurry is coated on the surfaces of the opposite sides of the current collector, and after rolling and die cutting, it is vacuum dried at 95-105°C for 5-10 hours to obtain a negative electrode sheet.

[0046] In some embodiments, the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction, and the particle size Dv50 of the negative electrode active material satisfy 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2 negative electrode sheet.

[0047] In some embodiments, the negative electrode slurry further comprises a binder, a conductive agent, and optionally a solvent, wherein the solvent includes water, polycarbonate, nitrogen-methyl pyrrolidone, and the like.

[0048] In some embodiments, the coating may be single-sided or double-sided. If double-sided coating is used, it is sufficient that the coating layer on one side satisfies the above formula.

[0049] According to another aspect of the present invention, the present invention also relates to a secondary battery, comprising the negative electrode sheet.

[0050] The secondary battery of the present invention has excellent energy density and good rate performance.

[0051] The battery of the present invention comprises the above-mentioned negative electrode sheet, positive electrode sheet, separator and electrolyte.

[0052] When the battery is a sodium ion battery: the positive electrode plate includes a positive electrode collector and a positive electrode active material, the positive electrode collector is aluminum foil, and the positive electrode active material is a layered oxide such as a sodium-nickel-iron-manganese complex, a sodium-iron complex, a sodium-nickel-manganese complex oxide, a polyanion, a Prussian blue material, and other materials known in the industry, which can be used alone or in combination.

[0053] The diaphragm may be a polyvinylidene fluoride membrane, a polypropylene membrane, or a multi-layer composite diaphragm, and the specific type is not limited.

[0054] The electrolyte includes sodium salt and organic solvent, and the specific type can be selected according to the application field.

[0055] According to another aspect of the present invention, the present invention also relates to

[0056] An electric device includes the secondary battery. The electric device of the present invention includes electric vehicles, portable devices, etc.

[0057] In the present invention, the porosity, the size La and D50 of the crystals of the negative electrode active material along the (100) direction are tested as follows:

[0058] Porosity test method: Measure according to the gas replacement method in GB / T 24586, porosity P = (V 表观体积 -V 真实体积 ) / V 表观体积 ×100%.

[0059] The test method for the size La of the crystal of the negative electrode active material along the (100) direction is as follows: the measurement is carried out in accordance with the provisions of Appendix E of GB / T24533-2019, and the half-peak width β corresponding to the (100) peak position and the corresponding diffraction angle θ are obtained, and then according to the Scherrer formula: La = (kλ) / (βcosθ) (k = 0.89, λ = 0.15406nm).

[0060] Negative electrode active material D V50 Test method: According to the particle size distribution laser diffraction method GB / T19077-2016, the particle size distribution is measured to obtain D V50 .

[0061] The following is further explained in conjunction with specific embodiments.

[0062] Example 1

[0063] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 70% (i.e., P=0.7), the size La of the crystal of the negative electrode active material along the (100) direction is 1.5 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 2 μm, (P / La) 1 / 2 / (0.1×D V50 )=3.42.

[0064] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0065] Prepare the negative electrode active material hard carbon, conductive agent and binder, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 2μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 1.5nm.

[0066] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0067] Example 2

[0068] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 60% (i.e., P=0.6), the size La of the crystal of the negative electrode active material along the (100) direction is 1.6 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 3 μm, (P / La) 1 / 2 / (0.1×D V50 )=2.04.

[0069] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0070] Prepare the negative electrode active material hard carbon, conductive agent and binder, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 3μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 1.6nm.

[0071] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0072] Example 3

[0073] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 48% (i.e., P=0.48), the size La of the crystal of the negative electrode active material along the (100) direction is 1.7 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 3 μm, (P / La) 1 / 2 / (0.1×D V50 )=1.77.

[0074] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0075] The negative electrode active material hard carbon, conductive agent and binder are prepared, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, and the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 3μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 1.7nm.

[0076] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0077] Example 4

[0078] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 55% (i.e., P=0.55), the size La of the crystal of the negative electrode active material along the (100) direction is 1.7 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 4.5 μm, (P / La) 1 / 2 / (0.1×D V50 )=1.26.

[0079] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0080] Prepare the negative electrode active material hard carbon, conductive agent and binder, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 4.5μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 1.7nm.

[0081] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0082] Example 5

[0083] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 45% (i.e., P=0.45), the size La of the crystal of the negative electrode active material along the (100) direction is 2 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 5.5 μm, (P / La) 1 / 2 / (0.1×D V50 )=0.86.

[0084] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0085] Prepare the negative electrode active material hard carbon, conductive agent and binder, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 5.5μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 2nm.

[0086] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0087] Example 6

[0088] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 40% (i.e., P=0.4), the size La of the crystal of the negative electrode active material along the (100) direction is 2.1 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 6 μm, (P / La) 1 / 2 / (0.1×D V50 )=0.73.

[0089] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0090] The negative electrode active material hard carbon, conductive agent and binder are prepared, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, and the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 6μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 2.1nm.

[0091] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0092] Comparative Example 1

[0093] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 60% (i.e., P=0.6), the size La of the crystal of the negative electrode active material along the (100) direction is 1.5 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 1.5 μm, (P / La) 1 / 2 / (0.1×D V50 )=4.22.

[0094] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0095] Prepare the negative electrode active material hard carbon, conductive agent and binder, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 1.5μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 1.5nm.

[0096] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0097] Comparative Example 2

[0098] A negative electrode sheet comprises a negative electrode current collector and a negative electrode material layer located on the surface of the negative electrode current collector, wherein the negative electrode material layer comprises a negative electrode active material, a conductive agent and a binder; the negative electrode active material is hard carbon, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber and carboxymethyl cellulose, the porosity P of the negative electrode sheet is 50% (i.e., P=0.5), the size La of the crystal of the negative electrode active material along the (100) direction is 2.3 nm, the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 7 μm, (P / La) 1 / 2 / (0.1×D V50 )=0.67.

[0099] The method for preparing the negative electrode sheet in this embodiment comprises the following steps:

[0100] The negative electrode active material hard carbon, conductive agent and binder are prepared, the mass ratio of hard carbon, conductive agent and binder is 96.5:1.5:2, the binder is CMC glue (solid content 1%) and SBR, and the mass ratio of CMC and SBR is 3:7. The particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% is 7μm, and the size La of the crystal of the negative electrode active material along the (100) direction is 2.3nm.

[0101] First, mix 50% of the hard carbon with the conductive agent and CMC glue, then add the remaining 50% of the hard carbon and deionized water to the above mixed slurry, continue stirring, and finally add SBR and continue stirring to obtain the negative electrode slurry. The solid content is controlled at 46%. The slurry is coated on the surfaces on both sides of the current collector. After rolling and die-cutting, it is vacuum dried at 100°C for 8 hours to obtain the negative electrode sheet.

[0102] Experimental example

[0103] The negative electrode sheets of each embodiment and comparative example are prepared to obtain batteries, the positive electrode sheet includes a positive electrode current collector and a positive electrode material layer, the positive electrode material layer includes a positive electrode active material, a conductive agent SP and a binder PVDF, the mass ratio of the positive electrode active material, the conductive agent SP and the binder PVDF is 97:1.5:1.5, the positive electrode active material is a sodium nickel iron manganese complex, the positive electrode sheet is obtained by mixing the positive electrode active material, the conductive agent SP, the binder PVDF and an appropriate amount of NMP to obtain a positive electrode slurry, and the positive electrode slurry is further coated on the surface of the positive electrode current collector aluminum foil, and is obtained by drying, rolling and die cutting. The diaphragm is a polyvinylidene fluoride film. The electrolyte is a 1 mol / L lithium hexafluorophosphate solution, the solvent is ethylene carbonate and ethyl methyl carbonate, and the volume ratio of ethylene carbonate and ethyl methyl carbonate is 1:1.

[0104] The electrochemical performance tests were performed on the above batteries.

[0105] 1. Power performance test

[0106] Using a soft-pack three-electrode, constant current charging tests were performed at different rates. At 25°C, the battery was fully charged at xC and discharged at 1C. The charging rate was transitioned from xC to a large rate with a gradient of 0.25C. 5 to 7 charging rates were selected for constant current charging (the battery design voltage was the upper limit voltage). The negative electrode potential was detected at the same time, and charging was stopped when the negative electrode potential was less than 0V.

[0107] The test obtained the full battery and negative electrode potential change curves at different rates, and the full battery SOC was used as the horizontal axis, and the full battery voltage and the real-time monitored negative electrode potential were used as the vertical axis.

[0108] According to the actual data of the above charging tests at different rates, the negative electrode potential during the charging process at different rates is screened. The screening method is: on the negative electrode potential change curve, select a data point every 10% SOC interval, select the negative electrode potential of the data point as the Y value, and the charging rate corresponding to the data point as the X value. Draw a scatter plot of the negative electrode potential under different SOC states, and draw a linear trend line for the scatter plot. The intersection of the trend line and the straight line of y=0, the horizontal coordinate of the intersection can be considered as the maximum charging rate under the SOC.

[0109] The trend line formula of the linear relationship is: Y=kX+b.

[0110] Y: negative electrode potential at different charging rates under the same SOC, unit V; X: charging rate, unit C; k: constant, the slope of the scatter plot trend line under a certain SOC, dimension is 1; b: constant, the intercept of the scatter plot trend line under a certain SOC, dimension is 1; 5. Select the maximum charging rate under SOC: X(max) = -b / k.

[0111] The maximum charging rate corresponding to 10% SOC is X(max)10%, and so on. The shortest charging time for 10%-80% SOC is: T=6 / X(max)20%+6 / X(max)30%+6 / X(max)40%+6 / X(max)50%+6 / X(max)60%+6 / X(max)70%+6 / X(max)80%, in minutes.

[0112] Maximum charging rate of 10%-80%: X(max)10%-80%=60×(80%-10%) / T.

[0113] 2. Energy density test

[0114] At 25°C, the battery is fully charged at 0.2C, fully discharged at 0.2C, and the battery is weighed. The ratio of the 0.2C full discharge capacity to the battery weight is the energy density of the battery. The expected energy density is 120Wh / kg, and the actual energy density is 120±5%Wh / kg (114-126Wh / kg) is considered moderate, 5%-20% lower than the expected energy density (96-114Wh / kg) is considered low, and 20% lower than the expected energy density is considered low (<96Wh / kg); 5%-20% higher than the expected energy density (126-132Wh / kg) is considered high, and 20% higher than the expected energy density (>132Wh / kg) is considered high.

[0115] The battery performance test results are shown in Table 1.

[0116] Table 1 Battery performance test results

[0117] Group Actual energy density (Wh / kg) Maximum charging rate Example 1 98 3.8C Example 2 116 3.6C Example 3 117 3.3C Example 4 121 3.1C Example 5 124 2.8C Example 6 140 2C Comparative Example 1 85 1.9C Comparative Example 2 110 1.8C

[0118] It can be seen from Examples 1-6 that when the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction and the particle size Dv50 of the negative electrode active material satisfy the relationship 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2, the negative electrode has good energy density and charging rate; when 3.2<(P / La) 1 / 2 / (0.1×D V50 )<4, the negative electrode has a higher rate performance and a lower energy density; when 0.7<(P / La) 1 / 2 / (0.1×D V50 )<0.8, the negative electrode has a higher energy density and a general charging capacity. 1 / 2 / (0.1×D V50 )>4 or (P / La) 1 / 2 / (0.1×D V50 )<0.7, the energy density of the negative electrode is low and the charging capacity is poor.

[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A negative electrode sheet, characterized in that: The invention comprises a negative electrode current collector and a negative electrode material layer located on at least one side of the negative electrode current collector, wherein the negative electrode material layer contains a negative electrode active material; the porosity P of the negative electrode sheet, the crystal size La of the negative electrode active material along the (100) direction, and the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4.

2. The negative electrode sheet according to claim 1, characterized in that: The porosity P of the negative electrode sheet, the size La of the crystals of the negative electrode active material along the (100) direction, and the particle size Dv50 corresponding to the cumulative volume percentage of the negative electrode active material reaching 50% satisfy the relationship: 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.

2.

3. The negative electrode sheet according to claim 1, characterized in that: The porosity P of the negative electrode sheet is 30% to 70%, the crystal size La of the negative electrode active material along the (100) direction is 1.5 to 2.2 nm; and the particle size Dv50 of the negative electrode active material is 2 to 7 μm.

4. The negative electrode sheet according to claim 3, characterized in that: The porosity P of the negative electrode sheet is 40% to 60%, the crystal size La of the negative electrode active material along the (100) direction is 1.6 to 2 nm; and the particle size Dv50 of the negative electrode active material is 3 to 5.5 μm.

5. The negative electrode sheet according to claim 1, characterized in that: The negative electrode active material includes at least one of hard carbon, soft carbon, graphite and carbon-based composite materials; And / or, the negative electrode sheet further includes a conductive agent and a binder, the mass content of the conductive agent in the negative electrode material layer is 1% to 3%, and the mass content of the binder in the negative electrode material layer is 1% to 3.5%.

6. The negative electrode sheet according to claim 5, characterized in that: The mass content of the hard carbon in the negative electrode active material is greater than 50%.

7. The method for preparing a negative electrode sheet according to any one of claims 1 to 6, characterized in that: The following steps are involved: Applying a negative electrode slurry containing a negative electrode active material on at least one side of the negative electrode current collector, wherein the particle size of the negative electrode active material is Dv50, and drying to obtain a negative electrode sheet; Testing the porosity P of the negative electrode material layer on at least one side of the negative electrode sheet and the size La of the crystals of the negative electrode active material along the (100) direction; The porosity P, La and particle size Dv50 are obtained to satisfy 0.7≤(P / La) 1 / 2 / (0.1×D V50 )≤4 negative electrode sheet.

8. The method for preparing a negative electrode sheet according to claim 8, characterized in that: The porosity P of the negative electrode sheet, the size La of the crystal of the negative electrode active material along the (100) direction, and the particle size Dv50 of the negative electrode active material satisfy 0.8≤(P / La) 1 / 2 / (0.1×D V50 )≤3.2 negative electrode; And / or, the negative electrode slurry further comprises a binder, a conductive agent, and optionally a dispersant and a solvent.

9. A secondary battery, characterized in that: The negative electrode sheet comprises the negative electrode sheet according to any one of claims 1 to 7.

10. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 9.

Citation Information

Cited By

  • A negative electrode sheet, a method for manufacturing the negative electrode sheet, and a battery

    CN122781819A

  • A negative electrode sheet, a method for manufacturing the negative electrode sheet, and a battery

    CN122781819B