Ternary positive electrode material, mixed positive electrode material, positive plate and battery
By covering metal elements on the surface of the NCM core and combining it with lithium manganese iron phosphate material, the safety problems of pure NCM power batteries in overcharge and needle punch testing are solved, and high energy density and safety performance are achieved, reducing the risk of high energy density and safety performance. Battery cost.
Patent Information
- Application Number
- CN202411372726.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-03
AI Technical Summary
Pure NCM power batteries have low safety in overcharge and needle punch testing, and existing solutions improve safety by increasing components but increase costs and affect energy density.
By covering metal elements Al and/or W, as well as Sr and/or Zr on the surface of the NCM core, a ternary positive electrode material is formed and combined with lithium manganese iron phosphate material to form a mixed positive electrode material to improve thermal stability and cyclic stability sex.
While maintaining high energy density, the safety performance of the battery is significantly improved, cost reduction, and enhanced overcharge and needle-punching safety of the battery by improving thermal stability and cycling stability.
Smart Images

Figure CN119069683A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a ternary positive electrode material, a mixed positive electrode material, a positive electrode sheet and a battery. Background Art
[0002] As an important component of modern energy storage devices, lithium-ion batteries are widely used in electric vehicles, portable electronic devices and other fields. 0.8 Co 0.1 Mn 0.1 O2, abbreviated as NCM) has attracted much attention due to its high energy density and good rate performance, and has become one of the mainstream positive electrode materials in the current lithium-ion battery market. However, pure NCM power batteries still have some challenges in practical applications, especially in overcharge and needle penetration tests, showing low safety.
[0003] In order to solve the safety problem of pure NCM power batteries in overcharge and needle penetration tests, the current common practice is to add some components such as safety valves, thermistors, etc. However, the additional addition of these components not only increases the manufacturing cost of the battery, but may also have a negative impact on the battery's energy density and other performance. Therefore, how to maintain the high energy density of NCM materials while improving its safety performance and reducing battery costs is an important topic in the current research and development of lithium-ion batteries. Summary of the invention
[0004] In view of this, the present application provides a ternary positive electrode material and a mixed positive electrode material, which improves the safety performance of the NCM material while maintaining its high energy density.
[0005] In a first aspect, the present application provides a ternary positive electrode material, comprising a NCM core and a coating layer covering at least a portion of the surface of the NCM core; the coating layer comprises a metal element M1 and a metal element M2, the metal element M1 is Al and / or W, and the metal element M2 is Sr and / or Zr;
[0006] Based on the mass of the ternary positive electrode material, the content of the metal element M1 is W1, the content of the metal element M2 is W2, and 0.2≤W1 / W2≤1.2.
[0007] In an optional embodiment, the coating layer includes metal elements Al, Zr, W and Sr, and the content of Al is W 1a 、Zr content W 2a 、W content 1b and Sr content W 2b Satisfy: 0.16 ≤ W 1a *W 1b / (W 2a *W2b )≤0.8.
[0008] In an optional embodiment, 800ppm≤W 1a ≤1200ppm.
[0009] In an optional embodiment, 2500ppm≤W 2a ≤3500ppm.
[0010] In an optional embodiment, 700ppm≤W 1b ≤1000ppm.
[0011] In an optional embodiment, 600ppm≤W 2b ≤1000ppm.
[0012] In an optional embodiment, the chemical formula of the NCM core is LiNi x Co y Mn z O2, where x+y+z=1, 0.8≤x<1, 0 <y<0.2,0<z<0.2。
[0013] In an optional embodiment, the ternary positive electrode material is a single crystal material, and its particle size Dv501 is 2 μm-5 μm.
[0014] In an optional embodiment, the metal element is selected from the group consisting of Al2O3, ZrO2, WO3 and SrO.
[0015] In a second aspect, the present application provides a mixed positive electrode material, including a lithium iron manganese phosphate material and the ternary positive electrode material described in the first aspect of the present application, and the mass ratio of the ternary positive electrode material to the lithium iron manganese phosphate material is 7:3-4:6.
[0016] In an optional embodiment, the lithium manganese iron phosphate material includes a LMFP core and a carbon coating layer covering at least a portion of the surface of the LMFP core, and the content of the carbon coating layer is 1%-3% based on the mass of the lithium manganese iron phosphate material.
[0017] In an optional embodiment, the chemical formula of the LMFP core is LiFe x Mn 1-x PO4,0 <x≤0.4。
[0018] In an optional embodiment, the particle size Dv502 of the lithium manganese iron phosphate material is 0.5 μm-1.5 μm.
[0019] In a third aspect, the present application also provides a positive electrode sheet, comprising a current collector and a positive electrode active material layer arranged on at least one side surface of the current collector, wherein the positive electrode active material layer comprises the ternary positive electrode material described in the first aspect of the present application or the mixed positive electrode material described in the second aspect of the present application.
[0020] In an optional embodiment, the positive electrode sheet formed by the ternary positive electrode material described in the first aspect of the present application is recorded as the first positive electrode sheet, and the positive electrode sheet formed by the mixed positive electrode material described in the second aspect of the present application is recorded as the second positive electrode sheet; the DSC thermal decomposition temperature of the first positive electrode sheet is T1, T1≥206°C; the DSC thermal decomposition temperature of the second positive electrode sheet is T2, T2≥212°C; and / or, the thermal decomposition enthalpy of the first positive electrode sheet is Q1, 1200J / g≥Q1≥800J / g; the thermal decomposition enthalpy of the second positive electrode sheet is Q2, Q2<800J / g.
[0021] In an optional embodiment, a pasted area and an insulating area are provided on the surface of the current collector along the length direction, and the pasted area is connected to the insulating area but does not overlap; the positive electrode active material layer is provided in the pasted area, and the positive electrode active material layer includes the mixed positive electrode material, and an insulating layer is provided in the insulating area, and the thickness H1 of the positive electrode active material layer, the thickness H2 of the current collector, the thickness H3 of the insulating layer and the mass proportion W3% of the lithium manganese iron phosphate material in the mixed positive electrode material satisfy: 4≤H1*H2*H3 / W3≤240.
[0022] In an optional embodiment, H1 is 30 μm-100 μm.
[0023] In an optional embodiment, H2 is 8 μm-16 μm.
[0024] In an optional embodiment, H3 is 1 μm-20 μm.
[0025] In an optional embodiment, W3 is 30-60.
[0026] In an optional embodiment, the insulating layer comprises inorganic particles and a binder in a mass ratio of (85-91):(9-15).
[0027] In an optional embodiment, the particle size of the inorganic particles satisfies: Dv99 / Dv503=3-5, and Dv503 is 0.6 μm-1.1 μm.
[0028] In an optional embodiment, the inorganic particles include at least one of aluminum oxide, boehmite, silicon dioxide, calcium oxide, titanium dioxide, zirconium dioxide, and magnesium oxide.
[0029] In an optional embodiment, the peeling force N of the insulating layer on the current collector is ≥ 0.3 kgf.
[0030] In a fourth aspect, the present application provides a battery, comprising the positive electrode sheet as claimed in the third aspect of the present application.
[0031] The technical solution of this application has the following advantages:
[0032] The ternary positive electrode material provided in the present application is obtained by coating at least two metal elements on at least part of the surface of the NCM core, wherein the metal element M1 is Al and / or W, the metal element M2 is Sr and / or Zr, and the content W1 of the metal element M1 and the content W2 of the metal element M2 satisfy: 0.2≤W1 / W2≤1.2, thereby enabling the ternary positive electrode material to have good thermal stability and cycle stability at the same time, thereby improving the safety performance of the ternary positive electrode material.
[0033] Additional aspects and advantages of the embodiments of the present application will be described and shown in part in the subsequent description, or explained through the implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0035] Figure 1 It is a schematic diagram of the structure of the positive electrode sheet prepared in Example 1 of the present application;
[0036] Figure 2 This is an XRD comparison chart of the positive electrode sheets prepared in Example 1 and Example 12 of the present application.
[0037] The reference numerals are described as follows:
[0038] 1. Active paste layer; 2. Current collector; 3. Insulating layer. DETAILED DESCRIPTION
[0039] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0040] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance. It should be noted that the terms "positive electrode active material layer" and "active paste layer" have the same meaning and can be replaced with each other; the terms "mixed positive electrode material" and "positive electrode active material" have the same meaning and can be replaced with each other.
[0041] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0042] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0043] In order to improve the safety performance of NCM power batteries without affecting their electrical performance, this application provides the following solutions.
[0044] According to a first aspect of the present application, a ternary positive electrode material is provided, comprising a NCM core and a coating layer covering at least a portion of the surface of the NCM core; the coating layer comprises a metal element M1 and a metal element M2, the metal element M1 is Al and / or W, and the metal element M2 is Sr and / or Zr;
[0045] Based on the mass of the ternary positive electrode material, the content of the metal element M1 is W1, the content of the metal element M2 is W2, and 0.2≤W1 / W2≤1.2.
[0046] The present application coats at least two metal elements on at least part of the surface of the NCM kernel, wherein the metal element M1 is Al and / or W, the metal element M2 is Sr and / or Zr, and the content W1 of the metal element M1 and the content W2 of the metal element M2 satisfy: 0.2≤W1 / W2≤1.2, thereby enabling the ternary positive electrode material to have good thermal stability and cycle stability at the same time, thereby improving the safety performance of the ternary positive electrode material. If W1 / W2 is too large or too small, it is not conducive to the cycle stability and safety of the ternary positive electrode material. As an example, the ratio of W1 / W2 can be, for example, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, etc., or within the range of any two of the above values.
[0047] In a specific embodiment, the coating layer includes metal elements Al, Zr, W and Sr at the same time, and the content of Al is W 1a 、Zr content W 2a 、W content 1b and Sr content W 2bBetween: 0.16≤W 1a *W 1b / (W 2a *W 2b )≤0.8, because Al has excellent thermal stability, it can prevent NCM particles from direct contact with the electrolyte, avoiding oxidation of the positive electrode material and the electrolyte under high voltage to produce gas and heat; W has good electrical conductivity and chemical stability as well as excellent thermal stability, which can not only improve the electronic transmission efficiency of the material, but also help to improve the thermal safety of the material; Zr and Sr can affect the lattice parameters and crystal structure stability of the material, which helps to reduce the phase change and structural degradation of the material, thereby improving the cycle life and stability of the battery; the above four metal elements work together to ensure that the ternary positive electrode material has both excellent electrochemical performance and high thermal stability. As an example, in some embodiments, W 1a *W 1b / (W 2a *W 2b ) can be 0.16, 0.25, 0.4, 0.5, 0.65, 0.8, etc. or within the range of any two of the above values. 1a *W 1b / (W 2a *W 2b ) ratio is too large or too small, which is not conducive to the cycle performance of the ternary positive electrode material.
[0048] In a specific embodiment, the metal elements Al, Zr, W and Sr in the coating layer of the ternary positive electrode material of the present application are present in their respective oxide forms, that is, the metal elements Al, Zr, W and Sr are from substances Al2O3, ZrO2, WO3 and SrO. In an optional embodiment, 800ppm≤W 1a ≤1200ppm, 2500ppm≤W 2a ≤3500ppm, 700ppm≤W 1b ≤1000ppm, 600ppm≤W 2b ≤1000ppm. As an example, the content of Al element in the ternary positive electrode material W 1a For example, it can be 800ppm, 900ppm, 1000ppm, 1100ppm, 1200ppm, etc. or within the range of any two of the above values. The content of Zr element W 2a For example, it can be 2500ppm, 2600ppm, 2800ppm, 3100ppm, 3300ppm, 3500ppm, etc. or within the range of any two of the above values. The content of W element W 1bIt can be 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm, 1000 ppm, etc., or within the range formed by any two of the above values. The content of Sr element can be 600 ppm, 650 ppm, 700 ppm, 750 ppm, 800 ppm, 850 ppm, 900 ppm, 950 ppm, 1000 ppm, etc., or within the range formed by any two of the above values.
[0049] To ensure that the cathode material has a high specific capacity, the NCM core can use a high-nickel ternary material with the chemical formula LiNi x Co y Mn z O2, where x + y + z = 1, 0.8 ≤ x < 1, 0 < y < 0.2, 0 < z < 0.2. However, the cycling performance and thermal stability of high-nickel ternary materials are poor, so the aforementioned metal element coating is more needed.
[0050] It can be understood that polycrystalline materials generally exist in the form of micron-sized aggregates, and there are a large number of grain boundaries inside the aggregates. During the charge and discharge process of the battery, due to the anisotropic lattice change, polycrystalline materials are prone to grain boundary cracking, resulting in the fragmentation of secondary particles, which in turn causes a rapid increase in side reactions, an increase in impedance, and a rapid decline in performance. By using single-crystal particles, not only can the grain boundaries be reduced and the occurrence of side reactions be reduced, but also the tap density can be increased, thereby improving the energy density of the material. Therefore, compared with polycrystalline materials, the safety performance and cycling performance of single-crystal materials are better. Therefore, a single-crystal ternary cathode material is selected in this application, and its particle size Dv501 is 2 μm - 5 μm, which can further improve the electrical performance and safety performance of the material. As an example, in some embodiments, the particle size Dv501 of the ternary cathode material can be 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, etc., or within the range formed by any two of the above values.
[0051] According to the second aspect of the present application, the present application provides a mixed cathode material, including lithium iron manganese phosphate material and the ternary cathode material described in the first aspect of the present application, and the mass ratio of the ternary cathode material to the lithium iron manganese phosphate material is 7:3 - 4:6.
[0052] Lithium manganese iron phosphate (LMFP for short) has good safety performance and cycle stability, can maintain good structural stability under high temperature and overcharge conditions, and is not prone to dangerous situations such as thermal runaway. Therefore, the present application compounds the lithium manganese iron phosphate material with the ternary positive electrode material, so that the lithium manganese iron phosphate material can separate the ternary positive electrode material with relatively poor thermal stability, avoid the heat accumulation of the ternary positive electrode material, thereby reducing the heat rapidly accumulated by the ternary positive electrode material during overcharge and acupuncture, and prevent the battery cell from thermal runaway. Therefore, the present application utilizes the framework structure of the lithium manganese iron phosphate material to ensure that the mixed positive electrode material has higher thermal stability and lower thermal runaway risk, so that the battery cell can meet the overcharge performance and acupuncture safety performance while taking into account the energy density. In some embodiments, the mass ratio of the ternary positive electrode material to the lithium manganese iron phosphate material can be, for example, 7:3, 6:4, 5:5, 4:6, etc. or within the range composed of any two of the above values.
[0053] It is understandable that the resistivity of pure LMFP material is relatively large, so the present application selects carbon-coated and / or nano-sized LMFP to effectively reduce the resistivity of LMFP. In an optional embodiment, the lithium manganese iron phosphate material includes an LMFP core and a carbon coating layer coating at least a portion of the surface of the LMFP core, and the content of the carbon coating layer is 1%-3% based on the mass of the lithium manganese iron phosphate material. The coating of an appropriate amount of carbon can improve the conductivity without affecting the electrical properties of LMFP. As an example, the content of the carbon coating layer can be, for example, 1%, 1.5%, 2%, 2.5%, 3%, etc., or within the range of any two of the above values. In some embodiments, the particle size Dv502 of the lithium manganese iron phosphate material is 0.5μm-1.5μm. As an example, the particle size Dv502 of the lithium manganese iron phosphate material can be, for example, 0.5μm, 0.75μm, 1.0μm, 1.25μm, 1.5μm, etc., or within the range of any two of the above values.
[0054] It is understandable that the introduction of an appropriate amount of manganese element in the LMFP core can increase the voltage platform of the lithium manganese iron phosphate material, thereby improving the energy density of the hybrid positive electrode material. Therefore, the chemical formula of the LMFP core selected in this application is LiFe x Mn 1- x PO4,0 <x≤0.4。
[0055] According to the third aspect of the present application, the present application also provides a positive electrode sheet, including a current collector and a positive electrode active material layer arranged on at least one side surface of the current collector, and the positive electrode active material layer includes the ternary positive electrode material described in the first aspect of the present application or the mixed positive electrode material described in the second aspect of the present application.
[0056] In a specific implementation manner, the positive electrode sheet formed by the ternary positive electrode material described in the first aspect of the present application is recorded as a first positive electrode sheet, and the positive electrode sheet formed by the mixed positive electrode material described in the second aspect of the present application is recorded as a second positive electrode sheet.
[0057] It is understandable that the thermal decomposition temperature is one of the important indicators for measuring the thermal stability of a substance. When the thermal decomposition temperature of a substance is high, it means that the substance can remain stable at a higher temperature and is not prone to decomposition or degradation. This application study found that the hybrid positive electrode sheet mixed with lithium iron manganese phosphate has higher thermal stability. Specifically, the DSC thermal decomposition temperature of the first positive electrode sheet is T1, T1 ≥ 206 ° C; the DSC thermal decomposition temperature of the second positive electrode sheet is T2, T2 ≥ 212 ° C, and T2 ≥ T1, T2-T1 ≥ 4 ° C, indicating that compared with the pure ternary positive electrode sheet (ie, the first positive electrode sheet), the hybrid positive electrode sheet mixed with lithium iron manganese phosphate material (ie, the second positive electrode sheet) has higher thermal stability, which significantly improves the overcharge safety and acupuncture safety of the battery cell. The term "thermal decomposition enthalpy" refers to the heat released by the complete decomposition of each gram of positive electrode material. In the present application, the thermal decomposition enthalpy of the first positive electrode sheet is Q1, 1200J / g≥Q1≥800J / g; the thermal decomposition enthalpy of the second positive electrode sheet is Q2, Q2<800J / g, indicating that compared with the pure ternary positive electrode sheet (i.e., the first positive electrode sheet), the hybrid positive electrode sheet mixed with lithium manganese iron phosphate material (i.e., the second positive electrode sheet) has higher thermal stability, which significantly improves the overcharge safety and puncture safety of the battery cell.
[0058] It should be noted that the thinner the positive electrode current collector (aluminum foil), the higher the energy density of the battery cell and the higher the puncture safety performance, but if the aluminum foil is too thin, the electrode sheet will break during rolling, affecting the battery cell yield; with the increase of the content of lithium iron manganese phosphate, the thermal stability of the positive electrode sheet is significantly enhanced, and the overcharge safety and puncture safety performance of the battery cell are also significantly improved, but if the content of lithium iron manganese phosphate is too high, the energy density of the battery cell will be reduced due to its low gram capacity and low compaction density; the thickness of the paste layer will affect the surface resistance of the electrode sheet while affecting the energy density of the battery cell. If the paste layer is too thick, the charging and discharging temperature rise of the battery cell will increase, and the cycle performance of the battery cell will deteriorate; if the finishing aluminum foil insulation layer is too thin, the puncture safety performance will deteriorate, and if it is too thick, the energy density of the battery cell will be reduced. Therefore, in an optional embodiment of the present application, the surface of the current collector is divided into a pasted area and an insulating area along the length direction, the pasted area is connected to the insulating area but does not overlap, the positive electrode active material layer is arranged in the pasted area, the positive electrode active material layer includes the mixed positive electrode material described in the second aspect of the present application, and the insulating layer is arranged in the insulating area. The thickness H1 of the positive electrode active material layer, the thickness H2 of the current collector, the thickness H3 of the insulating layer and the mass proportion W3% of the lithium manganese iron phosphate material in the mixed positive electrode material satisfy: 4≤H1*H2*H3 / W3≤240, thereby ensuring that the battery cell can take into account energy density, cycle performance, overcharge safety and acupuncture safety performance.
[0059] As an example, the value of H1*H2*H3 / W3 can be, for example, 4, 10, 30, 50, 80, 100, 125, 150, 175, 200, 220, 240, etc., or within the range of any two of the above values; the thickness H1 of the positive electrode active material layer is 30 μm-100 μm, for example, it can be 30 μm, 50 μm, 80 μm, 100 μm, etc., or within the range of any two of the above values; the thickness H2 of the current collector is 8 μm-16 μm, for example, it can be 8 μm, 1 0μm, 12μm, 14μm, 16μm, etc. or within the range formed by any two of the above values; the thickness H3 of the insulating layer is 1μm-20μm, for example, it can be 1μm, 3μm, 5μm, 8μm, 10μm, 12μm, 15μm, 18μm, 20μm, etc. or within the range formed by any two of the above values; the mass proportion W3 of the lithium manganese iron phosphate material in the mixed positive electrode material can be 30, 40, 50, 60, etc. or within the range formed by any two of the above values.
[0060] It is understandable that the insulating layer in the present application includes inorganic particles and adhesives. The inorganic particles may be, for example, at least one of aluminum oxide, boehmite, silicon dioxide, calcium oxide, titanium dioxide, zirconium dioxide, and magnesium oxide. The adhesive may be at least one of polymethyl methacrylate (PMMA), polyvinyl alcohol (PVA), polytetrafluoroethylene (PTFE), polyolefins (such as polypropylene PP, polyethylene PE, etc.) and polyvinylidene fluoride (PVDF). In order to ensure that the inorganic particles can be effectively adhered to the current collector during the acupuncture process, and the number of inorganic particles should be sufficient to improve the acupuncture pass rate, the mass of the inorganic particles and the adhesive must be (85-91): (9-15) in the present application. As an example, the mass of the inorganic particles and the adhesive is 85:15, 87:13, 89:11, 91:9, etc. or is within the range of any two of the above values.
[0061] In an optional embodiment, the particle size of the inorganic particles satisfies: Dv99 / Dv503=3-5, and the particle size Dv503 of the inorganic particles is 0.6μm-1.1μm. This can make the particle size distribution of the inorganic particles uniform, improve the bonding force between the insulating layer and the current collector, and ensure that the peeling force N of the insulating layer on the current collector is ≥ 0.3kgf. As an example, the particle size Dv503 of the inorganic particles can be, for example, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, 1.1μm, etc., or within the range of any two of the above values. The value of the particle size Dv99 / Dv503 of the inorganic particles can be 3, 3.5, 4, 4.5, 5, etc., or within the range of any two of the above values.
[0062] In a fourth aspect, the present application provides a battery, comprising the positive electrode sheet as claimed in claim 3. According to the above description, the battery provided by the present application can take into account energy density, cycle performance, overcharge safety and needle puncture safety performance.
[0063] The present application is further described in detail below in conjunction with specific examples, and these examples should not be construed as limiting the scope of protection claimed in the present application. Where specific experimental steps or conditions are not specified in the examples and comparative examples, the conventional experimental steps or conditions described in the literature in the art can be used. Where the manufacturer of the reagents or instruments used is not specified, they are all conventional reagent products that can be obtained commercially.
[0064] In all the examples and comparative examples of the present application, the unit % represents the mass percentage.
[0065] Example 1
[0066] S1. Preparation of positive electrode
[0067] First, an active paste layer 1 is coated on the positive electrode current collector aluminum foil. The specific operation is: the positive electrode active material, the conductive agent carbon nanotubes, and the binder PVDF are uniformly mixed in N-methylpyrrolidone (abbreviated as NMP) at a mass ratio of 96%, 2.4%, and 1.6% to obtain the positive electrode slurry to be coated. Among them, the positive electrode active material is a high-nickel ternary material and a lithium iron manganese phosphate material with a mass ratio of 7:3. The high-nickel ternary material is a single crystal material with a particle size Dv501 of 4.1μm. It includes an NCM core and a coating layer coated on the surface of the NCM core. Based on the mass of the high-nickel ternary material, the coating layer includes 1000ppm Al, 3000ppm Zr, 800ppm W and 700ppm Sr. The chemical formula of the NCM core is LiNi 0.8 Co 0.1 Mn 0.1 O2; the particle size Dv502 of the lithium manganese iron phosphate material is 0.9 μm, which includes a LMFP core and a carbon coating layer coated on the surface of the LMFP core. The content of the carbon coating layer is 1.5% based on the mass of the lithium manganese iron phosphate material. The chemical formula of the LMFP core is LiFe 0.4 Mn 0.6 PO4.
[0068] The positive electrode slurry is evenly coated on both sides of an aluminum foil (thickness 10 μm), and the coated slurry is baked to obtain an active paste layer with a thickness of 70 μm on both sides. Then, an insulating layer is coated on the empty foil position at the tail of the active paste layer on the aluminum foil. The specific operation is as follows: inorganic particulate alumina (Dv503=0.8 μm and Dv99=3.25 μm) and adhesive PVDF are mixed in a mass ratio of 90:10 and added to NMP and stirred evenly to form a slurry with a solid content of 45%. The slurry is then evenly coated on the empty foil at the tail of the active paste layer. After drying, an insulating layer connected to but not overlapping the paste layer is obtained, and the thickness is 10 μm. Finally, rolling, slitting, and sheeting are performed to obtain a positive electrode sheet to be wound, and its structure is as follows Figure 1 As shown, the XRD spectrum is shown in Figure 2 ,from Figure 2 It can be seen that the positive electrode sheet prepared in this embodiment has obvious lithium manganese iron phosphate characteristic peaks p1, p2, p3, and p4 between 19° and 36°.
[0069] S2. Preparation of negative electrode sheet
[0070] Graphite, conductive carbon black, sodium carboxymethyl cellulose and styrene-butadiene rubber (SBR) were added into deionized water in a blender at a mass ratio of 96:1.5:1:1.5, and the mixture was evenly mixed to obtain a negative electrode slurry to be coated with a solid content of 45%; the negative electrode slurry was coated on a 6 μm thick copper foil current collector, and after drying, the negative electrode sheet to be wound was obtained by rolling, slitting and sheeting.
[0071] S3. Production of finished batteries
[0072] The positive and negative electrode sheets to be wound are prepared into finished batteries through the steps of winding, packaging, baking, liquid injection, and formation.
[0073] Example 2
[0074] Except for the following contents, the rest is the same as Example 1.
[0075] The positive electrode active material adopts a high-nickel ternary material and a lithium iron manganese phosphate material with a mass ratio of 6:4. The high-nickel ternary material is a single crystal material with a particle size Dv501 of 2μm. It includes an NCM core and a coating layer coated on the surface of the NCM core. Based on the mass of the high-nickel ternary material, the coating layer includes 1000ppm Al, 2500ppm Zr, 1000ppm W and 800ppm Sr. The chemical formula of the NCM core is LiNi 0.8 Co 0.1 Mn 0.1 O2; the particle size Dv502 of the lithium manganese iron phosphate material is 0.5 μm, which includes a LMFP core and a carbon coating layer coated on the surface of the LMFP core. The content of the carbon coating layer is 2% based on the mass of the lithium manganese iron phosphate material. The chemical formula of the LMFP core is LiFe 0.3 Mn 0.7 PO4.
[0076] Example 3
[0077] Except for the following contents, the rest is the same as Example 1.
[0078] The positive electrode active material adopts a high-nickel ternary material and a lithium iron manganese phosphate material in a mass ratio of 5:5. The high-nickel ternary material is a single crystal material with a particle size Dv501 of 3.5μm. It includes an NCM core and a coating layer coated on the surface of the NCM core. Based on the mass of the high-nickel ternary material, the coating layer includes 800ppm Al, 3500ppm Zr, 700ppm W and 1000ppm Sr. The chemical formula of the NCM core is LiNi 0.9 Co 0.05 Mn 0.05 O2; the particle size Dv502 of the lithium manganese iron phosphate material is 1 μm, which includes a LMFP core and a carbon coating layer coated on the surface of the LMFP core. The content of the carbon coating layer is 1% based on the mass of the lithium manganese iron phosphate material. The chemical formula of the LMFP core is LiFe 0.2 Mn 0.8 PO4.
[0079] Example 4
[0080] Except for the following contents, the rest is the same as Example 1.
[0081] The positive electrode active material adopts a high-nickel ternary material and a lithium iron manganese phosphate material with a mass ratio of 4:6. The high-nickel ternary material is a single crystal material with a particle size Dv501 of 5μm. It includes an NCM core and a coating layer coated on the surface of the NCM core. Based on the mass of the high-nickel ternary material, the coating layer includes 1200ppm of Al, 2500ppm of Zr, 1000ppm of W and 600ppm of Sr. The chemical formula of the NCM core is LiNi 0.85 Co 0.1 Mn 0.15 O2; the particle size Dv502 of the lithium manganese iron phosphate material is 1.5 μm, which includes a LMFP core and a carbon coating layer coated on the surface of the LMFP core. The content of the carbon coating layer is 3% based on the mass of the lithium manganese iron phosphate material. The chemical formula of the LMFP core is LiFe 0.4 Mn 0.6 PO4.
[0082] Example 5
[0083] Except for the following contents, the rest is the same as Example 1.
[0084] Based on the mass of the high nickel ternary material, the coating layer includes 1500 ppm of Al, 2500 ppm of Zr, 1000 ppm of W and 700 ppm of Sr.
[0085] Example 6
[0086] Except for the following contents, the rest is the same as Example 1.
[0087] Based on the mass of the high nickel ternary material, the coating layer includes 800 ppm of Al, 3800 ppm of Zr, 700 ppm of W and 1000 ppm of Sr.
[0088] Example 7
[0089] Except for the following contents, the rest is the same as Example 1.
[0090] The coating layer includes 1100 ppm of Al, 3120 ppm of Zr, and 850 ppm of W based on the mass of the high nickel ternary material.
[0091] Example 8
[0092] Except for the following contents, the rest is the same as Example 1.
[0093] The positive electrode active material only uses high-nickel ternary material, and its coating layer includes 900 ppm of W, 2859 ppm of Zr and 720 ppm of Sr based on the mass of the high-nickel ternary material.
[0094] Example 9
[0095] Except for the following contents, the rest is the same as Example 1.
[0096] The positive electrode active material only uses high-nickel ternary material, and its coating layer includes 920 ppm of W and 3400 ppm of Zr based on the mass of the high-nickel ternary material.
[0097] Example 10
[0098] Except for the following contents, the rest is the same as Example 1.
[0099] The positive electrode active material only uses high-nickel ternary material, and its coating layer includes 1120 ppm of Al and 980 ppm of Sr based on the mass of the high-nickel ternary material.
[0100] Embodiment 11
[0101] Except for the following contents, the rest is the same as Example 1.
[0102] The positive electrode active material only uses high-nickel ternary materials.
[0103] Example 12
[0104] Except for the following contents, the rest is the same as Example 1.
[0105] The positive electrode active material only uses high-nickel ternary material, and no insulating layer is coated on the aluminum foil.
[0106] The XRD spectrum of the positive electrode sheet prepared in this embodiment is shown in Figure 2 .
[0107] Embodiment 13
[0108] Except for the following contents, the rest is the same as Example 1.
[0109] The aluminum foil is not coated with an insulating layer.
[0110] Embodiment 14
[0111] Except for the following contents, the rest is the same as Example 1.
[0112] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 60%; the prepared positive electrode slurry is evenly coated on the two sides of the aluminum foil (thickness 12μm), and the coated slurry is baked to obtain an active paste layer with a thickness of 50μm on both sides, and then an insulating layer is coated on the empty foil position at the tail of the active paste layer on the aluminum foil. The specific operation is: inorganic particulate silicon dioxide (Dv503=0.6μm and Dv99=2.5μm) and adhesive PVDF are mixed in a mass ratio of 85:15 and added to NMP and stirred evenly to form a slurry with a solid content of 50%, and then the slurry is evenly coated on the empty foil at the tail of the active paste layer. After drying, an insulating layer connected to but not overlapping with the paste layer is obtained, and the thickness is 10μm. Finally, rolling, slitting and sheeting are performed to obtain the positive electrode sheet to be wound.
[0113] Embodiment 15
[0114] Except for the following contents, the rest is the same as Example 1.
[0115] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 50%; the prepared positive electrode slurry is evenly coated on the two sides of the aluminum foil (thickness 8μm), and the coated slurry is baked to obtain an active paste layer with a thickness of 30μm on both sides, and then an insulating layer is coated on the empty foil position at the tail of the active paste layer on the aluminum foil. The specific operation is: inorganic particulate alumina (Dv503=0.8μm and Dv99=4μm) and adhesive PVDF are mixed in a mass ratio of 88:12 and added to the NMP solution and stirred evenly to form a slurry with a solid content of 45%, and then the slurry is evenly coated on the empty foil at the tail of the active paste layer. After drying, an insulating layer connected to but not overlapping with the paste layer is obtained, and the thickness is 10μm. Finally, rolling, slitting and sheeting are performed to obtain the positive electrode sheet to be wound.
[0116] Example 16
[0117] Except for the following contents, the rest is the same as Example 1.
[0118] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 40%; the prepared positive electrode slurry is evenly coated on the two sides of the aluminum foil (thickness 16μm), the coated slurry is baked to obtain an active paste layer with a thickness of 60μm on both sides, and then an insulating layer is coated on the empty foil position at the tail of the active paste layer on the aluminum foil. The specific operation is: inorganic particulate titanium dioxide (Dv503=1μm and Dv99=3μm) and adhesive PVDF are mixed in a mass ratio of 90:10 and added to the NMP solution and stirred evenly to form a slurry with a solid content of 45%, and then the slurry is evenly coated on the empty foil at the tail of the active paste layer. After drying, an insulating layer connected to but not overlapping with the paste layer is obtained, and the thickness is 10μm. Finally, rolling, slitting and sheeting are performed to obtain the positive electrode sheet to be wound.
[0119] Embodiment 17
[0120] Except for the following contents, the rest is the same as Example 1.
[0121] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 60%; the thickness of the aluminum foil is 8μm, the thickness of the active paste layer is 25μm, and the thickness of the insulating layer is 1μm.
[0122] Embodiment 18
[0123] Except for the following contents, the rest is the same as Example 1.
[0124] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 30%; the thickness of the aluminum foil is 16 μm, the thickness of the active paste layer is 100 μm, and the thickness of the insulating layer is 5 μm.
[0125] Embodiment 19
[0126] Except for the following contents, the rest is the same as Example 1.
[0127] The mass proportion of lithium manganese iron phosphate material in the positive electrode active material is 60%; the prepared positive electrode slurry is evenly coated on the two sides of the aluminum foil (thickness 8μm), and the coated slurry is baked to obtain an active paste layer with a thickness of 10μm on both sides, and then an insulating layer is coated on the empty foil position at the tail of the active paste layer on the aluminum foil. The specific operation is: inorganic particulate calcium oxide (Dv503=1μm and Dv99=6μm) and adhesive PVDF are mixed in a mass ratio of 86:14 and added to the NMP solution and stirred evenly to form a slurry with a solid content of 45%, and then the slurry is evenly coated on the empty foil at the tail of the active paste layer. After drying, an insulating layer connected to but not overlapping with the paste layer is obtained, and the thickness is 3μm. Finally, rolling, slitting and sheeting are performed to obtain the positive electrode sheet to be wound.
[0128] Example 1-A
[0129] Except for the following contents, the rest is the same as Example 1.
[0130] The coating layer includes 800 ppm of Al, 3500 ppm of Zr, 700 ppm of W and 1000 ppm of Sr based on the mass of the high nickel ternary material.
[0131] Example 1-B
[0132] Except for the following contents, the rest is the same as Example 1.
[0133] The coating layer includes 1000 ppm of Al, 2827 ppm of Zr, 950 ppm of W and 700 ppm of Sr based on the mass of the high nickel ternary material.
[0134] Example 1-C
[0135] Except for the following contents, the rest is the same as Example 1.
[0136] The coating layer includes 1200 ppm of Al, 2500 ppm of Zr, 1000 ppm of W and 600 ppm of Sr based on the mass of the high nickel ternary material.
[0137] Example 1-D
[0138] Except for the following contents, the rest is the same as Example 1.
[0139] The positive electrode active material is a high-nickel ternary material and lithium manganese iron phosphate material with a mass ratio of 6:4.
[0140] Example 1-E
[0141] Except for the following contents, the rest is the same as Example 1.
[0142] The positive electrode active material is a high-nickel ternary material and lithium manganese iron phosphate material in a mass ratio of 5:5.
[0143] Example 1-F
[0144] Except for the following contents, the rest is the same as Example 1.
[0145] The positive electrode active material is a high-nickel ternary material and lithium manganese iron phosphate material with a mass ratio of 4:6.
[0146] Example 1-G
[0147] Except for the following contents, the rest is the same as Example 1.
[0148] The thickness of the positive electrode active paste layer is 70 μm, the thickness of the aluminum foil is 10 μm, and the thickness of the insulating layer is 5.3 μm.
[0149] Example 1-H
[0150] Except for the following contents, the rest is the same as Example 1.
[0151] The thickness of the positive electrode active paste layer is 30 μm, the thickness of the aluminum foil is 8 μm, and the thickness of the insulating layer is 1 μm.
[0152] Embodiment 1-I
[0153] Except for the following contents, the rest is the same as Example 1.
[0154] The particle size of aluminum oxide in the insulating layer satisfies: Dv503=0.8 μm and Dv99=2.4 μm.
[0155] Example 1-J
[0156] Except for the following contents, the rest is the same as Example 1.
[0157] The particle size of aluminum oxide in the insulating layer satisfies: Dv503=0.8 μm and Dv99=4.0 μm.
[0158] Comparative Example 1
[0159] Except for the following contents, the rest is the same as Example 8.
[0160] Based on the mass of the high nickel ternary material, the coating layer includes 1000 ppm of Al2O3 and 800 ppm of SrO.
[0161] Comparative Example 2
[0162] Except for the following contents, the rest is the same as Example 8.
[0163] Based on the mass of the high nickel ternary material, the coating layer includes 150 ppm of Al2O3 and 1000 ppm of SrO.
[0164] Test Case
[0165] 1. Coating content test
[0166] The high-nickel ternary material is placed in a mixed solution of hydrochloric acid and nitric acid for 4 hours to ensure that both the coating and the matrix material can be dissolved, and the pretreated solution is introduced into the ICP mass spectrometer. ICP ionizes the atoms or ions in the solution through high temperature, and uses a mass spectrometer to analyze the mass-to-charge ratio of these ions to determine the content of specific elements in the sample. In ICP analysis, the detection parameters are set according to the specific elements contained in the coating (such as doping elements, coating materials, etc.), and the concentration of these elements is measured. Based on the results of the ICP measurement, combined with the sample pretreatment steps, the true content of the elements contained in the coating in the original sample is calculated.
[0167] The test method for the coating content in lithium manganese iron phosphate material is the same as above.
[0168] 2. Particle size test
[0169] Select ultrapure water as the dispersion medium, add 1g of ternary cathode material sample to 1L of dispersion medium, and ultrasonicate for 60 minutes to fully disperse the sample to form a uniform suspension or dispersion. Pour the prepared sample suspension or dispersion into the sample pool, turn on the laser particle size analyzer for testing, and after the test is completed, the computer will generate a particle size distribution diagram and related data report.
[0170] The particle size testing method for lithium manganese iron phosphate material and inorganic particles is the same as above.
[0171] 3. DSC thermal decomposition temperature and thermal decomposition enthalpy test
[0172] Before the test, it is necessary to prepare the DSC instrument and ensure that it is in good working condition. At the same time, prepare a dry and pure positive electrode sample. The positive electrode sample is charged to 4.2V at 0.5C constant current and constant voltage, and cut off at 0.05C, and then dissected.
[0173] During the test, place the sample in the DSC instrument, set the heating rate to 5℃ / min, the heating range to 25℃-350℃, the N2 protective atmosphere, and then start the test program. As the temperature rises, the DSC instrument will record the difference in heat flow rate between the sample and the reference, and draw a DSC curve. By analyzing the DSC curve, the starting temperature, peak temperature, and end temperature of the thermal decomposition of the sample can be determined. These temperatures represent the temperature at which the sample starts to thermally decompose, the thermal decomposition rate is the maximum, and the thermal decomposition ends, respectively. In addition, the peak area of the DSC curve can also be used to calculate the thermal decomposition enthalpy of the sample, that is, the heat released by the sample during the thermal decomposition process.
[0174] 4. Coating thickness test
[0175] The electrode after coating and drying is measured with a micrometer, and 10 positions are randomly selected on the electrode for testing. The average of the 10 data after the test is the thickness H0 of the electrode. The thickness H2 of the current collector before coating is measured with a micrometer according to the above method. The thickness of the coating H = H0-H2.
[0176] 5. Peel force test
[0177] Test equipment: tensile testing machine. Cut the rolled positive electrode into 25mm width, prepare a flat thin steel plate, and stick a double-sided tape on its center, stick the electrode on the double-sided tape, and make sure that the electrode and the tape are completely matched and fit to avoid test errors. Insert the steel plate with the fixed electrode into the lower clamp of the tensile testing machine and fix it vertically. Clamp the un-adhesive electrode on the upper clamp and fix it at 90° with the electrode of the lower clamp. Set the test width, peeling length and peeling speed parameters on the tensile testing machine. Start the test program, and the tensile testing machine will apply tensile force according to the set parameters and record the force value changes during the peeling process. After the test, data such as the peel strength curve and average value will be obtained.
[0178] 6. Test of battery capacity, thickness and energy density
[0179] The prepared finished battery was charged to full charge at constant current and constant voltage at 25°C, and then discharged to 3.0V at 0.5C, and the discharged capacity was recorded as the battery capacity;
[0180] The finished battery was charged to 30% SOC at 25°C, and the battery thickness was tested using 600g PPG.
[0181] Calculate volume energy density = battery capacity * platform voltage / battery length / width / thickness.
[0182] 7. Cycle test
[0183] The prepared finished battery was subjected to 2C / 4C charge and discharge cycles at 25°C, and the battery capacity retention rate and expansion rate were confirmed after 800 cycles.
[0184] 8. Overcharge test
[0185] The finished battery is subjected to 2C-5V overcharge and 2C-6V tests. The test method is as follows: at 25°C, the raw material battery is charged to 5V or 6V at a constant current and constant voltage of 2C, and maintained at 5V or 6V for 7 hours. The battery is considered to have passed if it does not catch fire or explode.
[0186] 9. Acupuncture test
[0187] The finished batteries are subjected to different systems of needle penetration tests. The test method is: after the battery is fully charged, needles of different diameters (2.5mm, 4mm) are used to completely penetrate the battery at a speed of 30mm / s. The battery is considered to have passed if it does not catch fire or explode.
[0188] 10. Hot box test
[0189] The finished battery was subjected to hot box tests at different temperatures (130°C, 135°C, 140°C). The test method is as follows: after the battery is fully charged, it is placed on the hot box test equipment, and the hot box is heated at a rate of 5°C / min. After heating to the corresponding temperature, it is maintained for 60 minutes, and then the hot box temperature is lowered. The battery is considered to have passed the test if it does not catch fire or explode.
[0190] The test results are shown in Tables 1 to 5. In Table 1, " / " indicates absence.
[0191] Table 1
[0192]
[0193]
[0194] Table 2
[0195]
[0196]
[0197] Table 3
[0198]
[0199]
[0200] Table 4
[0201]
[0202]
[0203] Table 5
[0204]
[0205]
[0206]
[0207] As can be seen from Table 1, compared with the DSC thermal decomposition temperature T1 of the pure ternary positive electrode sheet (i.e., the first positive electrode sheet), the DSC thermal decomposition temperature T2 of the mixed positive electrode sheet (i.e., the second positive electrode sheet) mixed with lithium iron manganese phosphate material is increased by more than 4°C, indicating that the mixed positive electrode material mixed with lithium iron manganese phosphate material has higher thermal stability. In addition, compared with the DSC thermal decomposition enthalpy Q1 of the pure ternary positive electrode sheet (i.e., the first positive electrode sheet), the DSC thermal decomposition enthalpy Q2 of the mixed positive electrode sheet (i.e., the second positive electrode sheet) mixed with lithium iron manganese phosphate material is significantly reduced, and Q2 / Q1 is less than 0.65, which indicates that the mixed positive electrode sheet mixed with lithium iron manganese phosphate material has higher thermal stability. Except for Example 19, the particle size of the inorganic particles in the insulating layer of other embodiments all satisfies Dv99 / Dv503=3-5, thereby improving the bonding force between the insulating layer and the current collector, and ensuring that the peeling force N of the insulating layer on the current collector is above 0.3kgf.
[0208] As can be seen from Table 2, the capacity, battery thickness, and volume energy density of Examples 1 to 7, 13, and 1-A to 1-J are roughly equivalent to those of Examples 8 to 12, indicating that the mixing of lithium manganese iron phosphate will not affect the capacity, battery thickness, and energy density of the battery. To ensure that the battery capacity is equivalent to that of Example 1, the batteries of Examples 14 to 17 and 19 are thicker than those of Example 1, so the energy density of the batteries is lower, while the positive electrode active paste layer of Example 18 is thicker, and the battery under the same capacity conditions is thinner, so the energy density is higher.
[0209] As can be seen from Table 3, compared with Examples 8-12, the cycle performance of Examples 1-7, Example 13, and Examples 1-A to 1-J is improved, indicating that the structural stability of the positive electrode material can be improved after the lithium manganese iron phosphate is mixed, thereby improving the cycle performance of the battery. The cycle performance of Examples 14-17 is equivalent to that of Example 1, the cycle performance of Example 18 is relatively poor, and the cycle performance of Example 19 is relatively good, indicating that the thickness of the active paste layer has an effect on the cycle performance of the battery. The thicker the active paste layer, the worse the cycle performance. The cycle performance of Comparative Example 1 is worse than that of Example 8, indicating that the coating element is not enough, resulting in poor structural stability of the material, thereby causing the cycle performance to deteriorate. The cycle performance of Comparative Example 2 is better than that of Example 8, indicating that the Sr element coating makes the positive electrode material structurally stable and has better cycle performance.
[0210] As can be seen from Table 4, Examples 1 to 7 and Examples 1-A to 1-J can all pass the test under 2C-5V overcharge and 2C-6V overcharge conditions, while Examples 8-12 all fail, indicating that the presence of lithium iron manganese phosphate can significantly improve the overcharge performance of the battery. This is because lithium iron manganese phosphate has high thermal stability that can ensure that the mixed positive electrode material will not be destroyed, thus avoiding thermal runaway. Examples 13-19 can also pass the test under 2C-5V overcharge and 2C-6V overcharge conditions, which indicates that the lithium iron manganese phosphate content is in the range of 30%-60%, which can make the battery's overcharge thermal stability performance meet the requirements and ensure that the structure will not be damaged during overcharge. However, Comparative Examples 1-2 cannot pass the above overcharge test, which indicates that the thermal stability of the simple ternary material is not enough and it quickly generates heat and decomposes during overcharge.
[0211] Examples 1-7 and 1-A to 1-J can pass the 2.5 mm and 4 mm puncture tests, while Example 13 can only pass with probability, indicating that the presence of the insulating layer at the end of the aluminum foil can effectively avoid the contact between the aluminum foil and the negative electrode, thereby improving the puncture pass rate; Examples 8-10 and 12 cannot pass the above-mentioned puncture test, Example 11 passes with probability and the passing probability is significantly lower than that of Example 13, indicating that the lithium manganese iron phosphate particles in the positive electrode active material can effectively wrap the cross-section of the aluminum foil when puncture occurs. Since lithium manganese iron phosphate has high thermal stability and low conductivity, it can avoid contact between the cross-section of the aluminum foil and the negative electrode, thereby avoiding battery failure due to heat accumulation. Examples 15, 16 and 18 can also pass the 2.5 mm and 4 mm puncture tests, while Examples 14, 17 and 19 can pass the test with a greater probability, which means that when the active paste layer is thinner, in order to ensure that the battery has a capacity comparable to that of Example 1, the battery needs to have more folds. When puncture occurs, the collector cross-section is more, and it is more likely to short-circuit the positive current collector and the negative electrode sheet, resulting in thermal runaway of the battery.
[0212] As shown in Table 5, Examples 1 to 7, 1-A to 1-J, and 13-19 can all pass the 130°C, 135°C, and 140°C hot box tests, and Examples 8-12 are likely to pass the 135°C and 140°C hot box tests, which indicates that the presence of lithium manganese iron phosphate in the mixed positive electrode material can effectively improve the thermal stability of the positive electrode sheet, thereby improving the safety performance of the battery. Comparative Examples 1-2 are likely to pass the above hot box test, indicating that the coating elements of the ternary material have a certain influence on the thermal stability of the material, and when the Al element content is higher, the thermal stability is better.
[0213] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A ternary positive electrode material, comprising a NCM core and a coating layer covering at least a portion of the surface of the NCM core; characterized in that: The coating layer includes a metal element M1 and a metal element M2, wherein the metal element M1 is Al and / or W, and the metal element M2 is Sr and / or Zr; Based on the mass of the ternary positive electrode material, the content of the metal element M1 is W1, the content of the metal element M2 is W2, and 0.2≤W1 / W2≤1.
2.
2. The ternary positive electrode material according to claim 1, characterized in that: The coating layer includes metal elements Al, Zr, W and Sr, and the content of Al is W 1a 、Zr content W 2a 、W content 1b and Sr content W 2b Satisfy: 0.16 ≤ W 1a *W 1b / (W 2a *W 2b )≤0.8; Optionally, 800ppm≤W 1a ≤1200ppm; Optionally, 2500ppm≤W 2a ≤3500ppm; Optionally, 700ppm≤W 1b ≤1000ppm; Optionally, 600ppm≤W 2b ≤1000ppm.
3. The ternary positive electrode material according to claim 1 or 2, characterized in that: The chemical formula of the NCM core is LiNi x Co y Mn z O2, where x+y+z=1, 0.8≤x<1, 0 <y<0.2,0<z<0.2; And / or, the ternary cathode material is a single crystal material, and its particle size Dv501 is 2 μm-5 μm; And / or, the metal element is selected from the group consisting of Al2O3, ZrO2, WO3 and SrO.
4. A mixed positive electrode material, characterized in that: It comprises a lithium iron manganese phosphate material and the ternary positive electrode material according to any one of claims 1 to 3, wherein the mass ratio of the ternary positive electrode material to the lithium iron manganese phosphate material is 7:3-4:
6.
5. The mixed positive electrode material according to claim 4, characterized in that: The lithium manganese iron phosphate material comprises an LMFP core and a carbon coating layer covering at least a portion of the surface of the LMFP core, and the content of the carbon coating layer is 1%-3% based on the mass of the lithium manganese iron phosphate material; And / or, the chemical formula of the LMFP core is LiFe x Mn 1-x PO4,0 <x≤0.4; And / or, the particle size Dv502 of the lithium iron manganese phosphate material is 0.5 μm-1.5 μm.
6. A positive electrode sheet, comprising a current collector and a positive electrode active material layer disposed on at least one side of the current collector, characterized in that: The positive electrode active material layer comprises the ternary positive electrode material according to any one of claims 1 to 3 or the mixed positive electrode material according to any one of claims 4 to 5.
7. The positive electrode sheet according to claim 6, characterized in that: The positive electrode sheet formed by the ternary positive electrode material according to any one of claims 1 to 3 is recorded as the first positive electrode sheet, and the positive electrode sheet formed by the mixed positive electrode material according to any one of claims 4 to 5 is recorded as the second positive electrode sheet; The DSC thermal decomposition temperature of the first positive electrode sheet is T1, T1≥206°C; the DSC thermal decomposition temperature of the second positive electrode sheet is T2, T2≥212°C; And / or, the thermal decomposition enthalpy of the first positive electrode sheet is Q1, 1200 J / g≥Q1≥800 J / g; the thermal decomposition enthalpy of the second positive electrode sheet is Q2, Q2<800 J / g.
8. The positive electrode sheet according to claim 6, characterized in that: A paste coating area and an insulating area are provided on the surface of the current collector along the length direction, the paste coating area is connected to the insulating area but does not overlap; the positive electrode active material layer is provided in the paste coating area, the positive electrode active material layer includes the mixed positive electrode material, and the insulating area is provided with an insulating layer, and the thickness H1 of the positive electrode active material layer, the thickness H2 of the current collector, the thickness H3 of the insulating layer and the mass proportion W3% of the lithium manganese iron phosphate material in the mixed positive electrode material satisfy: 4≤H1*H2*H3 / W3≤240; Optionally, H1 is 30 μm-100 μm; Optionally, H2 is 8 μm-16 μm; Optionally, H3 is 1 μm-20 μm; Optionally, W3 is 30-60.
9. The positive electrode sheet according to claim 8, characterized in that: The insulating layer comprises inorganic particles and a binder in a mass ratio of 85-91:9-15; Optionally, the particle size of the inorganic particles satisfies: Dv99 / Dv503=3-5, Dv503 is 0.6 μm-1.1 μm; Optionally, the inorganic particles include at least one of aluminum oxide, boehmite, silicon dioxide, calcium oxide, titanium dioxide, zirconium dioxide, and magnesium oxide; Optionally, a peeling force N of the insulating layer on the current collector is ≥ 0.3 kgf.
10. A battery, characterized in that: A positive electrode sheet comprising any one of claims 6 to 9.
Citation Information
Cited By
Battery cell and electric device
WO2026214207A1