Sulfide all-solid-state electrolyte membrane material and preparation method thereof

Through hot press-crosslinking technology, polymer molecules are filled in the all-solid electrolyte membrane to form a seepage network structure, which solves the problem of insufficient mechanical strength of the electrolyte membrane, significantly improves the safety and performance stability of the battery, and is a fully solid battery. Industrialization provides an effective path.

CN119069778AInactive Publication Date: 2024-12-03GUIZHOU MATERIAL IND TECH INSTITUE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411207750.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing all-solid electrolyte membranes have insufficient mechanical strength and are easily pierced by lithium dendrites, which affects the safety and performance stability of the battery.

Method used

Through hot press-crosslinking technology, polymer molecules are filled between sulfide particles to form a seepage network structure, enhancing the mechanical strength of the electrolyte membrane. The specific steps include mixing the sulfide electrolyte and the polymer binder ball mill, pre-pressing to form a thin film-like composite material, spraying the crosslinking agent and performing hot pressing treatment.

Benefits of technology

It significantly enhances the mechanical strength of the electrolyte membrane, alleviates the instability of lithium negative electrode materials, and provides an effective solution for the industrialization of all-solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069778A_ABST
    Figure CN119069778A_ABST
Patent Text Reader

Abstract

The invention discloses a sulfide all-solid-state electrolyte membrane material and a preparation method thereof, and belongs to the technical field of high polymer materials. The method comprises the following steps: step 1, uniformly mixing sulfide electrolyte and a polymer binder through ball milling, and then pre-pressing to obtain a film-shaped prefabricated composite material; 2, uniformly spraying a cross-linking agent on the surface of the prefabricated composite material; and 3, carrying out hot pressing on the composite material sprayed with the cross-linking agent to obtain the sulfide all-solid-state electrolyte membrane material. Compared with the prior art, the preparation method has the following beneficial effects that polymer molecules are filled among sulfide particles through hot pressing-crosslinking on the surface of the prefabricated composite material to form a seepage network structure, so that the mechanical strength of an electrolyte membrane is enhanced, and the instability of a lithium negative electrode material is relieved; and an effective thought is provided for realizing industrialization of the all-solid-state battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a sulfide all-solid electrolyte membrane material and a preparation method thereof. Background Art

[0002] All-solid-state lithium batteries are regarded as the development direction of the next generation of energy storage batteries. By using a non-flammable solid electrolyte layer to replace the low-ignition-point organic electrolyte in traditional lithium-ion batteries, the safety performance of lithium batteries can be greatly improved. At the same time, they can also be matched with lithium metal negative electrodes to achieve higher energy density and further develop the application potential of lithium batteries. Solid electrolytes are the core components of all-solid-state lithium batteries. Sulfide solid electrolytes have the advantages of high ionic conductivity and high ductility, and are an important research and development direction for all-solid-state batteries in the future.

[0003] Thinner electrolyte membranes can achieve higher energy density in batteries, thereby improving the performance advantages of all-solid-state batteries. However, existing all-solid-state electrolyte membranes have insufficient mechanical strength. When used as intermediate electrolyte materials, their thin thickness inevitably leads to a decrease in their mechanical strength. During high-voltage cycles, they are easily pierced by lithium dendrites, causing a short circuit between the positive and negative electrodes, which seriously affects the safety and performance stability of the battery. Summary of the invention

[0004] The purpose of an embodiment of the present invention is to provide a sulfide all-solid-state electrolyte membrane material and a preparation method thereof, which fills polymer molecules between sulfide particles through hot pressing-crosslinking to form a percolation network structure, thereby enhancing the mechanical strength of the electrolyte membrane and alleviating the instability of the lithium negative electrode material, thereby solving at least one technical problem involved in the background technology.

[0005] In order to solve the above-mentioned technical problems, the present invention is achieved as follows:

[0006] The embodiment of the present invention provides a method for preparing a sulfide all-solid-state electrolyte membrane material, comprising the following steps:

[0007] Step 1, mixing the sulfide electrolyte and the polymer binder uniformly by ball milling, and then pre-pressing to obtain a film-like prefabricated composite material;

[0008] Step 2, spraying a cross-linking agent uniformly on the surface of the prefabricated composite material;

[0009] Step three, hot pressing the composite material sprayed with the cross-linking agent to obtain a sulfide all-solid-state electrolyte membrane material.

[0010] Optionally, in step 1, the ball milling speed is 50-250 rpm and the time is 20-60 min.

[0011] Optionally, in step 1, the mass ratio of the sulfide electrolyte to the polymer binder is 100:(5-0.1).

[0012] Optionally, in step one, the polymer binder is thermoplastic polyamide.

[0013] Optionally, in step 1, the sulfide electrolyte is one or a combination of LiPSCl and LiSiPSCl.

[0014] Optionally, in step 2, the cross-linking agent is selected from glycidol, epichlorohydrin, and 2,3-epoxypropyltrimethylammonium chloride.

[0015] Optionally, in step three, the hot pressing temperature is 120-140 degrees Celsius, the pressure is 5 MPa, and the time is 2-10 minutes.

[0016] The present invention also provides a sulfide all-solid electrolyte membrane material, which is prepared by adopting the preparation method.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] By hot pressing and cross-linking on the surface of the prefabricated composite material, polymer molecules are filled into the space between sulfide particles to form a percolation network structure, which enhances the mechanical strength of the electrolyte membrane, alleviates the instability of the lithium negative electrode material, and provides an effective idea for the industrialization of all-solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:

[0020] Figure 1 The present invention provides a flow chart of a method for preparing a sulfide all-solid-state electrolyte membrane material. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] See also Figure 1As shown, an embodiment of the present invention provides a method for preparing a sulfide all-solid-state electrolyte membrane material, comprising the following steps:

[0023] Step S1, mixing the sulfide electrolyte and the polymer binder uniformly by ball milling, and then pre-pressing to obtain a film-shaped prefabricated composite material;

[0024] The polymer binder is thermoplastic polyamide; the sulfide electrolyte is one or a combination of LiPSCl (argentum sulfide solid electrolyte) and LiSiPSCl (lithium silicon phosphorus sulfur chlorine electrolyte). The mass ratio of the sulfide electrolyte to the polymer binder is 100:(5-0.1).

[0025] The ball milling speed is 50-250 rpm and the time is 20-60 min.

[0026] Step S2, spraying a cross-linking agent uniformly on the surface of the prefabricated composite material;

[0027] Wherein, the cross-linking agent is selected from glycidol, epichlorohydrin, and 2,3-epoxypropyltrimethylammonium chloride.

[0028] Step S3, hot pressing the composite material sprayed with the cross-linking agent to obtain a sulfide all-solid electrolyte membrane material.

[0029] Among them, the hot pressing temperature is 120-140 degrees Celsius, the pressure is 5Mpa, and the time is 2-10min.

[0030] The present invention also provides a sulfide all-solid electrolyte membrane material, which is prepared by adopting the preparation method.

[0031] The preparation method of the sulfide all-solid electrolyte membrane material provided by the present invention is described in detail below with reference to Examples 1-3.

[0032] Example 1

[0033] Embodiment 1 provides a method for preparing a sulfide all-solid-state electrolyte membrane material, comprising the following steps:

[0034] Step S1, weighing 10.1 g of 99 wt% LiPSCl solid electrolyte and 0.2 g of 1 wt% thermoplastic polyamide;

[0035] Step S2, weighing the raw materials in step S1 and mixing them evenly by ball milling at a ball milling rate of 220 rpm for 18 min, then heating to 130 degrees Celsius, and rolling for multiple times to form a dense film with a thickness of 50 μm;

[0036] Step S3, spraying propylene oxide evenly on the dense film;

[0037] Step S4, hot pressing the dense film sprayed with propylene oxide at a temperature of 140 degrees Celsius and a pressure of 5 MPa for 10 minutes to obtain a sulfide all-solid electrolyte membrane material.

[0038] Example 2

[0039] Embodiment 2 provides a method for preparing a sulfide all-solid-state electrolyte membrane material, comprising the following steps:

[0040] Step S1, weighing 9.0 g of 99 wt% LiSiPSCl solid electrolyte and 0.1 g of 1 wt% thermoplastic polyamide;

[0041] Step S2, weighing the raw materials in step S1 and mixing them evenly by ball milling at a ball milling rate of 250 rpm for 15 min, then heating to 130 degrees Celsius, and rolling them multiple times to form a dense film with a thickness of 50 μm;

[0042] Step S3, spraying epichlorohydrin uniformly on the dense film;

[0043] Step S4, hot pressing the dense film sprayed with epichlorohydrin at a temperature of 130 degrees Celsius and a pressure of 5 MPa for 8 minutes to obtain a sulfide all-solid electrolyte membrane material.

[0044] Example 3

[0045] Embodiment 3 provides a method for preparing a sulfide all-solid-state electrolyte membrane material, comprising the following steps:

[0046] Step S1, weighing 9.5 g of 99 wt% LiPSCl solid electrolyte and 0.15 g of 1 wt% thermoplastic polyamide;

[0047] Step S2, weighing the raw materials in step S1 and mixing them evenly by ball milling at a ball milling rate of 230 rpm for 17 min, then heating to 130 degrees Celsius, and rolling for multiple times to form a dense film with a thickness of 50 μm;

[0048] Step S3, spraying 2,3-epoxypropyltrimethylammonium chloride uniformly on the dense film;

[0049] Step S4, hot pressing the dense film sprayed with 2,3-epoxypropyltrimethylammonium chloride at a temperature of 120 degrees Celsius and a pressure of 5 MPa for 10 minutes to obtain a sulfide all-solid electrolyte membrane material.

[0050] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0051] In addition, it should be noted that the scope of the methods and systems in the embodiments of the present invention is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved. For example, the described methods may be performed in an order different from that described, and various steps may be added, omitted, or combined. In addition, features described with reference to certain examples may be combined in other examples.

[0052] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.

Claims

1. A method for preparing a sulfide all-solid electrolyte membrane material, characterized in that: The steps include: Step 1, mixing the sulfide electrolyte and the polymer binder uniformly by ball milling, and then pre-pressing to obtain a film-like prefabricated composite material; Step 2, spraying a cross-linking agent uniformly on the surface of the prefabricated composite material; Step three, hot pressing the composite material sprayed with the cross-linking agent to obtain a sulfide all-solid-state electrolyte membrane material.

2. The preparation method according to claim 1, characterized in that: In step 1, the ball milling speed is 50-250 rpm and the time is 20-60 min.

3. The preparation method according to claim 1 or 2, characterized in that: In step 1, the mass ratio of the sulfide electrolyte to the polymer binder is 100:(5-0.1).

4. The preparation method according to claim 3, characterized in that: In step 1, the polymer binder is thermoplastic polyamide.

5. The preparation method according to claim 4, characterized in that: In step 1, the sulfide electrolyte is one or a combination of LiPSCl and LiSiPSCl.

6. The preparation method according to claim 1, characterized in that: In step 2, the cross-linking agent is selected from glycidol, epichlorohydrin, and 2,3-epoxypropyltrimethylammonium chloride.

7. The preparation method according to claim 1, characterized in that: In step three, the hot pressing temperature is 120-140 degrees Celsius, the pressure is 5 MPa, and the time is 2-10 minutes.

8. A sulfide all-solid electrolyte membrane material, characterized in that: The preparation method is described in any one of claims 1 to 7.

Citation Information

Patent Citations

  • Sulfide electrolyte slurry, and preparation method and application thereof

    CN109786845A

  • Preparation method of ionic conductor / polyoxyethylene composite solid electrolyte based on ultraviolet crosslinking

    CN111313089A

  • Composite electrolyte membrane for all-solid-state lithium metal battery as well as preparation method and application of composite electrolyte membrane

    CN118281309A

  • Air-stable sulfide all-solid-state electrolyte membrane material and preparation method thereof

    CN118712471A