Coating liquid

By adding appropriate amounts of moisture, phosphorus, boron and surfactant to the coating liquid, the problem of poor wetting of the positive electrode active substance and the coating liquid is solved, the coating rate and uniformity of the coating film are improved, and more efficient coating is achieved Effect.

CN119069664APending Publication Date: 2024-12-03TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410363572.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-06-02
Filing Date
2024-03-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, the wettability of the positive electrode active material and the coating liquid is poor, which makes it difficult to improve the coating rate of the coating.

Method used

A coating liquid was developed that contains moisture, M elements (phosphorus and boron) and surfactant. The content of M elements is between 0.05% and 3.0%, the content of lithium is less than 0.1%, and the surface energy is less than 50mN/m. The absorbance is 0.1 or less, and the coating capacity of the coating liquid is improved by these compositions.

Benefits of technology

The uniformity and coating ratio of the coating are improved, the rise of solution pH is suppressed, the dissolution of M elements is promoted, the surface energy is reduced, the wetting of the coating liquid and the positive electrode active material is enhanced, and a more uniform coating is formed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069664A_ABST
    Figure CN119069664A_ABST
Patent Text Reader

Abstract

The present invention provides a coating liquid for forming a coating film on the surface of a positive electrode active material, the coating liquid containing a solvent and a solute, the solvent containing moisture, the solute containing an M element, the M element containing at least one element selected from phosphorus and boron, the content of the element M in the coating liquid is 0.05-3.0 mass%, the content of lithium in the coating liquid is less than 0.1 mass%, the absorbance of the coating liquid at a wavelength of 660 nm is 0.1 or less, and the surface energy of the coating liquid is 50 mN / m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coating fluid. Background Art

[0003] Japanese Patent Application Laid-Open No. 2022-47501 discloses that, in order to uniformly form a coating layer on the surface of a positive electrode active material, a slurry containing a positive electrode active material and a coating solution is formed into droplets, and the slurry droplets are dried by air flow. Summary of the invention

[0004] Compared with the conventional rolling flow method, the method disclosed in Japanese Patent Application Laid-Open No. 2022-47501 has advantages such as increased processing speed, etc. However, in the method disclosed in Japanese Patent Application Laid-Open No. 2022-47501, since the wettability between the positive electrode active material and the coating liquid is poor, there is a tendency that the coating coverage is difficult to increase.

[0005] An object of the present invention is to provide a coating solution having a high coating ability.

[0006] [1] A coating solution for forming a coating film on the surface of a positive electrode active material.

[0007] The coating solution contains a solvent and a solute,

[0008] The solvent contains water,

[0009] The solute contains the element M,

[0010] The M element contains at least one selected from phosphorus and boron,

[0011] The content of the M element in the coating solution is 0.05 mass % or more and 3.0 mass % or less,

[0012] The lithium content in the coating solution is less than 0.1% by mass.

[0013] The absorbance of the coating solution at a wavelength of 660 nm is less than 0.1,

[0014] The surface energy of the coating solution is 50 mN / m or less.

[0015] By surface energy, the coating ability of the coating solution can be evaluated. High coating ability means that the coating rate is easily improved. Low surface energy of the coating solution means that the coating solution and the positive electrode active material have good wettability. It can be considered that if the coating solution and the positive electrode active material have good wettability, when the coating solution is applied to the surface of the positive electrode active material, the coating solution uniformly wets and expands, so that the film formed becomes uniform and the coating rate improves.

[0016] In addition, the coating ability of the coating solution can also be evaluated by absorbance. The low absorbance of the coating solution means that the concentration of the particles contained in the coating solution is low, that is, the solute has a significant dissolved residue or few insoluble components. If the concentration of the particles contained in the coating solution is low, when the coating solution is applied to the surface of the positive electrode active material, the concave-convexity of the film formed becomes less, the unevenness of the thickness is also suppressed, and the coverage rate is improved.

[0017] In addition, the content of lithium in the coating solution of the present disclosure is less than 0.1% by mass. When the content of lithium in the coating solution is less than 0.1% by mass, the increase in solution pH can be suppressed, the dissolution of the M element in the coating solution can be promoted, and the surface energy can be reduced.

[0018] The coating solution of the present disclosure has a surface energy of 50 mN / m or less, an absorbance of 0.1 or less at a wavelength of 660 nm, and a lithium content of less than 0.1% by mass. In this case, the coating solution can have excellent coating ability.

[0019] [2] The coating solution as described in [1], further comprising a surfactant

[0020] The content of the surfactant in the coating solution is 0.01 mass % or more and 1.5 mass % or less.

[0021] [3] The coating solution according to [1] or [2], wherein the surface energy of the coating solution is 15 mN / m or more and 30 mN / m or less.

[0022] [4] A coating solution for forming a coating on the surface of a positive electrode active material, characterized in that

[0023] The coating solution contains a solvent, a solute and a surfactant.

[0024] The solvent contains water,

[0025] The solute contains the element M,

[0026] The M element contains at least one selected from phosphorus and boron,

[0027] The content of the M element in the coating solution is 1.5 mass % or more and 2.6 mass % or less,

[0028] The content of lithium in the coating solution is less than 0.1% by mass.

[0029] The absorbance of the coating solution at a wavelength of 660 nm is less than 0.1,

[0030] The surface energy of the coating solution is greater than 15 mN / m and less than 30 mN / m,

[0031] The content of the surfactant in the coating solution is 0.1 mass % or more and 1.0 mass % or less. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a line graph showing the relationship between the surface energy value and the coverage in No. 1 to 3;

[0033] Figure 2 is a line graph showing the relationship between the surface energy values ​​and the coverage of No. 4 to 10;

[0034] Figure 3 This is a graph showing the relationship between the surface energy value and the coverage in No. 11 and 12. DETAILED DESCRIPTION

[0035] The following will describe the features, advantages, and technical and industrial significance of an embodiment of the present disclosure (hereinafter referred to as "the present embodiment") and an example of the present disclosure (hereinafter referred to as "the present example") with reference to the accompanying drawings, wherein like symbols represent like elements. However, the present embodiment and the example are not intended to limit the technical scope of the present disclosure.

[0036] Coating fluid

[0037] The coating solution includes a solvent and a solute. The solvent includes water. The solute includes an M element. The element M includes at least one selected from phosphorus (P) and boron (B). The coating solution may also contain, for example, suspended matter (insoluble components), precipitates, etc. In addition, the "solute" in the present disclosure does not include the surfactant described later.

[0038] Solvents

[0039] The solvent contains water. The solvent preferably contains water as the main component. The solvent may also be composed of water. The solvent may contain, for example, ion-exchanged water. The solvent, for example, preferably contains ion-exchanged water as the main component. The solvent, for example, may also be composed of ion-exchanged water. The solvent may contain any component as long as it can dissolve the solute. The solvent may contain, for example, alcohol, etc. The solvent may contain, for example, ethanol, etc. In addition, "containing water as the main component" means that the water content in the solvent exceeds 50% by mass.

[0040] The content of water in the coating solution is preferably 90% by mass or more and 97% by mass or less. When the water content in the coating solution is less than 90% by mass, it may be difficult to use the coating solution to coat the positive electrode active material particles. When the water content in the coating solution exceeds 97% by mass, the solute concentration in the coating solution is low, and the coverage of the film may not be high. The content of water in the coating solution may be, for example, 91% by mass or more, or 93% by mass or more. The content of the solvent in the coating solution may be, for example, 96% by mass or less, or 95% by mass or less.

[0041] The amount of water in the coating solution is measured by volumetric titration using a Karl Fischer titrator. For example, a Karl Fischer titrator "product name MKA-610" produced by Kyoto Electronics Industry Co., Ltd. is prepared. In order to measure the amount of water, a titration solution and a solvent are prepared. As a titration solution, for example, "product name: Conpot 5K (made by Honeywell) can be considered, and as a solvent, "product name: Midiam K (made by Honeywell) can be considered. The amount of water is measured by anhydrating the solvent in the titration flask with a titration solution and adding the coating solution.

[0042] Solute

[0043] P is contained in the form of a phosphorus compound. As the phosphorus compound, for example, a phosphoric acid compound can be cited. The phosphoric acid compound may contain at least one selected from, for example, phosphoric anhydride (P2O5), orthophosphoric acid, pyrophosphoric acid, metaphosphoric acid, polyphosphoric acid and their sodium salts, lithium salts and potassium salts. As the phosphoric acid compound, metaphosphoric acid, polyphosphoric acid and their sodium salts, lithium salts and potassium salts are preferred. Compared with other phosphoric acid compounds, metaphosphoric acid and polyphosphoric acid can have longer molecular chains. By containing at least one of metaphosphoric acid and polyphosphoric acid in the solute, it can be expected that, for example, a continuous film can be easily formed. Thus, for example, it is expected to increase the coverage rate.

[0044] B is contained in the form of a boron compound. Examples of the boron compound include boric acid compounds. The boric acid compound may include at least one selected from, for example, orthoboric acid, metaboric acid, and tetraboric acid.

[0045] The solute preferably contains P and B. When the solute contains P and B, the surface energy can be expected to be further reduced.

[0046] The content of the M element in the coating solution is 0.05 mass % or more and 3.0 mass % or less. When the content of the M element in the coating solution is lower than 0.05 mass %, the concentration of the M element in the coating solution is low, and the coverage of the film may not be high. When the content of the M element in the coating solution exceeds 3.0 mass %, it is possible that the M element cannot be completely dissolved in the coating solution. The content of the M element in the coating solution can be, for example, 0.2 mass %, 0.5 mass %, 1.0 mass %, 1.5 mass %. The content of the M element in the coating solution can be 2.9 mass % or less, 2.8 mass % or less, 2.7 mass % or less, 2.6 mass % or less.

[0047] The content of lithium (Li) in the coating solution is less than 0.1% by mass. When the content of Li is 0.1% by mass or more, the pH value of the solution rises, and it is possible that the M element is not completely dissolved in the coating solution. In addition, in the coating solution, as long as the content of lithium (Li) is less than 0.1% by mass, the solute may also contain a lithium compound. The lithium compound may contain, for example, lithium hydroxide, lithium nitrate, lithium carbonate, etc.

[0048] The concentration of the solute in the coating solution is determined according to the following steps. 0.1 g of the coating solution is mixed with pure water and hydrochloric acid and heated. After cooling, hydrogen peroxide is further added and heated. After cooling, it is calibrated to 100 mL and a sample solution is prepared. An inductively coupled plasma atomic emission spectrometer (ICP-AES) device is prepared. For example, the concentration of the solute in the coating solution is determined using an ICP-AES device "product name CP-720" manufactured by Agilent Technologies.

[0049] Surfactants

[0050] The coating solution may also contain a surfactant. By containing a surfactant in the coating solution, it is expected that the coverage rate will be improved. The surfactant may be an insoluble component. The surfactant may also be a soluble component (solute). The surfactant may be water-soluble, for example. By dissolving the surfactant, it is possible to increase the coverage rate. The surfactant may be cationic, anionic, amphoteric or nonionic. By having the surfactant be nonionic, the coverage rate can be increased. The surfactant may contain at least one selected from, for example, polyether-modified siloxanes and polyethylene glycol alkyl ethers. As polyether-modified siloxanes, for example, "Product Name: Silsurf C208 (manufactured by SILTECH)", "Product Name: KF-945 (manufactured by Shin-Etsu Chemical Co., Ltd.)" and the like can be considered. As polyethylene glycol alkyl ethers, for example, polyethylene glycol monolauryl ether (manufactured by Tokyo Chemical Industry Co., Ltd.) and the like can be considered.

[0051] The content of the surfactant in the r' solution is preferably 0.01% to 1.5% by mass. When the content of the surfactant in the coating solution is less than 0.01% by mass, the effect of increasing the coverage by containing the surfactant may not be obtained. When the content of the surfactant in the coating solution exceeds 1.5% by mass, precipitation or an increase in insoluble components may occur. The content of the surfactant in the coating solution may be, for example, 0.1% by mass or more, 0.2% by mass or more, or 0.5% by mass or more. The content of the surfactant in the coating solution may be, for example, less than 1.4% by mass, less than 1.2% by mass, or less than 1.0% by mass.

[0052] Absorbance

[0053] The absorbance of the coating solution at a wavelength of 660nm is less than 0.1. Here, the absorbance at a wavelength of 660nm represents the intensity of scattered light caused by the microparticles present in the coating solution. The higher the absorbance value, the higher the concentration of the microparticles present in the coating solution, that is, there are more dissolved residues of the solute or more insoluble components (for example, refer to JIS-K0101). When a coating solution with a high concentration of microparticles is applied to the positive electrode active material, the microparticles adhere to the surface of the positive electrode active material, the film becomes uneven, and the thickness of the film becomes uneven. When the thickness of the film becomes uneven, a portion of the film with insufficient thickness or a portion that is not coated is generated, resulting in a reduction in the coating rate.

[0054] When the absorbance of the coating solution at a wavelength of 660 nm is 0.1 or less, it is considered that the concentration of the microparticles in the coating solution is low, the thickness of the film becomes uniform, and the coverage rate can be expected to increase. The absorbance of the coating solution at a wavelength of 660 nm may be 0.

[0055] The absorbance value is measured according to the following steps. Collect 3.5 mL of the coating solution in a quartz cell (10 mm × 10 mm × 45 mm). Use a UV-visible spectrophotometer to measure the absorbance of the coating solution. For example, prepare an UV-visible spectrophotometer "Product Name UV-1280" manufactured by Shimadzu Corporation. The temperature of the coating solution in the measurement is 25°C. At this time, the lower limit value of the absorbance is 0.000. However, the detection limit of the UV-visible spectrophotometer used in the absorbance measurement is 0.001. In addition, the zero point of the absorbance can be the absorbance obtained by placing ultrapure water with a conductivity of 17 MΩ·cm or more and 25°C into the measuring cell.

[0056] Surface energy

[0057] The surface energy of the coating liquid is less than 50 mN / m. Here, surface energy is synonymous with surface tension. By reducing the surface energy value of the coating liquid, the wettability with the positive electrode active material becomes better, and when the coating liquid is applied to the surface of the positive electrode active material, it is uniformly wetted and expanded. As a result, the formed film is uniform, the insufficient thickness of the film or the uncoated part is reduced, and the reduction of the coverage rate is suppressed.

[0058] When the surface energy of the coating solution is 50 mN / m or less, the thickness of the film becomes uniform and the coverage is expected to increase. The surface energy of the coating solution may be 45 mN / m or less, or 41 mN / m or less. The surface energy of the coating solution is preferably 30 mN / m or less, and preferably 26 mN / m or less. The surface energy of the coating solution is more preferably 20 mN / m or less.

[0059] On the other hand, if the surface energy of the coating solution is too small relative to the surface energy of the positive electrode active material, there is a tendency for the coating solution to be easily peeled off from the surface of the positive electrode active material. As a result, the film formed may be uneven and the coverage rate is reduced. Therefore, the surface energy is preferably more than 10mN / m.

[0060] The value of the surface energy is measured by the pendant drop method using a contact angle meter. For example, a contact angle meter "DMo-502" manufactured by Kyowa Interface Science Co., Ltd. is prepared. As a probe liquid, diiodomethane and n-hexadecane are prepared. The coating liquid is squeezed out from a capillary in the probe liquid, and the image is taken after 1000ms, and then the image is recorded 300 times at intervals of 1000ms. The recorded images read by the attached multifunctional comprehensive analysis software FAMAS are analyzed according to the Young-Laplace method to calculate the surface energy. The temperature of the coating liquid during the measurement is 25°C.

[0061] use

[0062] The coating solution disclosed in the present invention is used to form a coating on the surface of the positive electrode active material. The positive electrode active material can be composed of one particle or can contain two or more particles. The positive electrode active material has an average particle size (D50) of, for example, 1 μm or more and 30 μm or less. "D50" represents the particle size when the cumulative volume-based particle size distribution (cumulative distribution) is 50%. The particle size distribution can be measured by laser diffraction.

[0063] The positive electrode active material may contain any component. For example, the positive electrode active material may contain at least one selected from Li(NiCoMn)O2 and Li(NiCoAl)O2. For example, the "(NiCoMn)" in "Li(NiCoMn)O2" means that the total composition ratio in the brackets is 1. Li(NiCoMn)O2 may include, for example, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2, etc. Li(NiCoAl)O2 may include, for example, LiNi 0.8 Co 0.15 Al 0.05 O2, etc.

[0064] Method for preparing coating solution

[0065] The method for preparing the coating solution of the present invention is not particularly limited. For example, the coating solution is prepared by dissolving a solute in a solvent. When the solute contains both P and B as M elements, the two may be mixed in the solvent simultaneously or separately. In addition, when a surfactant is added, the surfactant may be mixed with the solute simultaneously or separately.

[0066] Sample preparation

[0067] Coating solutions No. 1 to 12 and positive electrode active materials coated with the coating solutions (hereinafter also referred to as "coated positive electrode active materials") were prepared as follows. Hereinafter, for example, "coating solution No. 1" may be simply referred to as "No. 1".

[0068] No.1

[0069] A coating solution was prepared by dissolving 6.0 g of metaphosphoric acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) in 92.14 g of ion-exchanged water.

[0070] As the positive electrode active material, NCM (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2). The powder of the positive electrode active material is dispersed in the coating solution to prepare a slurry (solid content concentration: 69 mass %). A spray dryer "MiniSprayDryerB-290" produced by BUCHI was prepared. The slurry was supplied to the spray dryer to produce a powder coated with the positive electrode active material. The air supply temperature of the spray dryer was 200°C and the air supply volume was 0.45m 3 / min. The coated positive electrode active material was heat treated in air. The heat treatment temperature was 200°C and the heat treatment time was 5 hours.

[0071] No.2

[0072] The coating solution No. 1 was prepared by dissolving polyethylene glycol monolauryl ether (manufactured by Tokyo Chemical Industry Co., Ltd.) as a polyethylene glycol alkyl ether at a concentration of 1.0 mass %. Then, a coated positive electrode active material was prepared in the same manner as in No. 1.

[0073] No.3

[0074] A coating solution was prepared by dissolving polyether-modified siloxane (KF-945 manufactured by Shin-Etsu Chemical Co., Ltd.) in the coating solution No. 1 to a concentration of 1.0 mass %. Then, a coated positive electrode active material was prepared in the same manner as in No. 1.

[0075] No.4

[0076] A phosphoric acid solution was prepared by dissolving 2.15 g of metaphosphoric acid (manufactured by Fujifilm and Koshun Pharmaceutical) in 66.05 g of ion exchange water. Furthermore, a coating solution was prepared by dissolving boric acid (manufactured by Nakalai Tesque) in the phosphoric acid solution so that the molar ratio of P to B was 1:1. Then, a coated positive electrode active material was prepared in the same manner as in No. 1.

[0077] No.5 to 6

[0078] Coating solution No. 5 was prepared by dissolving polyethylene glycol alkyl ether in coating solution No. 4 at a concentration of 0.5 mass %, and coating solution No. 6 was prepared by dissolving polyethylene glycol alkyl ether in a concentration of 1.0 mass %. Then, each coated positive electrode active material was prepared in the same manner as in No. 1.

[0079] No.7 to 10

[0080] The coating solution No. 7 was prepared by dissolving polyether-modified siloxane in the coating solution No. 4 to a concentration of 0.01 mass %, the coating solution No. 8 was prepared by dissolving polyether-modified siloxane in the coating solution No. 4 to a concentration of 0.1 mass %, the coating solution No. 9 was prepared by dissolving polyether-modified siloxane in the coating solution No. 4 to a concentration of 0.5 mass %, and the coating solution No. 10 was prepared by dissolving polyether-modified siloxane in the coating solution No. 4 to a concentration of 1.0 mass %. Then, each coated positive electrode active material was prepared by the same method as No. 1.

[0081] No.11

[0082] A phosphoric acid solution was prepared by dissolving 6.0 g of metaphosphoric acid (manufactured by Fujifilm and Koshun Pharmaceutical) in 109.0 g of ion exchange water. Furthermore, a coating solution was prepared by dissolving boric acid (manufactured by Nacalai Tesque) in the phosphoric acid solution so that the molar ratio of P to B was 1:1. Then, a coated positive electrode active material was prepared in the same manner as in No. 1.

[0083] No.12

[0084] A coating solution was prepared by dissolving polyethylene glycol alkyl ether in the coating solution No. 11 so as to have a concentration of 0.5 mass %. Then, a coated positive electrode active material was prepared in the same manner as in No. 1.

[0085] Evaluate

[0086] Coating fluid

[0087] Water content

[0088] The amount of water contained in the coating solution was measured by volumetric titration using a Karl Fischer titrator. The results are shown in Table 1.

[0089] Element M

[0090] The concentration (mass %) of the M element contained in the coating solution was measured by ICP-AES. The results are shown in Table 1. In addition, the concentration of Li contained in each coating solution was measured, but it could not be measured because it was not contained or was below the detection limit.

[0091] Absorbance

[0092] Absorbance

[0093] The absorbance of the coating solution was measured by UV-Vis spectrophotometer. The results are shown in Table 1.

[0094] Surface energy

[0095] The surface energy of the coating solution was measured by the pendant drop method using a contact angle meter. The results are shown in Table 1.

[0096] Coated positive electrode active material

[0097] coverage rate

[0098] The coating rate of the coated positive electrode active material was determined by X-ray photoelectron spectroscopy (XPS). As an XPS device, an XPS device "product name PHIX-tool" produced by Albuck Fiai was prepared. The sample powder formed by the coated positive electrode active material was set in the XPS device. Narrow scan analysis was performed with a pass energy of 224 eV. The measurement data was processed by the analysis software "product name MulTiPak" produced by Albuck Fiai.

[0099] By analyzing the measurement data, the ratio (element concentration) of each element was determined from the peak areas of Li1s, B1s, P2p, Ni2p3, Co2p3 and Mn2p3. The coverage was determined by the following formula (1).

[0100] θ=M / (M+Ni+Co+Mn)×100……(1)

[0101] In the above formula (1), θ represents the coverage (%). M, Ni, Co and Mn represent the ratio of each element. M represents P in the coated positive electrode active materials No. 1 to 3 and P and B in the coated positive electrode active materials No. 4 to 12, respectively.

[0102] The coverage rate is shown in Table 1 and Figure 1-Figure 3 The relative values ​​are expressed with reference to No. 1, 4 and 11 without surfactant. That is, the values ​​of No. 2 and 3 are relative values ​​with reference to No. 1, the values ​​of No. 5 to 10 are relative values ​​with reference to No. 4, and the value of No. 12 is relative value with reference to No. 11.

[0103] (Table 1)

[0104]

[0105] *1: Relative value based on No.1

[0106] *2: Relative value based on No.4

[0107] *3: Relative value based on No.11

[0108] result

[0109] According to Table 1 and Figures 1 to 3 The results show that sufficient coverage of the positive electrode active material can be achieved by using coating solutions No. 2, 3, 5, 7 to 10 and 12. In addition, by containing a surfactant, the surface energy is reduced, resulting in a higher coverage of the positive electrode active material.

[0110] The present embodiment and the present example are merely illustrative in all respects. The present embodiment and the present example are not intended to be interpreted restrictively. The technical scope of the present invention includes all changes within the meaning and scope equivalent to the description of the claims. For example, any structure can be extracted from the present embodiment and the present example, and they can be combined arbitrarily, which is also within the scope originally intended in the present application.

Claims

1. A coating solution for forming a coating film on the surface of a positive electrode active material, The coating solution contains a solvent and a solute, The solvent contains water, The solute contains the element M, The M element contains at least one selected from phosphorus and boron, The content of the M element in the coating solution is 0.05 mass % or more and 3.0 mass % or less, The lithium content in the coating solution is less than 0.1% by mass. The absorbance of the coating solution at a wavelength of 660 nm is less than 0.1, The surface energy of the coating solution is 50 mN / m or less.

2. The coating solution according to claim 1, further comprising a surfactant, The content of the surfactant in the coating solution is 0.01 mass % or more and 1.5 mass % or less. 3 . The coating solution according to claim 1 , wherein the surface energy of the coating solution is 15 mN / m or more and 30 mN / m or less.

4. A coating solution for forming a coating film on the surface of a positive electrode active material, The coating solution contains a solvent, a solute and a surfactant. The solvent contains water, The solute contains the element M, The M element contains at least one selected from phosphorus and boron, The content of the M element in the coating solution is 1.5 mass % or more and 2.6 mass % or less, The content of lithium in the coating solution is less than 0.1% by mass. The absorbance of the coating solution at a wavelength of 660 nm is less than 0.1, The surface energy of the coating solution is greater than 15 mN / m and less than 30 mN / m, The content of the surfactant in the coating solution is 0.1 mass % or more and 1.0 mass % or less.