High-specific-energy silicon-carbon negative electrode material as well as preparation method and application thereof
By depositing silicon nanolayers and artificial interface layers on the surface of carbon core materials, the problems of volume expansion and interface instability of silicon-based anode materials are solved, the cycle life and Coulomb efficiency of silicon-carbon anode materials are improved, and the performance of lithium batteries is improved.
Patent Information
- Application Number
- CN202411445760.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-16
AI Technical Summary
Silicon-based negative electrode materials have huge volume expansion problems during charging and discharging, resulting in reduced mechanical stability, unstable interface and attenuation of battery performance. The existing technology is difficult to effectively solve these problems.
The physical vapor deposition method is used to deposit uniformly and dense silicon nanolayers on the surface of the carbon core material, and an artificial interface layer is deposited on the surface of the silicon nanolayer. The closely connected silicon carbon material is prepared by magnetron sputtering technology. The designed artificial interface layer material is LiF and Li3N, stabilize the interface of silicon-carbon negative electrode, buffer volume changes and improve conductivity.
The cycle life and Coulomb efficiency of silicon-carbon negative electrode materials are improved, and the irreversible capacity decline is prevented, which improves the energy density and cycle stability of lithium batteries.
Smart Images

Figure CN119069684A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage materials and lithium battery negative electrode materials, and specifically relates to a high specific energy silicon-carbon negative electrode material and a preparation method and use thereof. Background Art
[0002] With the growing demand for improving battery energy density, the performance iteration of negative electrode materials has become the focus of industry research. At present, carbon-based materials represented by artificial graphite are the main materials used for negative electrodes of lithium-ion batteries. Graphite negative electrodes dominate the market with their mature technology and stable performance. With the advancement of science and technology and the increase in application needs, silicon-based negative electrodes have gradually come into people's view due to their potential high energy density advantages. However, silicon-based negative electrodes face many challenges in the process of commercialization, the most prominent of which is the problem of volume expansion.
[0003] The huge volume expansion of silicon negative electrode materials during the charging and discharging process is one of the main obstacles to its commercial application. During the lithiation process, the volume expansion rate of silicon is as high as 380%, which causes a sharp drop in the mechanical stability of silicon particles and electrode plates, and the contact between active particles becomes poor, which in turn affects the overall performance of the battery. In addition, the volume expansion will also cause the stability of the SEI film to decrease, which seriously challenges the life and safety performance of lithium batteries.
[0004] The existing technology mainly uses porous carbon as a carrier to prepare silicon-carbon negative electrode materials, embeds silicon nanoparticles into the pore structure of porous carbon, and uses the high conductivity and good mechanical stability of carbon materials to overcome the volume expansion of silicon. However, the porous carbon structure can provide limited space for silicon particles, and silicon particles are prone to agglomeration and shedding during the charging and discharging process. In addition, the above-mentioned existing technology may also have the problem of uneven distribution of silicon particles in the carbon matrix, which in turn affects the overall performance of the negative electrode material. In addition, due to the volume expansion and contraction of silicon, the silicon-carbon interface is easily destroyed and reconstructed, resulting in an increase in interface resistance and a decrease in battery performance. Summary of the invention
[0005] In order to solve the problems of unstable silicon-carbon bonding, uneven distribution of silicon particles and unstable interface in existing silicon-carbon negative electrode materials, the purpose of the present invention is to provide a high specific energy silicon-carbon negative electrode material and a preparation method and use thereof, which can maintain the stability of the interface film structure while alleviating the volume expansion problem of the silicon-carbon negative electrode.
[0006] To achieve the above objectives, the technical solution of the present invention is as follows.
[0007] The first aspect of the present invention provides a high specific energy silicon-carbon negative electrode material, which is obtained by sequentially depositing a silicon nanolayer and an artificial interface layer on the surface of a carbon core material using a physical vapor deposition method; the material of the artificial interface layer is at least one of LiF and Li3N; the thickness of the silicon nanolayer is 10nm to 800nm; the thickness of the artificial interface layer is 10nm to 50nm.
[0008] The present invention uses a physical vapor deposition method to deposit a uniform and dense silicon nanolayer of a certain thickness on the surface of the carbon core material, and then deposits an artificial interface layer on the surface of the silicon nanolayer to stabilize the silicon-carbon negative electrode interface. Among them, a complementary relationship is formed between the silicon nanolayer and the carbon core material. In the silicon-carbon negative electrode material, the silicon nanolayer acts as an active substance to provide lithium storage capacity; and the deposited silicon nanolayer is tightly combined with the carbon core material, which can not only buffer the structural collapse and failure of the electrode caused by the volume change of the silicon negative electrode during the charge and discharge process, but also improve the conductivity of the silicon-based material, and avoid the agglomeration of silicon-carbon particles during the charge and discharge cycle. This structural design improves the cycle life and coulomb efficiency of the silicon-carbon negative electrode material, while also preventing it from producing irreversible capacity decay, and solves the problems of unstable silicon-carbon bonding, uneven distribution of silicon particles, and unstable interface in the existing silicon-carbon negative electrode material.
[0009] In a preferred embodiment, the carbon core material is any one of natural graphite material, artificial graphite material, mesophase carbon microbeads, amorphous porous carbon, biomass carbon, and graphene.
[0010] The second aspect of the present invention provides a method for preparing the high specific energy silicon-carbon negative electrode material according to the first aspect, comprising the following steps:
[0011] A silicon nanolayer is uniformly deposited on the surface of the carbon core material by a physical vapor deposition method, and then an artificial interface layer is further deposited on the surface of the silicon nanolayer to prepare a high specific energy silicon-carbon negative electrode material.
[0012] In a preferred embodiment, before uniformly depositing the silicon nanolayer on the surface of the carbon core material, the carbon core material is further subjected to ball milling to perform surface treatment on the carbon core material to promote uniform deposition of the silicon nanolayer on the surface of the carbon core material.
[0013] In order to uniformly deposit a dense silicon nanolayer on the surface of the carbon core material, the carbon core material needs to be ball-milled before magnetron sputtering. The purpose of ball milling is to perform surface treatment and morphological optimization on the carbon core material. The carbon core material particles can be refined by ball milling, and its surface roughness can be improved. The adhesion and uniformity of the silicon target during magnetron sputtering can be increased, which helps to form a denser and more uniform silicon nanolayer. New surface defects or active sites may also be added during the ball milling process, which enhances the bonding force between the silicon target and the carbon core material, thereby helping to improve the stability and durability of the silicon nanolayer. Preferably, the ball milling modification is to place the carbon core material and the solvent in a ball milling device for ball milling, and dry to remove the solvent. The ball-to-material ratio of ball milling modification is 10:1, the ball milling speed is 300rpm~400rpm, and the ball milling time is 1h~3h.
[0014] In a preferred embodiment, the physical vapor deposition method is a magnetron sputtering method; the sputtering target material for depositing the silicon nanolayer is a silicon target material, and the sputtering target material for depositing the artificial interface layer is a LiF target material and / or a Li3N target material.
[0015] In a preferred embodiment, physical vapor deposition is performed in a radio frequency magnetron sputtering chamber, wherein a rotating sample stage is rotatably arranged in the radio frequency magnetron sputtering chamber, and is configured to place the carbon core material on the rotating sample stage; a stirring mechanism is rotatably arranged on the rotating sample stage, and is configured to uniformly deposit a silicon nanolayer and an artificial interface layer on the surface of the powder particles of the carbon core material during the radio frequency magnetron sputtering process. The present invention promotes uniform deposition of the silicon nanolayer and the artificial interface layer on the surface of the powder particles during the magnetron sputtering coating process by designing a vibrating stirring mechanism.
[0016] In a preferred embodiment, the process parameters for depositing the silicon nanolayer or the artificial interface layer are: the background vacuum is 0.1×10 -4 Pa~9.9×10 -4 Pa, the working gas pressure is 0.35Pa~0.55Pa, the purity of silicon target, LiF target and Li3N target is ≥99.99%; the target distance is 10cm~50cm, the sputtering temperature is 20℃~30℃, and the sputtering time is 1min~10min.
[0017] The method of the present invention sputters a uniform silicon nanolayer and an artificial interface layer capable of optimizing lithium ion transmission performance on the surface of a carbon core material through a radio frequency magnetron sputtering process, and strictly controls the process parameters of the sputtering process to make the structure and composition of the deposited silicon nanolayer and the artificial interface layer uniform.
[0018] The third aspect of the present invention provides a use of the high specific energy silicon-carbon negative electrode material described in the first aspect in preparing a silicon-carbon negative electrode for assembling a lithium battery.
[0019] In a preferred embodiment, the silicon-carbon negative electrode is obtained by dispersing the high specific energy silicon-carbon negative electrode material described in the first aspect with a conductive additive and a polymer binder in water, then coating the mixture on a metal substrate and drying the mixture;
[0020] The mass ratio of high specific energy silicon-carbon negative electrode material to conductive additive and polymer binder is 90:4:15;
[0021] The polymer adhesive is a mixture of polyacrylic acid and polyvinyl alcohol, and the mass ratio of polyacrylic acid to polyvinyl alcohol is 95:5-50:50.
[0022] In a preferred embodiment, the lithium battery is a soft-pack lithium battery or a half-cell.
[0023] In a preferred embodiment, the soft-pack lithium battery includes a silicon-carbon negative electrode, a diaphragm, a positive electrode and an aluminum-plastic film bag, the aluminum-plastic film bag is punched into a battery shape, the silicon-carbon negative electrode, the diaphragm, and the positive electrode are placed in the aluminum-plastic film bag in sequence, and an electrolyte is dripped into the aluminum-plastic film bag to assemble a soft-pack full battery; the silicon-carbon negative electrode is prepared from the silicon-carbon negative electrode material described in the first aspect.
[0024] In a preferred embodiment, the half-cell is formed by placing the silicon-carbon electrode, the separator, and the positive electrode in a standard CR2032 button-type battery shell in sequence, dripping the electrolyte, and assembling the half-cell.
[0025] In a preferred embodiment, the membrane is a Celgard membrane.
[0026] In a preferred embodiment, the positive electrode is obtained by dispersing NCM811, conductive additives and polyvinylidene fluoride in N-methylpyrrolidone, then coating the mixture on a metal substrate and drying the mixture; the mass ratio of NCM811, conductive additives and polyvinylidene fluoride is 95:5:5.
[0027] In a preferred embodiment, the conductive additive is conductive carbon black super-P; and the metal substrate is copper foil or aluminum foil.
[0028] In a preferred embodiment, the electrolyte is prepared by mixing dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate in an equal volume ratio, and then adding lithium hexafluorophosphate to prepare a basic electrolyte; and adding a negative electrode film-forming agent to the basic electrolyte to obtain the electrolyte.
[0029] In a preferred embodiment, the concentration of lithium hexafluorophosphate in the basic electrolyte is 1 mol / L; the negative electrode film-forming agent is fluoroethylene carbonate, and the mass percentage of the negative electrode film-forming agent in the electrolyte is 1% to 10%.
[0030] In a preferred embodiment, the preparation process of the silicon-carbon negative electrode or positive electrode further includes vacuum stirring for 2h to 3h before coating on the metal substrate; the drying temperature is 95°C to 100°C, and the drying time is 10h to 16h.
[0031] Beneficial effects of the present invention:
[0032] 1. The present invention deposits a uniform and dense silicon nanolayer on the surface of the carbon core material by a physical vapor deposition method, so that a complementary relationship is formed between the silicon nanolayer and the carbon core material, which can not only buffer the electrode structural collapse failure caused by the volume change of the silicon negative electrode during the charge and discharge process, but also improve the conductivity of the designed silicon-carbon negative electrode material; then an artificial interface layer is deposited on the surface of the silicon nanolayer to stabilize the silicon-carbon negative electrode interface, inhibit interface side reactions, maintain the stability of the interface film structure, and solve the problems of unstable silicon-carbon bonding, uneven distribution of silicon particles and unstable interface in existing silicon-carbon negative electrode materials.
[0033] 2. The present invention combines the advantages of the close connection between silicon-carbon materials prepared by magnetron sputtering technology and the designed artificial interface layer, thereby improving the cycle life and Coulomb efficiency of silicon-carbon negative electrode materials and preventing irreversible capacity decay.
[0034] 3. The silicon-carbon negative electrode material prepared by the present invention can be used to prepare a silicon-carbon negative electrode and assembled to form a lithium battery. The assembled lithium battery has excellent coulombic efficiency and cycle life. The coulombic efficiency of the first week of charge and discharge is above 85%, and the capacity retention rate is above 80%. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a test chart of the cycle stability of the NCM811 soft-pack full battery assembled with the LiF-Li3N / Si-NGr silicon-carbon negative electrode material of Example 1 at a rate of 0.2C.
[0036] Figure 2 This is a test chart of the cycle stability of the NCM811 soft-pack full battery assembled with the LiF-Li3N / Si-AGr silicon-carbon negative electrode material of Example 2 at a rate of 0.2C. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0038] Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without making any creative work shall fall within the scope of protection of the present invention.
[0039] With the advancement of science and technology and the increase in application needs, silicon-based negative electrodes have gradually entered people's field of vision due to their potential high energy density advantages. However, silicon-based negative electrodes face many challenges in the process of commercialization, among which the most prominent are volume expansion, poor conductivity, and unstable SEI membrane. The full English name of SEI membrane is Solid Electrolyte Interface, and its Chinese name is Solid Electrolyte Interface Membrane.
[0040] The huge volume expansion of silicon negative electrode materials during the charging and discharging process is one of the main obstacles to its commercial application. In order to overcome the volume expansion problem of silicon negative electrodes, the existing technology mainly deposits silicon layers or carbon layers in the gaps of silicon carbide, and uses carbon layers to wrap silicon layers. However, these technologies still face some challenges and defects, especially when the loading amount is high or the thickness of the silicon nanolayer exceeds a certain limit. For example, when the loading amount of silicon is too high, the volume change of silicon particles during the charging and discharging process will be more dramatic, resulting in a decrease in the structural stability between the silicon layer and the silicon carbide or carbon coating layer. This structural instability may lead to the pulverization and shedding of silicon particles and the rupture of the SEI film, thereby reducing the cycle life and safety of the battery. When the thickness of the silicon nanolayer exceeds 5nm, the expansion rate of the particles in the fully charged state will increase significantly and decay rapidly during the cycle. This is mainly because thicker silicon nanolayers are more prone to volume expansion and stress accumulation during the lithiation process, resulting in structural damage and performance degradation.
[0041] In addition, the low first charge efficiency of silicon negative electrode is also an important factor restricting its commercial application. During the first charge process of lithium-ion batteries, the electrolyte will undergo reduction decomposition on the surface of the silicon negative electrode to form a solid electrolyte phase interface film. This process irreversibly consumes a large amount of lithium ions from the positive electrode, resulting in a low coulombic efficiency of the first cycle, which in turn reduces the capacity and energy density of lithium-ion batteries. Since the surface area of silicon material is much higher than that of graphite, its first irreversible lithium loss is as high as 15% to 35%, which undoubtedly increases the difficulty of commercializing silicon negative electrodes.
[0042] Although the carbon coating in the existing technology can alleviate the volume expansion of silicon, it may also introduce new problems. For example, the thickness and uniformity of the carbon layer are difficult to accurately control, which may cause fluctuations in battery performance. At the same time, although the conductivity of the carbon layer is better than that of silicon, there is still room for improvement, especially in the application of high energy density batteries.
[0043] In summary, the existing technology has made some progress in solving the problem of silicon anode volume expansion, but it still faces challenges when the loading amount is high or the thickness of the silicon nanolayer is large. Therefore, it is necessary to further research and develop new silicon-based anode materials and their preparation technologies to improve their structural stability and cycle performance, and promote the commercial application of silicon-based anodes in the field of high-performance batteries.
[0044] The present invention uses magnetron sputtering technology to uniformly deposit a silicon nanolayer on the surface of the carbon core material, and constructs an artificial interface layer on the surface of the silicon nanolayer, and the material of the artificial interface layer is LiF and / or Li3N. Among them, the silicon nanolayer and the carbon core material have a stable structure, strong bonding force, and close connection; and due to the properties of the two-dimensional material, the volume change of the deposited silicon nanolayer during the cycle can be effectively alleviated. The artificial interface layer constructed on the surface of the silicon nanolayer can avoid the occurrence of side reactions between the prepared silicon-carbon negative electrode material and the electrolyte during the cycle, and maintain the stability of the interface film structure. Combining the advantages of the close connection between the silicon-carbon materials prepared by magnetron sputtering technology and the designed artificial interface layer, the cycle life and coulomb efficiency of the silicon-carbon negative electrode material are improved, and at the same time, it is also prevented from producing irreversible capacity decay.
[0045] Preparation of high specific energy silicon-carbon negative electrode half-cell: The prepared silicon-carbon negative electrode material, the designed polymer adhesive and the conductive super-P carbon are coated on a metal substrate in a certain proportion to prepare a silicon-carbon negative electrode, and then punched into an electrode with a diameter of 12 mm. The electrode, Celgard separator and metal lithium positive electrode are placed in a standard CR2032 button battery shell, and the electrolyte is dripped to assemble the half-cell.
[0046] High-energy-density silicon-carbon negative electrode full battery: The prepared silicon-carbon negative electrode material, the designed polymer adhesive and the conductive super-P carbon are coated on a metal substrate in a certain proportion to prepare a silicon-carbon negative electrode. The silicon-carbon negative electrode, Celgard separator and metal lithium positive electrode are placed in an aluminum-plastic film bag in the shape of a battery, and the electrolyte is dripped to assemble the soft-pack full battery.
[0047] Unless otherwise specified, the methods described in the following examples are all conventional methods; the reagents and materials described are all commercially available unless otherwise specified.
[0048] In the following examples, natural graphite material is denoted as NGr; artificial graphite material is denoted as AGr; mesophase carbon microspheres are denoted as MCMB; amorphous porous carbon powder is denoted as APC; biomass carbon powder is denoted as NC; and graphene powder is denoted as G. These carbon materials are all purchased on the market. Polyvinylidene fluoride is denoted as PVDF.
[0049] In the following embodiments, super-P is small particle conductive carbon black, which is a pure black ultra-fine powder and is used as a conductive agent to perform a conductive function.
[0050] NCM811 is a positive electrode material for lithium-ion batteries. Its chemical formula is nickel, cobalt, and manganese oxides in a ratio of 8:1:1. This ratio of positive electrode materials is widely used in lithium-ion batteries, in which the nickel content is relatively high, which helps to increase the energy density of the battery. At the same time, the addition of manganese and cobalt also helps to improve the cycle life and stability of the battery.
[0051] The Celgard separator is any one of Celgard 2320, Celgard 2325 and Celgard 2400. In the following embodiments of the present invention, Celgard 2320 is used as an example for assembling batteries.
[0052] The amount of excess acetone solvent used should be sufficient to immerse the NGr.
[0053] Example 1
[0054] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0055] (1) 500 g of natural graphite carbon material NGr was mixed with an excess of acetone solvent to immerse the NGr, and then placed in a ball milling jar with a ball-to-material ratio of 10:1. The ball milling jar and the ball milling beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 400 rpm for 2 hours. After ball milling, the mixture was allowed to stand and dry in air to obtain a modified carbon core material.
[0056] (2) Place the pre-shaped carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the shaped carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0057] Open the baffle of the sample pan and start the sample pan rotation at 8 rpm.
[0058] Open the Si target and start sputtering the silicon nanolayer. The process parameters of RF magnetron sputtering are: at the background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material with silicon nanolayer deposition was obtained, which was recorded as Si-NGr.
[0059] The artificial interface layer is further deposited on the surface of the carbon material with the silicon nanolayer deposited. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at the background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25°C, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-NGr silicon-carbon negative electrode material.
[0060] The thickness of the silicon nanolayer is 300 nm and the thickness of the artificial interface layer is 25 nm.
[0061] Example 2
[0062] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0063] (1) 500 g of artificial graphite material AGr and excess acetone solvent were mixed to immerse NGr, and then placed in a ball milling jar with a ball-to-material ratio of 8:1. The ball milling jar and ball milling beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 350 rpm for 3 hours. After ball milling, the mixture was allowed to stand and dry in air to obtain a modified carbon core material.
[0064] (2) Place the modified carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the modified carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0065] The baffle of the sample tray was opened and the sample tray was turned on with a rotation speed of 9 rpm. The Si target was opened and the silicon nanolayer was first sputtered. The process parameters of the RF magnetron sputtering were: the background vacuum was 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material deposited by the silicon nanolayer was obtained, which was recorded as Si-AGr.
[0066] The artificial interface layer is further deposited on the surface of the carbon material deposited with the silicon nanolayer. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at a background vacuum of 5.0×10 -4When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25°C, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-AGr silicon-carbon negative electrode material.
[0067] The thickness of the silicon nanolayer is 580nm and the thickness of the artificial interface layer is 43nm.
[0068] Example 3
[0069] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0070] (1) 500 g of mesophase carbon microspheres MCMB and excess acetone solvent were mixed to immerse NGr, and then placed in a ball mill with a ball-to-material ratio of 8:1. The ball mill and ball mill beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 380 rpm for 2 hours. After ball milling, the mixture was allowed to stand and dry in air to obtain a modified carbon core material.
[0071] (2) Place the modified carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the modified carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0072] The baffle of the sample tray was opened and the sample tray was turned on with a rotation speed of 9 rpm. The Si target was opened and the silicon nanolayer was first sputtered. The process parameters of the RF magnetron sputtering were: the background vacuum was 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material deposited by the silicon nanolayer was obtained, which was recorded as Si-MCMB.
[0073] The artificial interface layer is further deposited on the surface of the carbon material deposited with the silicon nanolayer. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at a background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25°C, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-MCMB silicon-carbon negative electrode material.
[0074] The thickness of the silicon nanolayer is 780 nm and the thickness of the artificial interface layer is 50 nm.
[0075] Example 4
[0076] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0077] (1) 500 g of amorphous porous carbon powder APC and excess acetone solvent were mixed to immerse NGr, and then placed in a ball milling jar with a ball-to-material ratio of 8:1. The ball milling jar and ball milling beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 380 rpm for 2 hours. After ball milling, the mixture was allowed to stand and dry in air to obtain a modified carbon core material.
[0078] (2) Place the modified carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the modified carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0079] The baffle of the sample tray was opened and the sample tray was turned on with a rotation speed of 9 rpm. The Si target was opened and the silicon nanolayer was first sputtered. The process parameters of the RF magnetron sputtering were: the background vacuum was 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material deposited by the silicon nanolayer was obtained, which was recorded as Si-APC.
[0080] The artificial interface layer is further deposited on the surface of the carbon material deposited with the silicon nanolayer. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at a background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25°C, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-APC silicon-carbon negative electrode material.
[0081] The thickness of the silicon nanolayer is 800 nm and the thickness of the artificial interface layer is 50 nm.
[0082] Example 5
[0083] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0084] (1) 500 g of biomass carbon powder NC was mixed with excess acetone solvent to immerse NGr, and then placed in a ball mill with a ball-to-material ratio of 8:1. The ball mill and ball mill beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 380 rpm for 2 hours. After ball milling, the mixture was left to dry in air to obtain a modified carbon core material.
[0085] (2) Place the modified carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the modified carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0086] The baffle of the sample tray was opened and the sample tray was turned on with a rotation speed of 9 rpm. The Si target was opened and the silicon nanolayer was first sputtered. The process parameters of the RF magnetron sputtering were: the background vacuum was 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material deposited by the silicon nanolayer was obtained, which was recorded as Si-NC.
[0087] The artificial interface layer is further deposited on the surface of the carbon material deposited with the silicon nanolayer. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at a background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25℃, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-NC silicon-carbon negative electrode material.
[0088] The thickness of the silicon nanolayer is 100 nm and the thickness of the artificial interface layer is 20 nm.
[0089] Example 6
[0090] A method for preparing a high specific energy silicon-carbon negative electrode material comprises the following steps:
[0091] (1) 500 g of graphene powder G was mixed with an excess of acetone solvent to immerse NGr, and then placed in a ball mill with a ball-to-material ratio of 8:1. The ball mill and the ball milling beads were made of zirconium oxide. The mixture was ball milled in a planetary ball mill at a speed of 380 rpm for 2 hours. After ball milling, the mixture was allowed to stand and dry in air to obtain a modified carbon core material.
[0092] (2) Place the modified carbon core material on a shaking stirring plate and cover it with a baffle. Select the corresponding Si target and LiF and Li3N target according to the predetermined deposition layer composition. The purity of the target is ≥99.99%. Wash the target with acetone and dry it. Pre-sputter for 5 minutes to remove oxides and other impurities on the surface of the target to ensure that the material deposited on the modified carbon core material is pure and free of impurities during the subsequent sputtering process. Depending on the target material, it is necessary to select the preferred sputtering time, sputtering power and sputtering pressure.
[0093] The baffle of the sample tray was opened and the sample tray was turned on with a rotation speed of 9 rpm. The Si target was opened and the silicon nanolayer was first sputtered. The process parameters of the RF magnetron sputtering were: the background vacuum was 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30 Pa, the working pressure was 0.30 Pa, the target distance was 40 cm, the sputtering power was 80 W, the sputtering temperature was 25° C., and the sputtering was performed for 10 min. The carbon material with silicon nanolayer deposition was obtained, which was recorded as Si-G.
[0094] The artificial interface layer is further deposited on the surface of the carbon material deposited with the silicon nanolayer. The LiF and Li3N targets are opened and the artificial interface layer is sputtered. The process parameters of the RF magnetron sputtering are: at a background vacuum of 5.0×10 -4 When the argon gas with a purity of 99.99% was introduced at 0.30Pa, the working pressure was 0.30Pa, the target distance was 40cm, the sputtering power was 100W, the sputtering temperature was 25°C, and the sputtering was performed for 2min. A high specific energy silicon-carbon negative electrode material was obtained, which was recorded as LiF-Li3N / Si-G silicon-carbon negative electrode material.
[0095] The thickness of the silicon nanolayer is 10 nm. The thickness of the artificial interface layer is 10 nm.
[0096] Application Example 1
[0097] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-NGr obtained in Example 1 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0098] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 1 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0099] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0100] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0101] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0102] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0103] The charge and discharge test of the soft-pack full battery prepared in Example 1 showed that the soft-pack full battery had an energy density of 360Wh / kg, a charge and discharge coulomb efficiency of 89% in the first week, and a capacity retention rate of 83% after 500 cycles at a rate of 0.2C. Figure 1 .
[0104] Application Example 2
[0105] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-AGr obtained in Example 2 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0106] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 2 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0107] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0108] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0109] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0110] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0111] The charge and discharge test of the soft-pack full battery prepared in Example 2 showed that the soft-pack full battery had an energy density of 350Wh / kg, a charge and discharge coulomb efficiency of 91% in the first week, and a capacity retention rate of 85% after 500 cycles at a rate of 0.2C. Figure 2 .
[0112] Application Example 3
[0113] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-MCMB obtained in Example 3 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0114] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 3 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0115] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0116] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0117] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0118] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0119] The charge and discharge test of the soft-pack full battery prepared in Example 3 showed that the soft-pack full battery had an energy density of 350Wh / kg, a charge and discharge coulomb efficiency of 90% in the first week, and a capacity retention rate of 87% after 500 cycles at a rate of 0.2C.
[0120] Application Example 4
[0121] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-APC obtained in Example 4 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0122] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 4 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0123] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0124] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0125] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0126] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0127] The charge and discharge test of the soft-pack full battery prepared in Example 4 showed that the soft-pack full battery had an energy density of 310Wh / kg, a charge and discharge coulomb efficiency of 89% in the first week, and a capacity retention rate of 90% after 500 cycles at a rate of 0.2C.
[0128] Application Example 5
[0129] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-NC obtained in Example 5 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0130] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 5 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0131] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0132] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0133] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0134] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0135] The charge and discharge test of the soft-pack full battery prepared in Example 5 showed that the soft-pack full battery had an energy density of 350Wh / kg, a charge and discharge coulomb efficiency of 88% in the first week, and a capacity retention rate of 81% after 500 cycles at a rate of 0.2C.
[0136] Application Example 6
[0137] The high specific energy silicon-carbon negative electrode material LiF-Li3N / Si-G obtained in Example 6 is used to assemble a NCM811 soft-pack full battery. The specific method is as follows:
[0138] Polyacrylic acid and polyvinyl alcohol are mixed in a mass ratio of 95:5 as a polymer binder. The high specific energy silicon-carbon negative electrode material prepared in Example 6 is dispersed in deionized water with super-P and a polymer binder in a mass ratio of 90:4:15, and a silicon-carbon negative electrode slurry is prepared after vacuum stirring for 2 hours. With copper foil as the substrate, the prepared silicon-carbon negative electrode slurry is coated on the copper foil; the copper foil with the silicon-carbon negative electrode slurry is placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain a multilayer silicon-carbon negative electrode for a lithium-ion battery.
[0139] NCM811, super-P and polyvinylidene fluoride were dispersed in N-methylpyrrolidone in a weight ratio of 95:5:5 to form a mixture; the mixture was stirred in a vacuum for 2 hours to form NCM811 positive electrode slurry. With Al foil as the substrate, the NCM811 positive electrode slurry was dripped on the Al foil, and then the NCM811 positive electrode slurry was flattened. The Al foil with the NCM811 positive electrode slurry was placed in a vacuum drying oven at 100°C and dried for 12 hours to obtain the NCM811 positive electrode of the lithium-ion battery.
[0140] Dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate are mixed in equal volumes to prepare a mixed solvent, lithium hexafluorophosphate is dissolved in the mixed solvent, wherein the concentration of lithium hexafluorophosphate is 1 mol / L; then 5 mass% of fluoroethylene carbonate is added, and the mixture is mixed evenly to prepare an electrolyte.
[0141] The multilayer silicon-carbon negative electrode, NCM811 positive electrode and Celgard separator are placed in a pre-shaped aluminum-plastic film battery strip, a certain amount of electrolyte is injected, and the NCM811 soft-pack full battery is assembled.
[0142] The packaged NCM811 soft-pack full battery was subjected to constant current charge and discharge at a current density of 0.05C for the formation process and testing, with a voltage range of 3.0V to 4.2V.
[0143] The charge and discharge test of the soft-pack full battery prepared in Example 6 showed that the soft-pack full battery had an energy density of 400Wh / kg, a charge and discharge coulomb efficiency of 85% in the first week, and a capacity retention rate of 80% after 500 cycles at a rate of 0.2C.
[0144] Table 1 Effect of silicon-carbon anode prepared with different carbon core materials on battery performance
[0145] Carbon Core Material Energy density First cycle charge and discharge coulomb efficiency Capacity retention rate Example 1 NGN 360Wh / kg 89% 83% Example 2 AG 350Wh / kg 91% 85% Example 3 MCMB 350Wh / kg 90% 87% Example 4 APC 310Wh / kg 89% 90% Example 5 NC 350Wh / kg 88% 81% Example 6 G 400Wh / kg 85% 80%
[0146] The results in Table 1 show that the present invention deposits silicon nanolayers and artificial interface layers of LiF and Li3N on the surfaces of different carbon materials by using magnetron sputtering technology. Combining the advantages of the close connection between silicon-carbon materials prepared by magnetron sputtering technology and the designed artificial interface layer, the cycle life and coulomb efficiency of the silicon-carbon negative electrode material are improved, while also preventing it from producing irreversible capacity decay. Based on this, the above-mentioned embodiments of the present invention, while improving the discharge capacity of the silicon negative electrode, fundamentally avoid the huge volume changes caused by the lithium insertion process of the silicon-based negative electrode material and the resulting interface film failure.
[0147] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high specific energy silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material is obtained by sequentially depositing a silicon nanolayer and an artificial interface layer on the surface of a carbon core material using a physical vapor deposition method; the material of the artificial interface layer is at least one of LiF and Li3N; The thickness of the silicon nanolayer is 10nm-800nm; the thickness of the artificial interface layer is 10nm-50nm.
2. The high specific energy silicon-carbon negative electrode material according to claim 1, characterized in that: The carbon core material is any one of natural graphite material, artificial graphite material, mesophase carbon microspheres, amorphous porous carbon, biomass carbon, and graphene.
3. A method for preparing the high specific energy silicon-carbon negative electrode material according to claim 1, characterized in that: The following steps are involved: A silicon nanolayer is uniformly deposited on the surface of the carbon core material by a physical vapor deposition method, and then an artificial interface layer is further deposited on the surface of the silicon nanolayer to prepare a high specific energy silicon-carbon negative electrode material.
4. The method for preparing a high specific energy silicon-carbon negative electrode material according to claim 3, characterized in that: Before uniformly depositing the silicon nanolayer on the surface of the carbon core material, the method further includes subjecting the carbon core material to ball milling and shaping so as to perform surface treatment on the carbon core material.
5. The method for preparing a high specific energy silicon-carbon negative electrode material according to claim 3, characterized in that: Physical vapor deposition is carried out in a radio frequency magnetron sputtering chamber, wherein a rotating sample stage is rotatably arranged in the radio frequency magnetron sputtering chamber, and the carbon core material is placed on the rotating sample stage; a stirring mechanism is rotatably arranged on the rotating sample stage, and the stirring mechanism is configured so that a silicon nanolayer and an artificial interface layer can be uniformly deposited on the surface of the powder particles of the carbon core material during the radio frequency magnetron sputtering process.
6. The method for preparing a high specific energy silicon-carbon negative electrode material according to claim 3, characterized in that: The process parameters for depositing silicon nanolayer or artificial interface layer are: background vacuum degree is 0.1×10 -4 Pa~9.9×10 -4 Pa, the working gas pressure is 0.35Pa~0.55Pa, and the purity of silicon target, LiF target and Li3N target is ≥99.99%; The target distance is 10cm to 50cm, the sputtering temperature is 20℃ to 30℃, and the sputtering time is 1min to 10min.
7. Use of the high specific energy silicon-carbon negative electrode material according to claim 1 in preparing a silicon-carbon negative electrode for assembling a lithium battery.
8. The use according to claim 7, characterized in that The silicon-carbon negative electrode is obtained by dispersing the high specific energy silicon-carbon negative electrode material, a conductive additive, and a polymer binder in water, then coating the mixture on a metal substrate, and drying the mixture; The mass ratio of high specific energy silicon-carbon negative electrode material to conductive additive and polymer binder is 90:4:15; The polymer adhesive is a mixture of polyacrylic acid and polyvinyl alcohol, and the mass ratio of polyacrylic acid to polyvinyl alcohol is 95:5-50:
50.
9. The use according to claim 7, characterized in that: The lithium battery is a soft-pack lithium battery or a half-battery.
Citation Information
Patent Citations
Silicon-carbon cathode material with artificial SEI layers, high specific volumetric capacity and cycle performance
CN106207177A
Anode and preparation method thereof, lithium battery
CN109148826A
High-specific-energy lithium metal battery based on alloy element modified diaphragm
CN111969162A
Silicon-based material coated with composite coating as well as preparation method and application of silicon-based material
CN115747760A
Silicon-carbon negative electrode material, battery negative electrode, battery and preparation method of silicon-carbon negative electrode material
CN117613233A
Cited By
Silicon-carbon negative electrode pre-lithiation method using magnetron sputtering technology and application of silicon-carbon negative electrode pre-lithiation method