Catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane and preparation method thereof
Through the preparation of titanium-aluminum-carbon MAX-phase ceramic film and hydrofluoric acid etching technology, the self-stacking and polymer coverage of MXenes-based catalytic electrodes are solved, and high-performance and stable catalytic electrodes are achieved, which are suitable for a variety of electrocatalytic reactions and Reduced costs.
Patent Information
- Application Number
- CN202411444848.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-16
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-10-16
AI Technical Summary
During the application process, the active sites are covered due to the self-stacking of two-dimensional layered materials, and the catalytic performance is not ideal, and the polymer binder cover leads to a reduced charge transfer rate and poor mechanical stability.
The porous ceramic membrane was prepared by phase conversion casting and reaction sintering method by etching the titanium-aluminum carbon MAX phase ceramic membrane, and the MXenes/MAX heterogeneous ceramic membrane was formed by hydrofluoric acid etching. The catalysis was prepared by immersion, hydrothermal or electrodeposition methods. The electrodes, avoid the use of polymer binders, directly grow layered Ti3C2 MXenes and catalytic layers in situ on the ceramic substrate.
The high performance and stability of the catalytic electrode are achieved, the disorderly accumulation of two-dimensional layered materials is avoided, sufficient active sites are exposed, mechanical stability and charge transfer rate are improved, suitable for a variety of electrocatalytic reactions, and reduced Preparation cost.
Smart Images

Figure BDA0005087447720000061 
Figure BDA0005087447720000071 
Figure HDA0005087447740000011
Abstract
Description
Technical Field
[0001] The invention relates to a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic film and a preparation method thereof, belonging to the technical field of new energy material preparation. Background Art
[0002] With the continuous consumption of traditional fossil energy and the gradual deterioration of the earth's ecological environment, the development of new energy and advanced energy conversion and storage technologies have attracted the attention of more and more countries. Hydrogen energy has extremely high combustion calorific value and energy density, and the only product after combustion is water, so it is considered to be the most noteworthy new energy. As the upstream of the hydrogen energy industry chain, hydrogen production is the cornerstone of the entire industry, so the development of hydrogen production technology has become a hot topic in recent years. Among them, hydrogen production by electrolysis of water is considered to have the most development potential because of its environmental friendliness, easy combination with other renewable energy sources (such as solar energy, wind energy, etc.) and high product purity. At the same time, hydrogen fuel cell technology in the downstream of the hydrogen energy industry chain is also very promising in the field of energy conversion. Electrocatalytic carbon dioxide technology can use renewable electricity to convert greenhouse gas carbon dioxide into chemicals with high added value. It can not only store renewable energy, but also help reduce the content of carbon dioxide in the atmosphere. It is an advanced energy conversion and storage technology. In addition, although many technologies such as electrochemical synthesis of ammonia, oxygen reduction, and methanol oxidation are still in the initial development stage, they also have very broad development space in the future. It is worth noting that in all the above fields, the development of high-performance and low-cost catalytic electrodes is the focus of people's attention.
[0003] Two-dimensional layered MXenes are considered to be a very good catalyst carrier due to their excellent conductivity, rich surface groups and special layered structure. Catalytic electrodes based on MXenes can not only carry out rapid charge transfer, but also effectively regulate the catalytic performance of active sites by virtue of the interaction between MXenes and catalysts. As an emerging two-dimensional layered material, MXenes are mainly formed by etching the precursor MAX phase ceramic, and its typical chemical formula is M n+1 X n T x, where M is mainly a transition metal (such as titanium, molybdenum, vanadium, etc.), X is carbon or nitrogen, and T refers to surface functional groups such as hydroxyl groups. Although the development of MXenes-based catalytic electrodes has achieved very good results recently, there is a problem that has always plagued this type of catalytic electrode, that is, during the application process, the two-dimensional layered MXenes materials often stack on each other "self-stacking" phenomenon, so that a large number of active sites are covered, and ultimately the catalytic performance of the electrode is not ideal. In addition, the main preparation method of the catalytic electrode is to use a polymer binder to evenly coat the powder catalyst on the surface of the conductive substrate, and this operation will cause a large number of active sites to be covered by the polymer and reduce the charge transfer rate of the catalytic electrode. Moreover, on such a catalytic electrode, the adhesion between the catalyst and the substrate is weak, and the catalyst is easy to fall off naturally during the use of the electrode, resulting in poor mechanical stability of the catalytic electrode. Summary of the invention
[0004] The present invention aims to propose a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane and a preparation method thereof. The method first prepares a high-strength porous titanium aluminum carbon MAX phase ceramic membrane by phase transformation tape casting combined with reaction sintering, and then performs hydrofluoric acid etching on it to obtain a MXenes / MAX heterogeneous ceramic membrane with a unique layered structure inside, and then prepares a catalytic electrode with excellent performance and stability by impregnation, hydrothermal or electrodeposition methods.
[0005] In order to achieve the purpose, the present invention adopts the following technical scheme:
[0006] A method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane comprises the following steps:
[0007] (1) mixing titanium carbide, metallic titanium, metallic aluminum powders with a solvent, a dispersant, and a binder by ball milling to obtain a uniform ceramic slurry;
[0008] (2) The ceramic slurry is degassed, cast, solidified by phase transformation, and naturally dried to obtain a ceramic membrane green body;
[0009] (3) sintering the ceramic membrane green body to obtain a porous titanium aluminum carbon MAX phase ceramic membrane;
[0010] (4) placing the porous titanium aluminum carbon MAX phase ceramic membrane in hydrofluoric acid for etching to obtain a MXenes / MAX heterogeneous ceramic membrane with a unique layered structure inside;
[0011] (5) forming a catalytic layer on the MXenes / MAX heterogeneous ceramic membrane by impregnation treatment, hydrothermal treatment, vapor deposition, vapor phase conversion and / or electrodeposition treatment, thereby obtaining a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane.
[0012] Furthermore, in step 1 (middle), the particle size of the titanium carbide, metallic titanium and metallic aluminum powders is 1-10 μm.
[0013] Furthermore, in step (1), the molar ratio of the titanium carbide, metallic titanium and metallic aluminum powders is 1:1.5-2:1-1.3.
[0014] Furthermore, in step (1), the solvent is N-methylpyrrolidone, the dispersant is at least one of KD-1 dispersant, polyvinylpyrrolidone and O-(2-aminopropyl)-O′-(2-methoxyethyl)polypropylene glycol, and the binder is at least one of polyvinyl alcohol, polyvinyl butyral and polyether sulfone.
[0015] Furthermore, in step (1), the rotation speed of the ball mill is 200-300 r min -1 , ball milling time is 36-50h.
[0016] Furthermore, in step (2), the ceramic slurry is first degassed for 0.5-1h, then poured into the mold tank, and the casting scraper height is adjusted to 0.5-1mm, and the casting speed is 30-100cm min -1 After the film is cast, it is placed in water for curing for 18-24 hours and then naturally dried to obtain the ceramic membrane green body.
[0017] Furthermore, in step (3), the sintering temperature is raised by first heating at 3-5°C min -1 The heating rate is raised to 660-700℃, kept at this temperature for 5-10min, and then heated at 3-5℃min -1 The heating rate is raised to 820-850℃, kept at this temperature for 10-15min, and then heated at 3-5℃min -1 The heating rate was raised to 1000-1050℃, and then the temperature was increased at 2-3℃min -1 The heating rate is raised to 1100-1500°C and kept at this temperature for 0.5-3h. The sintering atmosphere is argon or nitrogen.
[0018] Furthermore, in step (4), the mass concentration of the hydrofluoric acid is 30-40%, the etching temperature is 25-60° C., and the etching time is 2-24 h.
[0019] Furthermore, in step (4), the MXenes / MAX heterogeneous ceramic membrane has titanium aluminum carbon (Ti3AlC2) MAX phase ceramic as the skeleton, and the derived layered Ti3C2 MXenes are in-situ grown on the surface of the skeleton to form a layered structure.
[0020] Further, in step (5), the catalytic layer formed is a catalytic layer composed of at least one of platinum, ruthenium, molybdenum disulfide, molybdenum dioxide, nickel iron oxyhydroxide, nickel ferrite and cobalt ferrite in the form of at least one of nanoparticles, nanosheets and nanocubes, or a metal organic framework catalytic layer containing at least one transition metal of copper, nickel and iron, or a molybdenum disulfide catalytic layer doped with at least one element of phosphorus, nitrogen and selenium. The preparation method of the catalytic layer includes but is not limited to immersion treatment, hydrothermal treatment, vapor deposition, vapor phase conversion and / or electrodeposition treatment. For example, the following method can be used to form the corresponding catalytic layer:
[0021] The platinum catalyst layer was formed by impregnation treatment: the MXenes / MAX heterogeneous ceramic membrane was impregnated to a concentration of 0.01-0.5 mg mL -1 The MXenes / MAX heterogeneous ceramic membrane is formed by ultrasonicating the MXenes / MAX heterogeneous ceramic membrane in an ethanol solution of chloroplatinic acid for 6-24 hours and then vacuum drying the membrane at 40-120°C for 12-24 hours to obtain a catalytic layer, thereby obtaining a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane. The catalytic layer formed is a platinum nanoparticle layer.
[0022] A molybdenum sulfide catalytic layer is formed by hydrothermal treatment: sodium molybdate dihydrate and thiourea are first added to a mixture of propionic acid and deionized water, and the mixed solution and the MXenes / MAX heterogeneous ceramic membrane are transferred to a hydrothermal kettle after stirring evenly. The mixture is hydrothermally treated at 160-180°C for 8-12 hours to form a catalytic layer on the MXenes / MAX heterogeneous ceramic membrane, thereby obtaining a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane. The catalytic layer formed is a molybdenum sulfide nanosheet layer.
[0023] The nickel ferrite catalyst layer is formed by hydrothermal treatment: ferric nitrate nonahydrate and nickel chloride hexahydrate are added to the N,N-dimethylformamide solution, and magnetic stirring is performed to obtain a mixed solution. The mixed solution and the MXenes / MAX heterogeneous ceramic membrane are then transferred to a hydrothermal reactor and hydrothermally treated at 180-200°C for 10-20h to form a catalyst layer on the MXenes / MAX heterogeneous ceramic membrane, thereby obtaining a catalytic electrode based on the titanium aluminum carbon MAX phase ceramic membrane. The catalyst layer formed is a nickel ferrite nanoparticle layer.
[0024] The Cu-MOF catalyst layer was prepared by electrodeposition combined with hydrothermal treatment: sodium hydroxide and trimesic acid were first dissolved in deionized water to obtain a uniform electrolyte, and then a two-electrode system was constructed with MXenes / MAX heterogeneous ceramic membrane and platinum electrode as the working electrode and counter electrode respectively. The system was operated for 0.5-2h at a constant voltage of 2-5V to obtain the MXenes / MAX heterogeneous ceramic membrane after electrodeposition treatment. Subsequently, the MXenes / MAX heterogeneous ceramic membrane after electrodeposition treatment was placed in a copper nitrate solution, and the trimesic acid solution was slowly dripped into it. After magnetic stirring, it was transferred to a hydrothermal reactor and hydrothermally reacted at 80-95°C for 15-20h to form a catalyst layer on the MXenes / MAX heterogeneous ceramic membrane, and a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane was obtained. The catalyst layer formed was a Cu-MOF nanocube layer.
[0025] Hydrothermal treatment is used to form a phosphorus-doped molybdenum disulfide catalytic layer: sodium molybdate dihydrate, thiourea, and sodium hypophosphite monohydrate are added to deionized water in a molar ratio of 1:5-7:1-3 and stirred evenly. Then, concentrated hydrochloric acid is slowly dripped into it to adjust the pH value to 1-3, and then stirred evenly. The prepared mixed solution and the MXenes / MAX heterogeneous ceramic membrane are transferred to a hydrothermal kettle together, and the hydrothermal reaction is carried out at 200°C for 24 hours to form a catalytic layer on the MXenes / MAX heterogeneous ceramic membrane, and a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane is obtained. The catalytic layer formed is a phosphorus-doped molybdenum disulfide nanosheet layer containing rich defects.
[0026] The catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane prepared by the present invention is a layered Ti3C2 MXenes formed in situ on the surface of titanium aluminum carbon (Ti3AlC2) ceramic, and the catalytic layer grows from the layered phase. It can be applied to electrocatalytic fields such as full hydrolysis, oxygen reduction, carbon dioxide reduction, electrochemical synthesis of ammonia, methanol oxidation, and urea oxidation.
[0027] The present invention adopts a simple and easy-to-operate method to prepare a catalytic electrode based on titanium aluminum carbon MAX phase ceramics that can show excellent performance and stability in the field of electrocatalysis. Compared with the prior art, the beneficial effects of the present invention are embodied in:
[0028] The present invention first uses mature porous ceramic preparation technology to synthesize a porous titanium aluminum carbon MAX phase ceramic membrane, then obtains a MXenes / MAX heterogeneous ceramic membrane by etching, and then obtains a catalytic electrode based on the titanium aluminum carbon MAX phase ceramic membrane by using an easily industrialized processing process. Compared with other MXenes-based catalytic electrodes, the layered MXenes in the catalytic electrode prepared by the present invention are directly grown in situ on the surface of MAX phase ceramics with excellent conductivity and high mechanical strength, avoiding the disordered stacking of two-dimensional layered MXenes, thereby exposing sufficient active sites. At the same time, the present invention directly grows the catalytic layer on the surface of the ceramic substrate through an in situ growth process, avoiding the use of a polymer binder. In addition, the mechanical / chemical stability of the porous ceramic membrane itself is very good, and the hydrophilicity and internal pore structure of the surface are easy to adjust, so that the performance of the catalytic electrode based on the ceramic membrane is easy to adjust, which can meet the needs of a variety of electrocatalytic reactions. Finally, the preparation technology and process adopted by the present invention are relatively mature and low-cost, suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of (a) casting and (b) phase conversion molding in Example 1 of the present invention;
[0030] Figure 2 This is a cross-sectional scanning electron microscope image of the titanium aluminum carbon MAX phase ceramic film obtained after sintering at 1400° C. for 1.5 hours in an argon atmosphere in Example 1 of the present invention, where (a) corresponds to a small magnification and (b) corresponds to a large magnification.
[0031] Figure 3 This is a scanning electron microscope image of the MXenes / MAX heterogeneous ceramic membrane obtained after treatment with hydrofluoric acid (40 wt.%) for 12 hours in Example 1 of the present invention.
[0032] Figure 4 The Pt@TC / TAC-0.1 catalytic electrode prepared in Example 1 of the present invention ( Figure 4 (a)) and the MS@TC / TAC-12 catalytic electrode prepared in Example 2 ( Figure 4 (b) is a scanning electron microscope image of the sample.
[0033] Figure 5 Figure 2 is a diagram of the electrochemical testing device used in Examples 1, 2, and 3 of the present invention (a is the overall device, and b is a local enlarged view of the working electrode), wherein the working electrode is the prepared ceramic electrode, the reference electrode is a saturated silver / silver chloride (acidic environment) or a mercury / mercury oxide electrode (alkaline environment), and the counter electrode is a graphite rod.
[0034] Figure 6This is a diagram of the electrochemical testing device used in Examples 4 and 5 of the present invention, wherein the working electrode is the prepared ceramic electrode, the reference electrode is a saturated silver / silver chloride (acidic or neutral environment) or mercury / mercury oxide electrode (alkaline environment), the counter electrode is a platinum sheet electrode, and the ion exchange membrane is Nafion N117.
[0035] Figure 7 The LSV curve of hydrogen evolution of the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane prepared in Example 2 ( Figure 7 (a)) and overpotential ( Figure 7 (b) in the figure.
[0036] Figure 8 The oxygen evolution LSV curve of the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane prepared in Example 3 ( Figure 8 (a)) and the corresponding Tafel slope ( Figure 8 (b) in the figure.
[0037] Fig. 9 The Faraday efficiency (FE) of the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane prepared in Example 4 for the conversion of CO2 into formic acid in a CO2-saturated 0.5M KHCO3 electrolyte is Formate ) and the corresponding current density.
[0038] Fig.10 The yield and Faraday efficiency of electrochemically synthesized NH3 in N2-saturated 0.1MNa2SO4 electrolyte using the catalytic electrode based on titanium-aluminum-carbon MAX phase ceramic membrane prepared in Example 5. DETAILED DESCRIPTION
[0039] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby.
[0040] Example 1
[0041] In this embodiment, the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is prepared according to the following steps:
[0042] (1) Ceramic slurry: Titanium carbide powder with a particle size distribution range of 5-10 μm and metal titanium and metal aluminum powder with a particle size distribution range of 1-3 μm were mixed in a molar ratio of 1:1.5:1.3, and then 3% of the total mass of the above powders were added as a dispersant of O-(2-aminopropyl)-O′-(2-methoxyethyl) polypropylene glycol, 11.11% of polyethersulfone as a binder, and 30% of the total mass of the slurry was added as a solvent of N-methylpyrrolidone. The mixture was then poured into a ball mill for ball milling at a speed of 280 rmin. -1 , the ball milling time is 48h.
[0043] (2) After degassing the ceramic slurry for 30 minutes, pour it into the casting mold tank, adjust the scraper height to 1.0 mm, and control the casting speed to 30 cm min -1 After casting, the membrane was placed horizontally in a water tank. After standing for 18 hours, the sample was taken out of the water and placed in a room temperature environment to dry for 7 days to obtain a titanium aluminum carbon MAX phase ceramic membrane green body.
[0044] (3) The titanium aluminum carbon MAX phase ceramic film green body was placed in a corundum tube furnace with argon flowing at 3℃min -1 The temperature was raised to 660°C at a rate of 5°C min -1 The temperature was raised to 820℃ at a rate of 5℃min -1 The heating rate was increased to 1000°C, and then the heating rate was reduced to 2°C min -1 , the temperature was raised to 1400℃ and kept at this temperature for 1.5h to obtain a porous titanium aluminum carbon MAX phase ceramic membrane. The cross-sectional scanning electron microscope image is shown in Figure 2 As shown, it can be seen that the ceramic membrane has an asymmetric finger-like straight-through pore structure with a pore size of 80-100 μm, and there are many small pores of 0.5-2 μm inside the finger-like pores, indicating the existence of a hierarchical porous structure.
[0045] (4) The porous titanium aluminum carbon MAX phase ceramic membrane was placed in a hydrofluoric acid solution with a temperature of 25°C and a mass concentration of 40% and etched for 12 hours to obtain a MXenes / MAX heterogeneous ceramic membrane with a special layered structure inside. The scanning electron microscope image is shown in FIG. Figure 3 As shown, the special layered structure inside the ceramic membrane can be seen.
[0046] (5) The MXenes / MAX heterogeneous ceramic membrane was immersed in water with a mass concentration of 0.025, 0.05, 0.1, and 0.2 mg mL -1 The MXenes / MAX heterogeneous ceramic membrane was formed with a platinum nanoparticle catalytic layer, and catalytic electrodes based on titanium aluminum carbon MAX phase ceramic membrane were obtained, which were recorded as Pt@TC / TAC-0.025, Pt@TC / TAC-0.05, Pt@TC / TAC-0.1, and Pt@TC / TAC-0.2, respectively.
[0047] like Figure 4 As shown in (a), the platinum particles in the obtained Pt@TC / TAC-0.1 sample are evenly distributed on the surface of the catalytic electrode and in the special layered structure formed by etching.
[0048] Subsequently, a three-electrode system was constructed using the prepared catalytic electrode as the working electrode, saturated silver / silver chloride as the reference electrode, and graphite as the counter electrode ( Figure 5 ), and the electrochemical hydrogen evolution test was carried out in an acidic (0.5M H2SO4) electrolyte. The results are shown in Table 1. The hydrogen evolution performance of the catalytic electrode first increases with the increase of chloroplatinic acid concentration, and then increases at 0.1 mg mL -1 The performance of the Pt@TC / TAC-0.1 electrode peaked at 10 mA cm -2 The overpotential required for the current density is only 50mV, which is much lower than that of other catalytic electrodes, showing excellent hydrogen evolution activity. In addition, in order to verify the industrial application prospects of the prepared catalytic electrode, this example tests the electrode at a high current density (1000mAcm -2 ) were also compared. Among them, the Pt@TC / TAC-0.1 electrode output 1000mA cm -2 The overpotential required for the current density is only 346 mV, which is still much smaller than that of the other electrodes.
[0049] Table 1. HER performance of the Pt@TC / TAC-X (X: mass concentration of chloroplatinic acid) catalytic electrode prepared in Example 1 in 0.5MH2SO4 medium
[0050]
[0051] Example 2
[0052] In this embodiment, the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is prepared according to the following steps:
[0053] Step (1) to step (3): the same as in Example 1.
[0054] Step (4): Place the porous titanium aluminum carbon MAX phase ceramic membrane in a hydrofluoric acid solution at a temperature of 25°C and a mass concentration of 40%, and etch for 8, 10, and 12 hours, respectively, to obtain MXenes / MAX heterogeneous ceramic membranes with a special layered structure inside, recorded as TC / TAC-8, TC / TAC-10, and TC / TAC-12.
[0055] Step (5): Add sodium molybdate dihydrate and thiourea in a molar ratio of 1:8 to a mixture of propionic acid and deionized water in a volume ratio of 1:2, stir evenly, and transfer into a hydrothermal reactor together with the MXenes / MAX heterogeneous ceramic membrane prepared in the previous step. Perform a hydrothermal reaction at 180°C for 8 hours to form a molybdenum sulfide nanosheet catalytic layer on the MXenes / MAX heterogeneous ceramic membrane, and obtain catalytic electrodes based on titanium aluminum carbon MAX phase ceramic membranes, which are named MS@TC / TAC-8, MS@TC / TAC-10, and MS@TC / TAC-12, respectively.
[0056] The surface morphology of the catalytic electrode MS@TC / TAC-12 is shown in Figure 4 As shown in (b), petal-shaped MoS nanosheets grow uniformly on the surface of the catalytic electrode. Figure 4 In the enlarged image of (b), it can be clearly observed that the MoS nanosheets have been inserted into the interlayer of the layered structure formed by etching. Figure 5 As shown, the working electrode is the prepared catalytic electrode, the reference electrode is a saturated silver / silver chloride electrode, the counter electrode is a graphite electrode, and the electrolyte is 0.5M H2SO4. Figure 7 The LSV curves of the catalytic electrodes show that the performance of the catalytic electrodes gradually improves with the continuous extension of etching time. Among them, the MS@TC / TAC-12 electrode exhibits the best hydrogen evolution activity, and can output 10 mA cm at overpotentials of 137 mV, 259 mV, and 278 mV, respectively. -2 、1000mAcm -2 and 2000mA cm -2 The current density of the electrodes is much lower than that of MS@TC / TAC-8 (168 mV, 296 mV and 321 mV) and MS@TC / TAC-10 (142 mV, 283 mV and 305 mV).
[0057] Example 3
[0058] In this embodiment, the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is prepared according to the following steps:
[0059] Step (1) to step (4): the same as in Example 1.
[0060] Step (5): Add ferric nitrate nonahydrate and nickel chloride hexahydrate to the N,N-dimethylformamide solution at a molar ratio of 1:1, and stir magnetically for 0.5 h to obtain a uniform mixed solution. Then transfer the prepared MXenes / MAX heterogeneous ceramic membrane and the mixed solution to a hydrothermal reactor and perform hydrothermal treatment at 200°C for 10, 15, and 20 h to form a nickel ferrite nanoparticle catalytic layer on the MXenes / MAX heterogeneous ceramic membrane, and obtain catalytic electrodes based on titanium aluminum carbon MAX phase ceramic membranes, which are respectively recorded as Ni / Fe-200-10, Ni / Fe-200-15, and Ni / Fe-200-20.
[0061] like Figure 5 As shown, the prepared catalytic electrode was used as the working electrode, the mercury / mercury oxide electrode was used as the reference electrode, and graphite was used as the counter electrode to conduct an electrochemical oxygen evolution test in an alkaline (1M KOH) medium. The test results are shown in Figure 8 As shown in Table 2, the Ni / Fe-200-15 electrode outputs 10 mA cm-2 The required overpotential is 225 mV and the Tafel slope is 79 mV dec -1 , both better than Ni / Fe-200-10 (265mV, 82mV dec -1 ) and Ni / Fe-200-20 electrode (303mV, 114mV dec -1 ), showing the best oxygen evolution performance.
[0062] Table 2. OER performance of the Ni / Fe-200-x (x: hydrothermal time) electrode prepared in Example 3 in 1M KOH medium.
[0063]
[0064] Example 4
[0065] In this embodiment, the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is prepared according to the following steps:
[0066] Step (1) to step (4): the same as in Example 1.
[0067] Step (5): The MXenes / MAX heterogeneous ceramic membrane is used as the working electrode, the platinum electrode is used as the counter electrode, and the mixed solution of trimesic acid and sodium hydroxide (mass ratio 7:4) is used as the electrolyte to construct a two-electrode system. Subsequently, the working electrode is subjected to electrodeposition treatment at a constant voltage of 5 V for 2 h to obtain a MXenes / MAX heterogeneous ceramic membrane loaded with trimesic acid.
[0068] Step (6): First, prepare -1 The copper nitrate aqueous solution and the concentration are 0.018g mL -1 Secondly, the MXenes / MAX heterogeneous ceramic membrane after electrodeposition treatment was placed in a copper nitrate solution, and then the trimesic acid ethanol solution was slowly dripped into it until the volume ratio of the two solutions reached 1:1, followed by magnetic stirring for 0.5h, and then transferred to a hydrothermal kettle together, and hydrothermally reacted at 95°C for 15h, that is, a Cu-MOF nanocube catalytic layer was formed on the MXenes / MAX heterogeneous ceramic membrane, and a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane was obtained, which was recorded as Cu-BTC-95-15.
[0069] like Figure 6As shown, the prepared Cu-BTC-95-15 electrode was inserted into an H-type electrolytic cell as a working electrode, a platinum sheet electrode was used as a counter electrode, and a saturated silver / silver chloride electrode was used as a reference electrode to conduct an electroreduction test of carbon dioxide in a CO2-saturated 0.5M KHCO3 electrolyte. The prepared catalytic electrode exhibited excellent electrocatalytic carbon dioxide reduction activity and had good selectivity for formic acid products. Fig. 9 The Faradaic efficiency and corresponding partial current density of the Cu-BTC-95-15 electrode for converting CO2 into formic acid products in the voltage range of -0.9 to -1.3 V (vs. RHE) are shown. As the voltage increases from -0.9 V (vs. RHE) to -1.3 V (vs. RHE), the Faradaic efficiency (FE Formate ) first gradually increased from the initial 19%, reached a peak value (52%) at a voltage of -1.2 V (vs. RHE), and then dropped to 47% at -1.3 V (vs. RHE). In terms of current density, the partial current density corresponding to the formic acid product steadily increased with the increase of applied voltage, reaching a maximum value of 20.6 mA cm at -1.3 V (vs. RHE). -2 .
[0070] Example 5
[0071] In this embodiment, the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is prepared according to the following steps:
[0072] Step (1) to step (4): the same as in Example 1.
[0073] Step (5): Sodium molybdate dihydrate, thiourea, and sodium hypophosphite monohydrate are added to deionized water in a molar ratio of 1:5:1 and stirred for 10 minutes. Then, concentrated hydrochloric acid is slowly dripped into it to adjust the pH value to ~2, and stirring is continued for 30 minutes. The prepared mixed solution and the MXenes / MAX heterogeneous ceramic membrane are transferred into a hydrothermal reactor together, and the hydrothermal reaction is carried out at 200°C for 24 hours to form a phosphorus-doped molybdenum disulfide nanosheet catalyst layer on the MXenes / MAX heterogeneous ceramic membrane, and a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane is obtained, which is named TC / TAC-MS-P-1.
[0074] like Figure 6 As shown, the prepared TC / TAC-MS-P-1 electrode was inserted into an H-type electrolytic cell as a working electrode, a platinum sheet electrode was used as a counter electrode, and a saturated silver / silver chloride electrode was used as a reference electrode to conduct an electrochemical ammonia synthesis test in a 0.1M Na2SO4 electrolyte saturated with N2. Fig.10The results show that within the voltage range of -0.4 to -0.8 V (vs. RHE), the yield of electrochemical ammonia synthesis gradually increases with the increase of applied voltage, reaching a peak value (56 μg mg) at -0.6 V (vs. RHE). -1 cat. h -1 ), and then the voltage is increased, the yield begins to gradually decrease. In the same voltage range, the Faraday efficiency and yield of electrochemical ammonia synthesis have the same trend, and also reach a peak value (10.6%) at -0.6V (vs.RHE).
[0075] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the above disclosed methods and technical contents without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane, characterized in that: The steps include: (1) mixing titanium carbide, metallic titanium, metallic aluminum powders with a solvent, a dispersant, and a binder by ball milling to obtain a uniform ceramic slurry; (2) The ceramic slurry is degassed, cast, solidified by phase transformation, and naturally dried to obtain a ceramic membrane green body; (3) sintering the ceramic membrane green body to obtain a porous titanium aluminum carbon MAX phase ceramic membrane; (4) placing the porous titanium aluminum carbon MAX phase ceramic membrane in hydrofluoric acid for etching to obtain a MXenes / MAX heterogeneous ceramic membrane with a layered structure inside; (5) forming a catalytic layer on the MXenes / MAX heterogeneous ceramic membrane, i.e., preparing a catalytic electrode based on a titanium aluminum carbon MAX phase ceramic membrane.
2. The method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (1), the molar ratio of the titanium carbide, metallic titanium and metallic aluminum powders is 1:1.5-2:1-1.
3.
3. The method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (1), the solvent is N-methylpyrrolidone, the dispersant is at least one of KD-1 dispersant, polyvinylpyrrolidone and O-(2-aminopropyl)-O′-(2-methoxyethyl)polypropylene glycol, and the binder is at least one of polyvinyl alcohol, polyvinyl butyral and polyether sulfone.
4. The method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (1), the speed of the ball mill is 200-300 r min -1 , ball milling time is 36-50h.
5. The method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (2), the ceramic slurry is first degassed for 0.5-1h, then poured into the mold tank, the casting scraper height is adjusted to 0.5-1mm, and the casting speed is 30-100cm min -1 After the film is cast, it is placed in water for curing for 18-24 hours and then naturally dried to obtain the ceramic membrane green body.
6. The method for preparing a catalytic electrode based on a titanium-aluminum-carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (3), the sintering temperature is raised by: firstly heating at 3-5°C min -1 The heating rate is raised to 660-700℃, kept at this temperature for 5-10min, and then heated at 3-5℃min -1 The heating rate is raised to 820-850℃, kept at this temperature for 10-15min, and then heated at 3-5℃min -1 The heating rate was raised to 1000-1050℃, and then the temperature was increased at 2-3℃min -1 The heating rate is raised to 1100-1500°C and kept at this temperature for 0.5-3h. The sintering atmosphere is argon or nitrogen.
7. The method for preparing a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (4), the mass concentration of the hydrofluoric acid is 30-40%, the etching temperature is 25-60° C., and the etching time is 2-24 h.
8. The method for preparing a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (4), the MXenes / MAX heterogeneous ceramic membrane has a titanium aluminum carbon MAX phase ceramic as a skeleton, and the layered MXenes derived therefrom grow in situ on the surface of the skeleton to form a layered structure.
9. The method for preparing a catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane according to claim 1, characterized in that: In step (5), the catalytic layer is prepared by impregnation treatment, hydrothermal treatment, vapor deposition, vapor phase conversion and / or electrodeposition treatment, and the formed catalytic layer is a catalytic layer composed of at least one of platinum, ruthenium, molybdenum disulfide, molybdenum dioxide, nickel iron hydroxide, nickel ferrite and cobalt ferrite in the form of at least one of nanoparticles, nanosheets and nanocubes, or a metal organic framework catalytic layer containing at least one transition metal of copper, nickel and iron, or a molybdenum disulfide catalytic layer doped with at least one element of phosphorus, nitrogen and selenium.
10. A catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane prepared by the preparation method according to any one of claims 1 to 9.
11. An application of the catalytic electrode based on titanium aluminum carbon MAX phase ceramic membrane according to claim 10, characterized in that: The invention is applied to the electrocatalytic field including one of full hydrolysis, oxygen reduction, carbon dioxide reduction, electrochemical ammonia synthesis, methanol oxidation or urea oxidation.
Citation Information
Patent Citations
Method for synthesizing spherical MAX-phase powder material with main phase being Ti2AlC
CN106032324A
Preparation method and application of carbon dot-doped titanium carbide hydrogel composite material
CN108258218A
Oxygen atom in-situ doped MAX phase and in-situ doped MXene flexible membrane electrode material as well as preparation method and application thereof
CN113401904A
Porous conductive ceramic membrane loaded with photoelectric catalyst as well as preparation method and application of porous conductive ceramic membrane
CN114100637A
Tungsten carbide-based self-supporting membrane electrode and preparation method thereof
CN114292123A
Cited By
Preparation method of MXenes material rich in carbon defects in magnesium-carbon dioxide battery
CN120109207A