Rare earth modified non-noble metal monatomic catalyst as well as preparation method and application thereof

Through the multi-step three-speed pyrolysis method and the introduction of rare earth oxide nanoparticles, the electronic structure of Fe-N-C catalyst is regulated, and the problems of low utilization rate and poor stability of Fe-N-C catalyst are solved, and efficient oxygen reduction reaction is achieved Improved performance and stability.

CN119069724APending Publication Date: 2024-12-03GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310632504.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The active site utilization rate of existing Fe-N-C single-atom catalysts is low, resulting in poor oxygen reduction reaction (ORR) performance, and poor stability of Fe SACs, which are susceptible to Fenton reaction, resulting in catalyst inhomogeneity and instability.

Method used

The rare earth modified non-precious metal single atom catalyst is prepared by multi-step three-cycle pyrolysis method. Through the introduction of rare earth oxide nanoparticles, the electronic structure of the catalyst is regulated, the high dispersion and active site exposure of metal atoms are ensured, and the unique characteristics of rare earths are utilized. Reduce the effect of Fenton response.

Benefits of technology

It improves the activity and stability of the catalyst, especially under acidic conditions, exhibits excellent ORR activity, the half-wave potential reaches more than 0.8V, and the stability is significantly improved. It is suitable for fuel cells and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069724A_ABST
    Figure CN119069724A_ABST
Patent Text Reader

Abstract

The invention provides a rare earth modified non-noble metal monatomic catalyst and a preparation method and application thereof.The preparation method comprises the following steps that a porous carbon carrier, a transition metal source, an organic ligand and a solvent are mixed, dried, subjected to primary pyrolysis and subjected to secondary pyrolysis, and an unmodified product is obtained; mixing, drying and carbonizing a rare earth source, a solvent and the unmodified product to obtain the rare earth modified non-noble metal monatomic catalyst, according to the preparation method, the electronic structure of the catalyst can be regulated and controlled, a novel catalyst with M-N6 active sites is obtained, full exposure of the active sites under the loading of metal atoms with certain density is ensured, the layering porosity is provided, and meanwhile, by introducing the rare earth oxide nanoparticles and utilizing the characteristics of rare earth elements, the preparation method is simple, and the preparation cost is low. Fenton reaction generated by metal Fe is reduced, and the activity and stability of the catalyst are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a rare earth modified non-noble metal single atom catalyst and a preparation method and application thereof. Background Art

[0002] Due to the consumption of fossil fuels and the related environmental pollution, the development of clean and sustainable energy has always attracted much attention. The oxygen reduction reaction (ORR) is the core reaction of many renewable energy conversion and storage systems (such as metal-air batteries and fuel cells). It determines the conversion efficiency, but its slow kinetics greatly limit its commercial application. Therefore, the development of efficient ORR electrocatalysts is crucial to promote the widespread application of electrochemical energy systems. However, the current noble metal-based catalysts (such as platinum and its alloys) used for cathode oxygen reduction reaction (ORR) are severely hindered in large-scale application and commercialization due to their high cost, low abundance and poor durability. It is necessary to develop resource-abundant, highly active and durable non-noble metal-based ORR catalysts.

[0003] Single-atom catalysts have been shown to be the most effective candidates for driving the oxygen reduction reaction (ORR) in fuel cells and metal-air batteries due to their large atomic utilization and high electrocatalytic activity. Among them, non-precious metal nitrogen-doped carbon materials, especially iron and heteroatom-doped carbon, and atomically dispersed Fe / N / C catalysts (Fe SACs) are the most promising candidates for electrocatalytic reactions. However, not all single-atom sites in carbon-supported SACs participate in ORR activity. Generally speaking, the MN on the outer surface of the catalyst is x Atomic fractions are better able to participate in the ORR, while those blocked by dense graphene domains or water-flooded micropores remain inactive. So far, the utilization efficiency of these atomic sites, i.e., the effective sites contributing to the ORR among the total metal elements in SACs, cannot meet the existing needs. The presence of inaccessible atomic species in carbon supports not only wastes metal resources (which is more costly when relying on precious metal sites), but also leads to catalytic heterogeneity and instability. Therefore, the development of better preparation methods and reliable active site quantification techniques is crucial to improve the utilization of active sites.

[0004] In the prior art, in response to the above problems, a N-graphene-supported Gd2O3-Co heterostructure (Gd2O3-Co / NG) was prepared by a sol-gel-assisted method, and it was demonstrated that the addition of Gd2O3 to metallic Co can significantly improve its electrocatalytic performance for ORR. The resulting electrocatalyst exhibited excellent ORR activity with a half-wave potential of 0.82 V, which is comparable to the state-of-the-art Pt / C catalyst. The excellent ORR performance of Gd2O3-Co / NG is highly related to the important synergistic effect of Gd2O3 with metallic Co (i.e., valence electron effect and high oxygen vacancies) and the unique features of the N-graphene structure (i.e., porosity and electron-rich N doping).

[0005] In addition, the prior art also discloses that efficient electrocatalytic CO2 reduction can be achieved by changing the local electron density of the nickel three-dimensional orbit with gadolinium, and a Ni-Gd-N ternary doped carbon black electrocatalyst is produced, in which the Ni active site is exposed outside the carbon layer and the Ni nanoparticles are wrapped inside the carbon layer. Theoretical calculations and experiments show that adding Gd atoms to Ni-based electrocatalysts can change the local electron density of Ni three-dimensional orbits and adjust the size of Ni nanoparticles, thereby enhancing the electronic activity of Ni and reducing the HER performance of Ni.

[0006] At the same time, the prior art also discloses a method combining electrospinning technology and in-situ growth to synthesize Ce-doped Co3O4 nanoparticles embedded in carbon nanofiber complex catalysts (Ce@Co3O4 / CNFs); in an alkaline environment, the Ce@Co3O4 / CNFs catalyst exhibits performance comparable to that of Pt / C and RuO2, with half-wave potentials of 0.810 V and 380 mV (@10 mA cm) for ORR and OER, respectively. -2 ); and, an all-solid-state rechargeable zinc-air battery with Ce@Co3O4 / CNFs as cathode catalyst was assembled, which has a relatively narrow discharge-charge voltage difference and good cycle performance.

[0007] However, the existing technology still does not provide a solution to the low atomic utilization of active sites of Fe-NC SACs, which leads to poor ORR performance. In addition, how to improve the ORR activity by adjusting the electronic structure of Fe-NC catalysts is still a huge challenge. In current research, the preparation methods of single-atom catalysts mainly include atomic layer deposition, chemical vapor deposition, wet chemical method (including co-precipitation, impregnation and photochemical method, etc.), ball milling and high-temperature pyrolysis. Among these synthesis methods, wet chemical method and high-temperature pyrolysis method are commonly used and easy to operate in the preparation of electrochemical ORR catalysts. In the wet chemical method, the atomic dispersion of metal precursors and the migration and agglomeration of stably formed single atoms are the key to the synthesis of SACs. In addition, high-temperature pyrolysis can easily aggravate the sintering between metal particles, leading to particle agglomeration (>5nm), so that the nanoparticles in the catalyst have a wider size distribution, lower specific surface area and mass activity. Therefore, we need to select a suitable carrier to stabilize the metal particles. In addition, due to the influence of Fenton reaction, the stability of Fe SACs catalysts is generally poor and will damage the proton exchange membrane.

[0008] Based on the above research, it is necessary to provide a method for preparing a rare earth modified non-precious metal single atom catalyst, which can regulate the electronic structure of the single atom catalyst to ensure that its active sites are fully exposed under a certain density of metal atom loading, while providing layered porosity and improving catalytic activity. Summary of the invention

[0009] The purpose of the present invention is to provide a rare earth modified non-precious metal single atom catalyst and its preparation method and application. The preparation method can regulate the electronic structure of the catalyst to obtain a new catalyst with M-N6 active sites, ensure that the active sites are fully exposed under a certain density of metal atom loading, provide layered porosity, and at the same time, by introducing rare earth oxide nanoparticles and utilizing the characteristics of rare earth elements, reduce the Fenton reaction generated by the metal, and improve the activity and stability of the catalyst.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a method for preparing a rare earth modified non-precious metal single atom catalyst, the preparation method comprising the following steps:

[0012] (1) mixing, drying, performing primary pyrolysis and secondary pyrolysis on a porous carbon support, a transition metal source, an organic ligand and a solvent to obtain an unmodified product;

[0013] (2) Mixing a rare earth source, a solvent and the unmodified product of step (1), drying and carbonizing to obtain the rare earth modified non-precious metal single atom catalyst.

[0014] The present invention adopts a multi-step / three-step pyrolysis method to change the electronic structure in the catalyst, so that the coordination mode of the transition metal is not the traditional M-N4 coordination, but a catalyst with an M-N6 active site is obtained, thereby improving the activity of the catalyst, especially the catalytic activity under acidic conditions; and the present invention uses rare earth modification, the free radical quenching ability of rare earths, the unique oxygen storage and release functions, and the unique 4f orbital and rich valence states of rare earths to effectively reduce the impact of the Fenton reaction, and accurately regulates the electronic structure and local coordination environment of the catalytic material, thereby improving the intrinsic activity, stability and catalytic activity of the catalyst; at the same time, the oxygen affinity of the rare earth elements is used to stabilize the surface oxygen of the porous carbon carrier, inhibit the surface reconstruction of the catalyst during the electrocatalytic process, and thus improve the catalytic stability.

[0015] Preferably, the temperature of the primary pyrolysis in step (1) is 950-1100°C, for example, 950°C, 1000°C or 1100°C, and the time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] Preferably, the atmosphere of the primary pyrolysis in step (1) comprises a protective gas, or a mixed gas of a protective gas and a reducing gas.

[0017] Preferably, the protective gas comprises nitrogen and / or argon, and the reducing gas comprises hydrogen.

[0018] Preferably, when the atmosphere of the primary pyrolysis is a mixture of a protective gas and a reducing gas, the reducing gas accounts for 3-10 vol% of the mixed gas, for example, it can be 3 vol%, 5 vol% or 10 vol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the temperature of the secondary pyrolysis in step (1) is 650-800°C, for example, 650°C, 700°C or 800°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0020] The present invention changes the coordination environment of transition metals through two pyrolysis processes, wherein the first pyrolysis is performed at a higher temperature. On the one hand, at a higher temperature, the volatilization of Zn in the carbon carrier produces a defect anchoring effect. On the other hand, the metal combines with N in the porous carbon carrier to form a coordination bond, which is conducive to the high dispersion of metal atoms. If the temperature of the first pyrolysis is too high, the metals will agglomerate and easily form nanoparticles. If the temperature of the first pyrolysis is too low, ... not only will most of the metals not completely coordinate with N, resulting in a decrease in the amount of metal doping, but also will result in a decrease in the degree of graphitization of the catalyst, which is not conducive to the ORR process; the second pyrolysis is performed at a lower temperature than the first pyrolysis, and the purpose of the second pyrolysis is to dope the N element. If the temperature of the second pyrolysis is too high, the pyrolysis time of the entire process of the second pyrolysis will be long, which will easily lead to the agglomeration of metal atoms, which is not conducive to the high dispersion of metal atoms and reduces the atomic utilization rate; if the temperature of the second pyrolysis is too low, it will be not conducive to the etching of NH3, resulting in a decrease in the N content in the catalyst.

[0021] Preferably, the time of the secondary pyrolysis in step (1) is 10-60 min, for example, 10 min, 20 min, 30 min, 40 min, 50 min or 60 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0022] The time of the secondary pyrolysis of the present invention affects the coordination environment of the transition metal. If the first period of the secondary pyrolysis is too short, on the one hand, the volatilization of Zn will be incomplete, resulting in a decrease in the porosity of the catalyst. On the other hand, the newly introduced metal cannot form coordination with the N in the N-doped carbon carrier well, resulting in a decrease in the metal loading. If the time of the secondary pyrolysis is too long, not only the structure of the carbon carrier is prone to collapse, but also the metal is prone to agglomerate into particles, reducing the utilization rate of atoms.

[0023] Preferably, the atmosphere of the secondary pyrolysis in step (1) comprises NH3.

[0024] Preferably, when the atmosphere of the secondary pyrolysis is a mixed gas of ammonia and a reducing gas, ammonia accounts for 20-100 vol% of the mixed gas, for example, it can be 20 vol%, 40 vol%, 60 vol% or 80 vol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] The present invention uses an ammonia atmosphere or a mixture of ammonia and reducing gas only during the secondary pyrolysis. Through ammonia etching, most of the pyridine nitrogen with a six-membered ring structure in the original nitrogen-doped carbon structure is converted into pyrrole nitrogen with a five-membered ring structure, and finally a high-purity pyrrole-type iron-nitrogen site catalyst is obtained. If both the primary pyrolysis and the secondary pyrolysis are carried out in an ammonia atmosphere, the etching time is too long, which destroys the structure of the catalyst.

[0026] Preferably, the porous carbon carrier in step (1) is prepared by the following method:

[0027] The Zn-ZIF material is calcined in a protective atmosphere to obtain the porous carbon support.

[0028] The porous carbon carrier of the present invention is obtained by calcining Zn-ZIF material. Since the metal Zn volatilizes at high temperature, the obtained porous carbon carrier produces defect anchoring, adsorption and spatial confinement effects, thereby obtaining a nitrogen-containing porous carbon carrier capable of improving catalytic performance.

[0029] Preferably, the calcination temperature is 500-800°C, for example, 500°C, 600°C, 700°C or 800°C, and the calcination time is 1-3h, for example, 1h, 2h or 3h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] The preparation of the carrier is carried out at a relatively low temperature in order to form an N-doped carbon carrier with uniform size distribution and controllable morphology.

[0031] Preferably, the Zn-ZIF material is prepared by the following method: mixing zinc salt, ligand and solvent, and then centrifuging and washing to obtain the Zn-ZIF material.

[0032] Preferably, the molar ratio of zinc ions to ligands in the zinc salt is (1-6):(1-6), for example, 1:6, 1:4, 1:2, 1:1, 2:1, 4:1 or 6:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] Preferably, the molar amount of the zinc salt is 0.005-0.025 mol, for example, 0.005 mol, 0.01 mol, 0.015 mol, 0.02 mol or 0.025 mol, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the stirring rate of the mixed zinc salt, ligand and solvent is 300-960 r / min, for example, 300 r / min, 360 r / min, 420 r / min, 480 r / min, 540 r / min, 600 r / min, 660 r / min, 720 r / min, 780 r / min, 840 r / min, 900 r / min, or 960 r / min, and the time is 3-12 h, for example, 3 h, 5 h, 10 h or 12 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] Preferably, the centrifugation time is 3-5 min, for example, 3 min, 4 min or 5 min, and the rotation speed is 5000-12000 rpm, for example, 5000 rpm, 8000 rpm or 12000 rpm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0036] Preferably, the zinc salt includes any one of ZnSO4·7H2O, Zn(NO3)2·6H2O or ZnCl2, or a combination of at least two thereof.

[0037] Preferably, the ligand is 2-methylimidazole.

[0038] Preferably, the mixing method in step (1) includes ultrasonic dispersion.

[0039] The mixing in step (1) of the present invention comprises first dispersing the porous carbon carrier in deionized water, and then adding the transition metal source and the organic ligand for ultrasonic dispersion.

[0040] Preferably, the ultrasonic dispersion time is 10-60 min, for example, 10 min, 30 min or 60 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, the drying temperature in step (1) is 60-80°C, for example, 60°C, 70°C or 80°C, and the drying time is more than 12 hours, for example, 12 hours, 16 hours or 20 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] In the present invention, step (1) is also preceded by deionized water washing before drying.

[0043] Preferably, the transition metal source in step (1) comprises any one of tetrachlorophenylporphyrin iron, ferric acetylacetonate, ferric chloride, ferrous acetate, ferrous sulfate, ferrous chloride, cobalt acetate, cobalt sulfate, cobalt chloride, nickel chloride, nickel (II) acetate tetrahydrate or nickel nitrate, or a combination of at least two thereof.

[0044] Preferably, the organic ligand in step (1) includes any one or a combination of at least two of EDTA (ethylenediaminetetraacetic acid, aminocarboxyl ligand, 6 coordinating atoms, which can coordinate with almost all metals), dopamine, ethylenediamine, glycine (aminocarboxyl ligand), lactic acid (hydroxycarboxyl biligand), phenoxide ion or 1,10-phenanthroline.

[0045] Preferably, the solvent in step (1) comprises deionized water.

[0046] Preferably, the amount of the rare earth source added in step (2) is 0.5-5wt% of the unmodified product, for example, it can be 0.5wt%, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] The amount of rare earth source added in the present invention will affect the catalytic effect of the catalyst. If the amount added is too little, the electronic structure of the single-atom catalyst cannot be adjusted to improve its catalytic activity. In addition, the free radical quenching ability of too little rare earth is limited, and the effect of reducing the Fenton reaction is not obvious. If the amount added is too much, the particle size of the CeO2 nanoparticles formed is too large, which is not conducive to the full utilization of Ce atoms. In addition, since the Ce element is not a reactive site, the excessive proportion of the Ce element in the overall catalyst is also not conducive to the ORR process.

[0048] Preferably, the rare earth source in step (2) includes any one of cerium (III) acetate hydrate, cerium chloride, hydrated yttrium carbonate, yttrium chloride, lanthanum chloride, lanthanum acetylacetonate, praseodymium chloride, praseodymium acetylacetonate (III) hydrate, neodymium (III) chloride, neodymium (III) acetylacetonate, samarium chloride or samarium (III) acetate hydrate, or a combination of at least two thereof, preferably a cerium source.

[0049] Preferably, the solvent in step (2) comprises any one of deionized water, ethanol, methanol, isopropanol or formamide, or a combination of at least two thereof.

[0050] Preferably, the mixing method in step (2) includes magnetic stirring for 2-5 hours, for example, 2 hours, 3 hours, 4 hours or 5 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0051] Preferably, the drying method in step (2) includes rotary evaporation drying.

[0052] Preferably, the carbonization temperature in step (2) is 500-800°C, for example, 500°C, 600°C, 700°C or 800°C, and the time is 1-4h, for example, 1h, 2h, 3h or 4h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0053] Preferably, the carbonization atmosphere in step (2) comprises a protective gas, or a mixed gas of a protective gas and a reducing gas, wherein the reducing gas accounts for 3-10 vol% of the mixed gas, for example, 3 vol%, 5 vol% or 10 vol%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0054] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps:

[0055] (1) mixing a zinc salt, a ligand and a solvent, and then centrifuging and washing to obtain the Zn-ZIF material, and calcining the Zn-ZIF material in a protective atmosphere to obtain a porous carbon support;

[0056] (2) ultrasonically dispersing the transition metal source, the organic ligand, the solvent and the porous carbon support of step (1) for 10-60 min, then drying at 60-80° C. for more than 12 h, and then pyrolyzing at 950-1100° C. for 1-3 h in a protective gas or a mixed atmosphere of a protective gas and a reducing gas, and pyrolyzing at 650-800° C. for 10-60 min in an NH3 atmosphere to obtain an unmodified product;

[0057] (3) subjecting a rare earth source, a solvent and the unmodified product of step (2) to magnetic stirring for 2-5 hours, then subjecting the mixture to rotary evaporation drying, and then carbonizing the mixture in a protective gas or a mixture of a protective gas and a reducing gas at a temperature of 500-800° C. for 1-4 hours to obtain the rare earth modified non-precious metal single atom catalyst;

[0058] The rare earth source is added in an amount of 0.5-5 wt % of the unmodified product.

[0059] In a second aspect, the present invention provides a rare earth modified non-precious metal single atom catalyst, wherein the rare earth modified non-precious metal single atom catalyst is prepared by the preparation method described in the first aspect.

[0060] In a third aspect, the present invention provides a fuel cell, comprising the rare earth modified non-precious metal single atom catalyst as described in the second aspect.

[0061] Compared with the prior art, the present invention has the following beneficial effects:

[0062] (1) The present invention loads transition metal single atoms on a porous carbon carrier and modifies it with rare earth elements to obtain a catalyst with higher catalytic activity than commercial Pt / C. The catalyst has excellent stability and good application prospects.

[0063] (2) The synthesis process of the present invention is precise, and the structure of the synthesized rare earth modified atomically dispersed catalyst is clear, which can realize the modification of different sites of different RE elements on the carbon support loaded with transition metal single atoms;

[0064] (3) The present invention utilizes the unique 4f orbital and rich valence states of rare earths to site-specifically modify the carbon support loaded with transition metal single atoms derived from ZIF-8, which can accurately regulate the electronic structure and local coordination environment of the catalytic material and improve the intrinsic activity of the catalyst; the oxygen affinity of rare earth elements is utilized to stabilize the surface oxygen of the unmodified product, inhibit the surface reconstruction of the catalyst during the electrocatalytic process, and thus improve its catalytic stability;

[0065] (4) ORR onset potential (E) of the rare earth modified non-precious metal single atom catalyst obtained in the present invention under acidic conditions onset ) can reach above 1.0.V, and the half-wave potential (E 1 / 2 ) can reach above 0.8V (vs.RHE). BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 This is a spherical aberration electron microscope image of the rare earth modified non-precious metal single atom catalyst described in Example 1 of the present invention at a scale of 100 nm;

[0067] Figure 2 This is a spherical aberration electron microscopy image of the rare earth modified non-precious metal single atom catalyst described in Example 1 of the present invention at a scale of 2 nm;

[0068] Figure 3 The XRD diagram of the rare earth modified non-precious metal single atom catalyst described in Example 1 of the present invention and the XRD diagram of standard CeO2;

[0069] Figure 4 It is an LSV curve diagram of the rare earth modified non-precious metal single atom catalyst described in Example 1 of the present invention, the Pt / C catalyst of Comparative Example 1, and the non-precious metal single atom catalyst of Comparative Example 2 in 0.5M H2SO4 solution. DETAILED DESCRIPTION

[0070] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0071] Example 1

[0072] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst, the preparation method comprising the following steps:

[0073] (1) dissolving zinc salt and 2-methylimidazole in methanol, ultrasonically dispersing them uniformly, and then magnetically stirring them at a speed of 600 r / min for 6 hours, wherein the molar amount of the zinc salt is 0.01 mol, and the molar ratio of zinc ions in the zinc salt to 2-methylimidazole is 1:4, and then centrifuging for 4 minutes, and then washing and collecting to obtain the Zn-ZIF material, and calcining the Zn-ZIF material at a temperature of 650° C. for 1 hour in an argon atmosphere to obtain a porous carbon carrier;

[0074] The zinc salt is ZnCl2;

[0075] (2) dispersing the porous carbon support described in step (1) in deionized water, then adding ferrous chloride and an organic ligand 1,10-phenanthroline, performing ultrasonic dispersion for 20 minutes, washing with deionized water, and then drying at 60°C for 14 hours, and then performing a primary pyrolysis at a temperature of 1000°C for 1 hour in argon gas, and a secondary pyrolysis at a temperature of 800°C for 30 minutes in an NH3 atmosphere to obtain an unmodified product;

[0076] (3) ultrasonically dispersing the unmodified product of step (2) in deionized water, then adding a rare earth source, magnetically stirring for 4 hours, then rotary drying, and then carbonizing at 700° C. for 2 hours in an argon atmosphere to obtain the rare earth modified non-precious metal single atom catalyst;

[0077] The rare earth source is added in an amount of 4 wt% of the unmodified product; the rare earth source is cerium (III) acetate hydrate;

[0078] The spherical aberration electron microscopy images of the rare earth modified non-precious metal single atom catalyst described in this example at 0.5 μm scale and 2 nm scale are as follows: Figure 1 and Figure 2 As shown, the XRD patterns of the rare earth modified non-precious metal single atom catalyst and the standard CeO2 are shown in Figure 3 As shown, the LSV curve of the rare earth modified non-precious metal single atom catalyst in 0.5MH2SO4 solution is as follows Figure 4 shown.

[0079] Example 2

[0080] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst, the preparation method comprising the following steps:

[0081] (1) dissolving zinc salt and 2-methylimidazole in methanol, ultrasonically dispersing them uniformly, and then magnetically stirring them at a speed of 300 r / min for 12 hours, wherein the molar amount of the zinc salt is 0.025 mol, and the molar ratio of zinc ions in the zinc salt to the ligand is 1:1, and then centrifuging for 3 minutes, and then washing and collecting to obtain the Zn-ZIF material, and calcining the Zn-ZIF material at a temperature of 500° C. for 3 hours in a nitrogen atmosphere to obtain a porous carbon support;

[0082] The zinc salt is ZnCl2;

[0083] (2) dispersing the porous carbon support described in step (1) in deionized water, then adding ferric acetylacetonate and 1,10-phenanthroline, performing ultrasonic dispersion for 60 minutes, washing with deionized water, and then drying at 80° C. for 12 hours, and then pyrolyzing at 1100° C. for 1 hour in a mixed gas of hydrogen and argon (wherein hydrogen accounts for 5 vol%), and pyrolyzing at 650° C. for 60 minutes in an NH3 atmosphere to obtain an unmodified product;

[0084] (3) ultrasonically dispersing the unmodified product of step (2) in deionized water, then adding a rare earth source, magnetically stirring for 2 h, then rotary drying, and then carbonizing at 500° C. for 4 h in an argon atmosphere to obtain the rare earth modified non-precious metal single atom catalyst;

[0085] The added amount of the rare earth source is 0.5wt% of the unmodified product; the rare earth source is yttrium chloride.

[0086] Example 3

[0087] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst, the preparation method comprising the following steps:

[0088] (1) dissolving zinc salt and 2-methylimidazole in methanol, uniformly dispersing by ultrasonication, and then magnetically stirring at a speed of 960 r / min for 3 h, wherein the molar amount of zinc salt is 0.005 mol, and the molar ratio of zinc ions in the zinc salt to ligands is 1:6, and then centrifuging for 5 min, and then washing and collecting to obtain the Zn-ZIF material, and calcining the Zn-ZIF material at a temperature of 800° C. for 1 h in a nitrogen atmosphere to obtain a porous carbon support;

[0089] The zinc salt is Zn(NO3)2·6H2O;

[0090] (2) dispersing the porous carbon support described in step (1) in deionized water, then adding ferric chloride and EDTA, performing ultrasonic dispersion for 10 minutes, washing with deionized water, and then drying at 60°C for 12 hours, and then performing a primary pyrolysis at a temperature of 950°C for 3 hours in an argon atmosphere, and a secondary pyrolysis at a temperature of 800°C for 10 minutes in an NH3 atmosphere to obtain an unmodified product;

[0091] (3) ultrasonically dispersing the unmodified product of step (2) in deionized water, then adding a rare earth source, magnetically stirring for 5 h, then rotary drying, and then carbonizing in a mixed gas of hydrogen and argon (wherein hydrogen accounts for 3 vol%) at a temperature of 800° C. for 1 h to obtain the rare earth modified non-precious metal single atom catalyst;

[0092] The added amount of the rare earth source is 5wt% of the unmodified product, and the rare earth source is cerium (III) acetate hydrate.

[0093] Example 4

[0094] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the atmosphere for the primary pyrolysis in step (2) is an NH3 atmosphere.

[0095] Example 5

[0096] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the temperature of the first pyrolysis in step (2) is 850°C.

[0097] Example 6

[0098] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the temperature of the first pyrolysis in step (2) is 1200°C.

[0099] Example 7

[0100] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the atmosphere for the secondary pyrolysis in step (2) is a pure argon atmosphere.

[0101] Example 8

[0102] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the temperature of the secondary pyrolysis in step (2) is 600°C.

[0103] Example 9

[0104] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the temperature of the secondary pyrolysis in step (2) is 900°C.

[0105] Example 10

[0106] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the time for the secondary pyrolysis in step (2) is 5 minutes.

[0107] Embodiment 11

[0108] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the time for the secondary pyrolysis in step (2) is 80 minutes.

[0109] Example 12

[0110] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the amount of rare earth source added in step (3) is 0.1 wt%.

[0111] Embodiment 13

[0112] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Embodiment 1 except that the amount of rare earth source added in step (3) is 8 wt %.

[0113] Embodiment 14

[0114] This embodiment provides a method for preparing a rare earth modified non-precious metal single atom catalyst. The preparation method is the same as that of Example 1 except that step (1) is not performed and the porous carbon carrier of step (2) is replaced with a commercial carbon carrier BP-2000.

[0115] Comparative Example 1

[0116] This comparative example provides a commercial Pt / C catalyst, wherein the content of Pt is 20wt%;

[0117] The loading of the Pt / C catalyst in this comparative example is 0.2 mg cm -2 The LSV curve in 0.5M H2SO4 solution is as follows Figure 4 shown.

[0118] Comparative Example 2

[0119] This comparative example provides a method for preparing a non-precious metal single-atom catalyst, which is the same as Example 1 except that step (3) is not performed;

[0120] The LSV curve of the catalyst in 0.5M H2SO4 solution is as follows: Figure 4 shown.

[0121] Comparative Example 3

[0122] This comparative example provides a method for preparing a rare earth modified non-precious metal single-atom catalyst. The preparation method is the same as Example 1 except that step (2) does not involve secondary pyrolysis.

[0123] Comparative Example 4

[0124] This comparative example provides a method for preparing a rare earth modified non-precious metal single-atom catalyst. The preparation method is the same as Example 1 except that step (2) does not involve a single pyrolysis step.

[0125] Comparative Example 5

[0126] This comparative example provides a method for preparing a rare earth modified non-precious metal single atom catalyst, which is the same as Example 1 except that in step (2), the first pyrolysis and the second pyrolysis are not performed, but the pyrolysis is performed at 500°C for 2h in a nitrogen atmosphere.

[0127] The catalysts obtained in the above examples and comparative examples were tested for ORR starting potential, half-wave potential and electrochemical stability. The test conditions were: scanning voltage 0.2-1.05 V (vs. RHE), scanning rate 5 mV / s, and the mass of the catalyst added to the glassy carbon electrode was 0.8 mg / cm 2 .

[0128] The test results are shown in Table 1:

[0129] Table 1

[0130]

[0131]

[0132] From Table 1, we can see the following points:

[0133] (1) The catalyst obtained by the present invention has excellent catalytic performance under acidic conditions and high stability. Figure 1 It can be seen that the catalyst of the present invention has an obvious dodecahedral structure and a particle size of about 100 nm. Figure 2 Obvious lattice fringes can be seen, corresponding to the crystal planes of rare earth oxides; in addition, from the spherical aberration electron microscope Figure 2It can be seen that a large number of single atoms are densely distributed in the catalyst. Figure 3 The XRD analysis results show that the catalyst has obvious CeO2 diffraction peaks, indicating the successful introduction of Ce. Figure 4 It can be seen that the catalyst obtained by the present invention has good electrochemical ORR activity.

[0134] (2) It can be seen from Example 1 and Comparative Examples 1-2 that the catalyst obtained by the present invention has higher catalytic activity than commercial platinum-carbon catalysts and catalysts not modified with rare earths; it can be seen from Example 1 and Comparative Examples 3-5 that the pyrolysis process of the present invention can change the coordination environment of the transition metal, and no catalyst with Fe-N6 active sites can be obtained without primary pyrolysis and secondary pyrolysis, or pyrolysis under conventional conditions, so the performance of the catalyst obtained in Comparative Examples 3-5 decreases; it can be seen from Example 1 and Examples 4-11 that the atmosphere and temperature of the primary pyrolysis of the present invention, as well as the atmosphere, temperature and time of the secondary pyrolysis, will affect the performance of the catalyst; it can be seen from Example 1 and Examples 12-13 that the addition amount of the rare earth source will affect the modification effect of the rare earth, thereby affecting the performance of the catalyst; it can be seen from Example 1 and Example 14 that the carbon carrier prepared by the Zn-ZIF material of the present invention can provide adsorption, anchoring and spatial confinement, thereby facilitating the change of the electronic structure and coordination environment of the catalyst.

[0135] In summary, the present invention provides a rare earth modified non-precious metal single atom catalyst and a preparation method and application thereof. The preparation method can regulate the electronic structure of the catalyst to obtain a new catalyst with M-N6 active sites, thereby ensuring that the active sites are fully exposed under a certain density of metal atom loading, providing layered porosity, and at the same time, by introducing rare earth oxide nanoparticles and utilizing the characteristics of rare earth elements, the Fenton reaction produced by the metal is reduced, thereby improving the activity of the catalyst.

[0136] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a rare earth modified non-precious metal single atom catalyst, characterized in that: The preparation method comprises the following steps: (1) mixing, drying, performing primary pyrolysis and secondary pyrolysis on a porous carbon support, a transition metal source, an organic ligand and a solvent to obtain an unmodified product; (2) Mixing a rare earth source, a solvent and the unmodified product of step (1), drying and carbonizing to obtain the rare earth modified non-precious metal single atom catalyst.

2. The preparation method according to claim 1, characterized in that: The temperature of the primary pyrolysis in step (1) is 950-1100° C. and the time is 1-3 h; Preferably, the atmosphere of the primary pyrolysis in step (1) comprises a protective gas, or a mixed gas of a protective gas and a reducing gas; Preferably, the temperature of the secondary pyrolysis in step (1) is 650-800°C; Preferably, the secondary pyrolysis time in step (1) is 10-60 min; Preferably, the atmosphere of the secondary pyrolysis in step (1) comprises NH3.

3. The preparation method according to claim 1 or 2, characterized in that: The porous carbon carrier in step (1) is prepared by the following method: In a protective atmosphere, calcining the Zn-ZIF material to obtain the porous carbon support; Preferably, the calcination temperature is 500-800°C and the time is 1-3h; Preferably, the Zn-ZIF material is prepared by the following method: mixing zinc salt, ligand and solvent, and then centrifuging and washing to obtain the Zn-ZIF material.

4. The preparation method according to any one of claims 1 to 3, characterized in that The mixing method in step (1) includes ultrasonic dispersion; Preferably, the ultrasonic dispersion time is 10-60 min; Preferably, the drying temperature in step (1) is 60-80° C. and the drying time is more than 12 hours.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The transition metal source in step (1) comprises any one of tetrachlorophenylporphyrin iron, ferric acetylacetonate, ferric chloride, ferrous acetate, ferrous sulfate, ferrous chloride, cobalt acetate, cobalt sulfate, cobalt chloride, nickel chloride, nickel acetate tetrahydrate or nickel nitrate, or a combination of at least two thereof; Preferably, the organic ligand in step (1) comprises any one or a combination of at least two of EDTA, dopamine, ethylenediamine, glycine, lactic acid, phenoxide ion or 1,10-phenanthroline; Preferably, the solvent in step (1) comprises deionized water.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The amount of the rare earth source added in step (2) is 0.5-5wt% of the unmodified product; Preferably, the rare earth source in step (2) comprises any one of cerium acetate hydrate, cerium chloride, hydrated yttrium carbonate, yttrium chloride, lanthanum chloride, lanthanum acetylacetonate, praseodymium chloride, praseodymium acetylacetonate hydrate, neodymium chloride, neodymium acetylacetonate, samarium chloride or samarium acetate hydrate, or a combination of at least two thereof; Preferably, the solvent in step (2) comprises any one of deionized water, ethanol, methanol, isopropanol or formamide, or a combination of at least two thereof.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The mixing method in step (2) includes magnetic stirring for 2-5 hours; Preferably, the drying method in step (2) includes rotary evaporation drying; Preferably, the carbonization temperature in step (2) is 500-800° C. and the time is 1-4 h; Preferably, the carbonization atmosphere in step (2) comprises a protective gas, or a mixture of a protective gas and a reducing gas.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) mixing a zinc salt, a ligand and a solvent, and then centrifuging and washing to obtain the Zn-ZIF material, and calcining the Zn-ZIF material in a protective atmosphere to obtain a porous carbon support; (2) ultrasonically dispersing the transition metal source, the organic ligand, the solvent and the porous carbon support of step (1) for 10-60 minutes, then drying at 60-80° C. for more than 12 hours, and then pyrolyzing at 950-1100° C. for 1-3 hours in a protective gas or a mixed atmosphere of a protective gas and a reducing gas, and then pyrolyzing at 650-800° C. for 10-60 minutes in an NH3 atmosphere to obtain an unmodified product; (3) subjecting a rare earth source, a solvent and the unmodified product of step (2) to magnetic stirring for 2-5 hours, then subjecting the mixture to rotary evaporation drying, and carbonizing the mixture at a temperature of 500-800° C. for 1-4 hours in a protective gas or a mixture of a protective gas and a reducing gas to obtain the rare earth modified non-precious metal single atom catalyst; The rare earth source is added in an amount of 0.5-5 wt % of the unmodified product.

9. A rare earth modified non-precious metal single atom catalyst, characterized in that: The rare earth modified non-precious metal single atom catalyst is prepared by the preparation method described in any one of claims 1 to 8.

10. A fuel cell, characterized in that: The fuel cell comprises the rare earth modified non-precious metal single atom catalyst as claimed in claim 9.

Citation Information

Cited By

  • CoCe-SNC catalyst as well as preparation method and application thereof

    CN120914267A

  • Monatomic iron-loaded granular active carbon composite material as well as preparation method and application thereof

    CN120920041A

  • A granular activated carbon composite material loaded with single-atom iron, its preparation method and its application

    CN120920041B