Electrolyte additive, non-aqueous electrolyte and lithium ion battery
By using electrolyte additives with specific structures in lithium-ion batteries, the SEI film rich in phosphorus and Si-C is formed, which solves the performance problems of lithium-ion batteries at high and low temperatures, and improves the stability and cycle life of the battery. .
Patent Information
- Application Number
- CN202410952435.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-03
AI Technical Summary
The electrolyte is unstable in high-temperature environments, resulting in side reactions and interface mask decomposition, and the electrolyte ion conduction capacity decreases in low-temperature environments, affecting battery performance and cycle life.
Develop an electrolyte additive with a specific structure that can form a SEI film rich in phosphorus and Si-C in lithium-ion batteries, reduce interface impedance, capture HF, reduce electrode metal ions dissolution, and enhance battery high and low temperatures. performance.
It significantly improves the high-temperature storage and circulation performance of lithium-ion batteries, enhances the low-temperature discharge capacity, expands the working temperature range, and improves safety and stability.
Smart Images

Figure CN119069800A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ion batteries, and in particular to an electrolyte additive, a non-aqueous electrolyte and a lithium ion battery. Background Art
[0002] As a secondary electrochemical energy storage device, lithium-ion batteries meet people's needs for high-efficiency energy, environmental protection and low energy consumption. With its advantages of high potential, high energy, long cycle life, wide temperature operation, no memory effect, and environmental friendliness, it is widely used in digital, power, energy storage, aviation and other fields.
[0003] However, the expansion of application fields has put forward higher requirements for lithium-ion batteries. For example, when lithium-ion batteries are used in aerospace equipment, vehicles, ships and other equipment, their high temperature and low temperature resistance are facing challenges. In high temperature environments, a series of problems such as electrolyte instability, violent side reactions between electrolytes and electrode materials, and decomposition of solid electrolyte interface films are serious safety hazards faced by lithium-ion batteries in high temperature environments. Specifically, the commonly used electrolyte lithium hexafluorophosphate is chemically and thermodynamically unstable, easily decomposes to produce hydrofluoric acid, corrodes the electrolyte interface film and causes the dissolution of electrode transition metal ions, which is not conducive to the performance of lithium-ion batteries. At the same time, PF5 generated by electrolyte decomposition easily attacks the lone pair electrons on the oxygen atoms in the organic solvent, resulting in the ring-opening polymerization and ether bond breakage of the organic solvent. This reaction is particularly serious at high temperatures, deteriorating the battery storage performance and cycle performance. In low temperature environments, the ion conductivity of the electrolyte decreases, which increases the internal resistance of the battery. The existence of internal resistance leads to the loss of battery capacity at high rate currents, which is not conducive to the cycle life of the battery. Therefore, it is particularly important to improve the thermal stability and electrochemical performance of lithium-ion batteries at high and low temperatures. People have also proposed some solutions, such as optimizing electrolyte formula, material coating and element doping, etc. Among them, the electrolyte is one of the most important components in lithium-ion batteries, and its stability is directly related to the performance of lithium-ion batteries. Therefore, developing new electrolyte additives is the most effective and cost-effective method.
[0004] Based on this, how to develop a new additive that can regulate the interaction between the electrode and the electrolyte and stabilize the electrolyte so that the final lithium-ion battery can have both high temperature resistance and low temperature resistance is one of the important technical problems that need to be solved in this field. Summary of the invention
[0005] The main purpose of the present invention is to provide an electrolyte additive, a non-aqueous electrolyte and a lithium ion battery to solve the problem that the high temperature storage performance, high temperature cycle performance and low temperature discharge performance of lithium ion battery electrolyte in the prior art are poor.
[0006] In order to achieve the above object, the first aspect of the present invention provides an electrolyte additive having a structure shown in the following formula I:
[0007]
[0008] Wherein, R1, R2, R3, R4, and R5 are each independently selected from a substituted or unsubstituted C1-C5 straight-chain or branched hydrocarbon group, a substituted or unsubstituted C6-C10 aryl group, a cyano group, or a C1-C5 cyano hydrocarbon group.
[0009] Furthermore, R1 and R2 are each independently selected from a C1-C4 straight chain or branched hydrocarbon group, a cyano group or a C1-C5 cyano hydrocarbon group, and R3, R4, and R5 are each independently selected from a C1-C4 straight chain or branched hydrocarbon group, a substituted or unsubstituted C6-C8 aromatic group.
[0010] Furthermore, the straight-chain or branched hydrocarbon group of C1 to C5 is any one of the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, vinyl, propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, and 1-methyl-2-butenyl; the aryl group of C6 to C10 is phenyl; and the cyano hydrocarbon group of C1 to C5 is any one of the group consisting of methylcyano, ethylcyano, propionyrano, and benzylcyano.
[0011] Furthermore, when the C1-C5 straight-chain or branched hydrocarbon group or the C6-C10 aryl group has a substituent, the substituents each independently include halogen; preferably, the substituents each independently are fluorine.
[0012] Furthermore, R1 and R2 are each independently selected from any one of ethyl, cyano, vinyl and tert-butyl, and R3, R4 and R5 are each independently selected from any one of methyl, ethyl, vinyl, tert-butyl, trifluoromethyl, phenyl and fluorophenyl.
[0013] Furthermore, the electrolyte additive has a structure shown in any one of the following structural formulas 1 to 5:
[0014]
[0015] The second aspect of the present invention provides a non-aqueous electrolyte comprising a lithium salt and an organic solvent. The non-aqueous electrolyte also includes at least one of the above-mentioned electrolyte additives, and the mass fraction of the electrolyte additive in the non-aqueous electrolyte is 0.1% to 4%, preferably 0.1% to 2.5%.
[0016] Further, the lithium salt is selected from one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium trifluoromethanesulfonate, lithium methylsulfonate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, lithium difluoro(dioxalato)phosphate, lithium tetrafluoroborate, lithium tetrafluoro(oxalato)phosphate, lithium bis(trifluoromethanesulfonyl)imide, and lithium bis(fluorosulfonyl)imide; preferably lithium hexafluorophosphate; preferably, the mass fraction of the lithium salt in the non-aqueous electrolyte is 6% to 25%, more preferably 10% to 20%.
[0017] Further, the organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, butylene carbonate, methyl acetate, ethyl acetate, propyl acetate, propyl propionate, γ-butyrolactone, 1,3-dioxolane, crown ether, dimethoxymethane, diethoxymethane, ethoxymethoxymethane, and fluorinated ethylene carbonate; preferably, the mass fraction of the organic solvent in the non-aqueous electrolyte is 65% to 85%.
[0018] Further, the non-aqueous electrolyte further includes an additive, and the additive is selected from one or more of vinylene carbonate, vinylidene ethylene carbonate, fluorinated ethylene carbonate, 1,3-propane sultone, ethylene sulfate, 1,4-butane sultone, maleic anhydride, 2-methylmaleic anhydride, methylene methanedisulfonate, tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphate, adiponitrile, succinonitrile, 1,3,6-hexanetricarbonitrile, and triallyl phosphate; preferably, the additive is selected from one or more of vinylene carbonate, fluorinated ethylene carbonate, and 1,3-propane sultone.
[0019] Further, the mass fraction of the additive in the non-aqueous electrolyte is 0.1% to 4%.
[0020] The third aspect of the present invention provides a lithium-ion battery, including a positive electrode, a negative electrode, and an electrolyte, and the electrolyte is the above-mentioned non-aqueous electrolyte.
[0021] Further, the positive electrode includes a positive electrode material, and the positive electrode material is selected from one or more of lithium cobaltate, lithium manganate, lithium iron phosphate, and lithium nickel cobalt manganese oxide, and the molecular formula of lithium nickel cobalt manganese oxide is LiNi x Co y Mn (1-x-y) O2, where 0.5 < x < 0.9, x + y ≤ 1; preferably, the positive electrode material is a ternary material of lithium nickel cobalt manganate LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0022] Further, the negative electrode includes a negative electrode material, and the negative electrode material is selected from one or more of graphite, hard carbon, lithium titanate, and silicon-carbon composite materials, preferably artificial graphite.
[0023] By applying the technical solution of the present invention, a new compound is provided as an electrolyte additive, thereby effectively reducing the interface impedance and improving the low-temperature performance of the battery. At the same time, the additive can effectively capture HF, reduce its damage to the SEI membrane active electrode, reduce the dissolution of electrode metal ions, and improve the high-temperature storage and cycle performance of lithium-ion batteries. DETAILED DESCRIPTION
[0024] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.
[0025] As described in the background art, the prior art has the problem that the high temperature storage performance, high temperature cycle performance and low temperature discharge performance of lithium ion battery electrolyte are all poor. In order to solve the above technical problems, the first aspect of the present invention provides an electrolyte additive having a structure shown in the following formula I:
[0026]
[0027] Wherein, R1, R2, R3, R4, and R5 are each independently selected from a substituted or unsubstituted C1-C5 straight-chain or branched hydrocarbon group, a substituted or unsubstituted C6-C10 aryl group, a cyano group, or a C1-C5 cyano hydrocarbon group.
[0028] The compound with the above structure, when used as an electrolyte additive in the operation of lithium-ion batteries, can preferentially form a thin, uniform and dense SEI film rich in phosphorus and Si-C at the positive electrode, thereby effectively reducing the interface impedance and improving the low-temperature performance of the battery. At the same time, the compound can effectively capture HF in the electrolyte of the lithium-ion battery, reduce the damage of HF to the active electrode of the SEI film, reduce the dissolution of electrode metal ions, and thus improve the storage and cycle performance of the lithium-ion battery.
[0029] Furthermore, when R1 and R2 are each independently selected from a straight chain or branched hydrocarbon group of C1 to C4, a cyano group or a cyano hydrocarbon group of C1 to C5, and R3, R4, and R5 are each independently selected from a straight chain or branched hydrocarbon group of C1 to C4, a substituted or unsubstituted aromatic group of C6 to C8, the corresponding compounds obtained, when used as additives in battery electrolytes, exhibit more significant high temperature storage resistance, cycle performance, and better low temperature resistance.
[0030] In several preferred embodiments, the straight chain or branched hydrocarbon group of C1 to C5 is any one of the groups consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, vinyl, propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, and 1-methyl-2-butenyl; the aryl group of C6 to C10 is phenyl; the cyano hydrocarbon group of C1 to C5 is any one of the groups consisting of methyl cyano, ethyl cyano, propionyl cyano, and benzyl cyano. After a large number of experiments, the inventors have selected these specific groups in the above range, and found that when the structure in the above formula I includes these groups, the resulting compound can more effectively make the electrolyte containing it show chemical stability and long cycle characteristics.
[0031] In the actual application process, the inventors found through a large number of experiments that when a special halogen-containing group is introduced into the additive, a SEI film containing LiX (X is a halogen) can be formed at the negative electrode, thereby significantly reducing the low-temperature impedance of the negative electrode interface film, so that the corresponding electrolyte exhibits better low-temperature resistance. Therefore, further, the present invention preferably includes halogens when there are substituents in the straight or branched hydrocarbon group of C1 to C5 and the aromatic group of C6 to C10. More preferably, after a large number of experiments and comparisons, the inventors preferably select fluorine as the substituents, and found that the electrolyte additive obtained at this time not only makes the low-temperature discharge of the obtained lithium-ion battery higher, but also can be better compatible with other additives that can be added to the electrolyte, thereby further improving the cycle stability of the battery.
[0032] Furthermore, in order to optimize the electron cloud structure in the compound of formula I, the inventors have conducted a large number of experiments and have preferably selected R1 and R2 connected to the P-containing group from any one of ethyl, cyano, vinyl and tert-butyl, and R3, R4 and R5 connected to the Si-containing group from any one of methyl, ethyl, vinyl, tert-butyl, trifluoromethyl, phenyl and fluorophenyl. It is found that the compounds obtained at this time, when used as electrolyte additives, can more effectively form an interface film containing P and Si-C, thereby making the final lithium-ion battery more resistant to low temperatures.
[0033] In several preferred embodiments, the electrolyte additive has a structure shown in any one of the following structural formulas 1 to 5:
[0034]
[0035] After a large number of experiments, the inventors selected the above-mentioned compounds with specific structures and applied them as additives to the electrolyte for lithium-ion batteries. The resulting lithium-ion batteries have significantly improved high and low temperature resistance, a larger operating temperature range, and higher safety and stability.
[0036] The compound 1 provided by the present invention is a known synthetic compound with a CAS number of 757-44-8. The synthetic routes of compound 2, compound 3, compound 4, compound 5 and compound 6 are shown below. According to the synthetic routes below, the above compounds 2 to 6 can be prepared by the synthetic methods commonly used in the art for phosphoryl-containing silane compounds.
[0037]
[0038]
[0039] The second aspect of the present invention provides a non-aqueous electrolyte, comprising a lithium salt and an organic solvent, the non-aqueous electrolyte further comprising at least one of the above-mentioned electrolyte additives, and the mass fraction of the electrolyte additive in the non-aqueous electrolyte is 0.1% to 4%, preferably 0.1% to 2.5%. The non-aqueous electrolyte can make the lithium-ion battery in which it is located have good high-temperature storage performance and high-temperature cycle performance, while taking into account the low-temperature discharge performance of -20°C.
[0040] As mentioned above, the compound having the structure of formula I prepared by the present invention can be preferentially oxidized in an organic system, thereby forming a thin, uniform and dense interface film rich in P elements and Si-C on the surface of the positive electrode of the battery; at the same time, the Si-O and Si-C bonds in its structure can capture HF in the electrolyte, effectively protecting the stability of the interface film. Therefore, when it is used as an additive in the electrolyte, it can reduce the occurrence of side reactions between the electrolyte and the electrode, and at the same time improve the intrinsic chemical stability of the electrolyte, so that it has a wider operating temperature range and a longer service life. In particular, the inventors have conducted a large number of experiments and have found that the mass fraction of the electrolyte additive in the non-aqueous electrolyte is 0.1% to 4%, more preferably 0.1% to 2.5%, and specifically 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.3%, 1.5%, 1.7%, 1.9%, 2.0%, 2.2%, 2.5%, but are not limited to the listed values, and other values not listed in this numerical range are also applicable. The inventors have conducted a large number of experiments and found that within this dosage range, the above-mentioned compound additives in the prepared non-aqueous electrolyte can more effectively exert various performances, thereby further maintaining the stability of the electrode structure and improving the high temperature storage, cycle performance, and low temperature discharge of the lithium-ion battery.
[0041] In several preferred embodiments, the lithium salt is selected from one or more of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium trifluoromethanesulfonate (LiCF3SO3), lithium methanesulfonate (LiCH3SO3), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium difluorobis(oxalatophosphate) (LiPF2(C2O4)2), lithium tetrafluoroborate (LiBF4), lithium tetrafluorooxalatophosphate (LiPF4(C2O4)), lithium bis(trifluoromethylsulfonyl imide) (LiN(SO2CF3)2) and lithium bis(fluorosulfonyl imide) (LiN(SO2F)2); preferably lithium hexafluorophosphate. In several more preferred embodiments, the mass fraction of the lithium salt in the non-aqueous electrolyte is 6% to 25%. The inventor has optimized the content of the lithium salt through a large number of experiments, so as to better match the type and amount of the above-mentioned compound additives, and more effectively improve the chemical stability and high and low temperature resistance of the obtained electrolyte. More preferably, the mass fraction of the lithium salt in the non-aqueous electrolyte is 10% to 20%, specifically 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, so as to more significantly improve the electrochemical performance of the lithium-ion battery on the basis of better coordination with the additive.
[0042] Further, the organic solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), butylene carbonate (BC), methyl acetate (MA), ethyl acetate (EA), propyl acetate (EP), propyl propionate (PP), γ-butyrolactone (GBL), 1,3-dioxolane (DOL), crown ether (CE), dimethoxymethane, diethoxymethane, ethoxymethoxymethane and fluoroethylene carbonate (FEC). In a preferred embodiment, the organic solvent is a mixed solvent of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate, and the weight ratio of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in the mixed solvent is 1: (1-2): (1-2). Theoretically, the organic solvent can be selected from the types commonly used in the art, but the inventor has selected the above-mentioned specific organic solvent composition through a large number of experiments, and found that the electrolyte system obtained based on the solvent system and the obtained formula I compound additive can be better adapted, so that the obtained non-aqueous electrolyte exhibits higher high temperature and low temperature resistance. In order to further improve the electrochemical performance of the obtained non-aqueous electrolyte, preferably, the mass fraction of the organic solvent in the non-aqueous electrolyte is 65% to 85%, specifically 65%, 68%, 70%, 73%, 75%, 78%, 80%, 82%, 83%, 84%, 85%, but not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0043] Further, the non-aqueous electrolyte also includes an auxiliary agent, and the auxiliary agent is selected from one or more of vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, 1,4-butane sultone, maleic anhydride, 2-methylmaleic anhydride, methylene disulfonate, tris(trimethylsilyl) borate, tris(trimethylsilyl) phosphate, adiponitrile, succinonitrile, 1,3,6-hexane trinitrile and tripropargyl phosphate. The inventor has found through a large number of experiments that the above-mentioned auxiliary agent can be matched with the additive of the compound of formula I to form a stable solid electrolyte interface film on the surface of the positive and negative active materials where it is located, inhibiting the oxidative decomposition of the electrolyte on the positive electrode surface, effectively blocking the direct contact between the electrode and the electrolyte, reducing the consumption of the electrolyte and the damage of the electrode material, reducing the dissolution of transition metal ions inside the electrode and depositing them on the surface, stabilizing the electrode structure, thereby further improving the high temperature performance and low temperature performance of the battery. Preferably, the auxiliary agent is selected from one or more of vinylene carbonate, fluoroethylene carbonate and 1,3-propane sultone. The inventors further optimized the auxiliary agent types through a large number of experiments, obtained these three and their corresponding combinations, and found that they have higher compatibility with the additive of the compound of formula I, thereby being able to more significantly improve the chemical stability and high temperature and low temperature resistance of the obtained electrolyte.
[0044] In order to more effectively improve the comprehensive performance of the non-aqueous electrolyte, the inventors have, after a large number of experiments, preferably selected the mass fraction of the additive in the non-aqueous electrolyte to be 0.1% to 4%, specifically 0.1%, 0.5%, 1.0%, 1.5%, 1.9%, 2.0%, 2.5%, 3.0%, 3.5%, 3.6%, 3.8%, and 4.0%, but are not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] In several preferred embodiments, the non-aqueous electrolyte comprises, by weight percentage, 0.5% of compound 2, 0.5% of VC, 0.5% of PS, 14% of LiPF6, and 84.5% of solvent, and EC / EMC / DEC in the solvent is (1:2:2), and the structural formula of compound 2 is shown below; or, by weight percentage, the non-aqueous electrolyte comprises 0.5% of compound 3, 0.5% of VC, 0.5% of PS, 14% of LiPF6, and 84.5% of solvent, and EC / EMC / DEC in the solvent is (1:2:2), and the structural formula of compound 3 is shown below:
[0046]
[0047]
[0048] The third aspect of the present invention provides a lithium-ion battery, which includes a positive electrode, a negative electrode, and an electrolyte, and the electrolyte is the above-mentioned non-aqueous electrolyte. The obtained lithium-ion battery has excellent performance, especially showing good high-temperature and low-temperature resistance, high capacity retention rate after high-temperature cycling, excellent capacity retention rate and recovery rate after high-temperature storage, and can also show a high discharge rate in a low-temperature environment of -20°C.
[0049] Further, the positive electrode includes a positive electrode material, and the positive electrode material is selected from one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, and lithium nickel cobalt manganese oxide. The molecular formula of lithium nickel cobalt manganese oxide is LiNi x Co y Mn (1-x-y) O2, where 0.5 < x < 0.9 and x + y ≤ 1. Through a large number of experiments, the inventor preferably selects the positive electrode material as the ternary material lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2, and the obtained lithium-ion battery has higher electrical performance.
[0050] Further, the negative electrode includes a negative electrode material, and the negative electrode material is selected from one or more of graphite, hard carbon, lithium titanate, and silicon-carbon composite materials. The preferred negative electrode material is artificial graphite, so as to better match the above non-aqueous electrolyte system and improve the cycle stability.
[0051] The following further describes the present application in detail with specific embodiments, and these embodiments should not be construed as limiting the scope claimed by the present application.
[0052] Unless otherwise defined, all professional terms used hereinafter have the same meaning as commonly understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the protection scope of the present invention.
[0053] Example 1
[0054] Preparation of a non-aqueous electrolyte for a lithium-ion battery:
[0055] 1. Preparation of electrolyte additives:
[0056] Compound 1 (CAS 757-44-8) is used as the electrolyte additive, and its structure is as follows:
[0057]
[0058] 2. Preparation of non-aqueous electrolyte: In a glove box filled with argon (O2 <1ppm, H2O <1ppm), ethylene carbonate (EC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC) were mixed in a mass ratio of 1:2:2 as an organic solvent, and then the additive compound 1 was added. After sufficient mixing, lithium hexafluorophosphate and an auxiliary agent vinylene carbonate (VC) were added, and the non-aqueous electrolyte was obtained after mixing. The addition amount of each component is shown in Table 1.
[0059] Example 2
[0060] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0061] 1. Preparation of electrolyte additive: same as in Example 1.
[0062] 2. Preparation of non-aqueous electrolyte: Compound 1 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the components added were different, as shown in Table 1.
[0063] Example 3
[0064] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0065] 1. Preparation of electrolyte additive: same as in Example 1.
[0066] 2. Preparation of non-aqueous electrolyte: Compound 1 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the components added were different, as shown in Table 1.
[0067] Example 4
[0068] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0069] 1. Preparation of electrolyte additives:
[0070]
[0071] Compound 2 was prepared according to the above synthetic route, and its structure is:
[0072]
[0073] 2. Preparation of non-aqueous electrolyte: Compound 2 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the components added were different, as shown in Table 1.
[0074] Example 5
[0075] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0076] 1. Preparation of electrolyte additives:
[0077]
[0078] Compound 3 was prepared according to the above synthetic route, and its structure is:
[0079]
[0080] 2. Preparation of non-aqueous electrolyte: Compound 3 was used as an electrolyte additive, and the same preparation method as in Example 1 was adopted, but the amounts of the added components were different, as shown in Table 1.
[0081] Example 6
[0082] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0083] 1. Preparation of electrolyte additives:
[0084]
[0085] Compound 4 was prepared according to the above synthetic route, and its structure is:
[0086]
[0087] 2. Preparation of non-aqueous electrolyte: Compound 4 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the components added were different, as shown in Table 1.
[0088] Example 7
[0089] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0090] 1. Preparation of electrolyte additives:
[0091]
[0092] Compound 5 was prepared according to the above synthetic route, and its structure is:
[0093]
[0094] 2. Preparation of non-aqueous electrolyte: Compound 5 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the components added were different, as shown in Table 1.
[0095] Example 8
[0096] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0097] 1. Preparation of electrolyte additives:
[0098]
[0099] Compound 6 was prepared according to the above synthetic route, and its structure is:
[0100]
[0101] 2. Preparation of non-aqueous electrolyte: Compound 6 was used as an electrolyte additive and the same preparation method as in Example 1 was adopted, but the amounts of the added components were different, as shown in Table 1.
[0102] Example 9
[0103] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0104] 1. Preparation of electrolyte additive: same as in Example 1.
[0105] 2. Preparation of non-aqueous electrolyte: Compound 1 was used as an electrolyte additive, and the same preparation method as in Example 1 was adopted, but the amounts of the added components were different, as shown in Table 1 (the amount of VC was reduced, and the additive FEC was additionally added).
[0106] Example 10
[0107] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0108] 1. Preparation of electrolyte additive: same as in Example 1.
[0109] 2. Preparation of non-aqueous electrolyte: Compound 1 was used as an electrolyte additive, and the same preparation method as in Example 1 was adopted, but the amounts of the added components were different, as shown in Table 1 (the amount of VC was reduced, and the auxiliary agent PS was additionally added).
[0110] Embodiment 11
[0111] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0112] The only difference between this embodiment and embodiment 10 is that compound 2 is first prepared according to the method in embodiment 4, and an equal weight of compound 2 is used to replace compound 1 in the non-aqueous electrolyte.
[0113] Example 12
[0114] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0115] The only difference between this embodiment and embodiment 10 is that compound 3 is first prepared according to the method in embodiment 5, and an equal weight of compound 3 is used to replace compound 1 in the non-aqueous electrolyte.
[0116] Embodiment 13
[0117] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0118] The only difference between this embodiment and embodiment 1 is that the amount of compound 1 added to the non-aqueous electrolyte is 0.05 g instead of 0.5 g.
[0119] Embodiment 14
[0120] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0121] The only difference between this embodiment and embodiment 1 is that the amount of compound 1 added to the non-aqueous electrolyte is 4.5 g instead of 0.5 g.
[0122] Embodiment 15
[0123] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0124] The only difference between this embodiment and embodiment 1 is that in the organic solvent added to the non-aqueous electrolyte, the mass ratio of ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) is 2:1:1, and the total amount of organic solvent remains unchanged.
[0125] Example 16
[0126] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0127] The only difference between this embodiment and embodiment 1 is that the mass ratio of the organic solvents, ethylene carbonate (EC), propyl propionate (PP), and dimethyl carbonate (DMC) added to the non-aqueous electrolyte is 1:2:2, and the total amount added remains unchanged.
[0128] Comparative Example 1
[0129] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0130] The only difference between this comparative example and Example 1 is that compound 1 is not added. The specific components are shown in Table 1.
[0131] Comparative Example 2
[0132] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0133] The difference between this comparative example and Example 1 is that compound 1 is not added, and VC is replaced by an equal weight of FEC. The specific components are shown in Table 1.
[0134] Comparative Example 3
[0135] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0136] The only difference between this comparative example and Example 9 is that compound 1 is not added. The specific components are shown in Table 1.
[0137] Comparative Example 4
[0138] Preparation of a non-aqueous electrolyte for lithium-ion batteries:
[0139] The difference between this comparative example and Example 1 is that the compound 1 in the non-aqueous electrolyte is replaced by an equal weight of a compound with CAS No. 24630-67-9, the structure of which is as follows:
[0140]
[0141] Test Method
[0142] (1) Preparation of lithium-ion batteries:
[0143] Positive electrode: LiNi 0.8 Co 0.1 Mn 0.1 O2 material, adhesive PVDF and conductive agent SuperP are dispersed and mixed in a mass ratio of 94.5%:1.5%:4%, and NMP is used as a solvent to uniformly prepare a positive electrode slurry for a lithium-ion battery with a certain viscosity. The mixed slurry is uniformly coated on both sides of an aluminum foil, and then dried, rolled and die-cut to obtain a positive electrode sheet.
[0144] Negative electrode: artificial graphite, conductive agent SuperP, thickener CMC, binder SBR are dispersed and mixed in a mass ratio of 94.5%:1.5%:1.5%:2.5%, and deionized water is used as a solvent to uniformly prepare a lithium-ion battery negative electrode slurry with a certain viscosity. The mixed slurry is evenly coated on both sides of the copper foil, and then dried, rolled and die-cut to obtain a negative electrode sheet;
[0145] Battery assembly: The positive electrode, separator and negative electrode are stacked to form a square soft-pack battery cell, which is packaged with a polymer aluminum-plastic film and filled with the lithium-ion battery non-aqueous electrolyte prepared in the above embodiments and comparative examples. After the steps of formation and capacity separation, a lithium-ion battery with a capacity of 3000mAh is prepared.
[0146] (2) Performance test of lithium-ion batteries:
[0147] High temperature cycle performance test: Place the lithium-ion battery in a 45°C constant temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge it at a constant current of 1C to a voltage of 4.4V, then charge it at a constant voltage of 4.4V to a current of 0.05C, then discharge it at a constant current of 1C to a voltage of 3.0V, and record the first discharge capacity of the battery as C0. This is a charge and discharge cycle. Then, perform 400 cycles of 1C / 1C charge and discharge at 45°C, and record the discharge capacity as C1. Calculate the capacity retention rate = (C1 / C0)*100%;
[0148] High temperature storage performance test: Lithium-ion batteries are charged to 4.4V at 0.5C constant current at 25°C, then charged at constant voltage until the current drops to 0.05C, and then discharged at 0.5C constant current to 3.0V, recording the discharge capacity at this time as C0. Then charge the battery to 4.4V at 0.5C constant current, and then charge at constant voltage until the current drops to 0.05C. Then place the battery in a 60°C constant temperature oven for 30 days and take it out. After the battery is placed in a 25°C environment for 24h, it is discharged to 3.0V at 0.5C constant current at 25°C, recording the discharge capacity at this time as C1, and then charged to 4.4V at 0.5C constant current, then charged at constant voltage to a cut-off current of 0.05C, and discharged to 3.0V at 0.5C constant current. Record the discharge capacity at this time as C2. Calculate capacity retention rate = C1 / C0*100%; capacity recovery rate = C2 / C0*100%;
[0149] Low temperature discharge performance test: Lithium-ion battery is charged to 4.4V at 0.5C constant current at 25℃, then charged at constant voltage until the current drops to 0.05C, then discharged to 3.0V at 0.5C constant current, and the discharge capacity at this time is recorded as C0. Then the battery is charged to 4.4V at 0.5C constant current, and the battery is placed in a -20℃ low temperature constant temperature box for 4 hours, and then discharged to 3.0V at 0.5C constant current, and the discharge capacity at this time is recorded as C1. Calculate the low temperature discharge rate = (C1 / C0)*100%.
[0150] The test results are shown in Table 2.
[0151] Table 1
[0152]
[0153]
[0154] Table 2
[0155]
[0156]
[0157] It can be seen from the test results in Table 2 that, compared with the comparative examples, the lithium-ion batteries obtained in the embodiments have better high-temperature cycle performance, high-temperature storage performance and low-temperature discharge performance due to the use of the additive containing a special structure prepared by the present invention in the electrolyte. Since the additive can be preferentially oxidized in lithium-ion batteries, a thin, uniform and dense interface film rich in P elements and Si-C is formed on the surface of the positive electrode, which helps to reduce the internal resistance of the interface, improve the lithium ion transmission efficiency, and improve the low-temperature performance of the battery. The Si-O and Si-C bonds in the additive compound can capture HF in the electrolyte, effectively protect the stability of the interface film, reduce the occurrence of side reactions between the electrolyte and the electrode, and further maintain the stability of the electrode structure, thereby improving the high-temperature storage and high-temperature cycle performance of the battery.
[0158] From the comparison between Example 2 and Example 4 and Example 5, it can be seen that compared with Compound 1, Compound 2 forms a LiF / LiO-containing SEI film at the negative electrode. The LiF / LiO interface is a fast channel for lithium ion transmission, which can reduce the impedance of the negative electrode interface film at low temperatures, effectively increase the lithium ion diffusion rate, and improve low-temperature discharge performance. The fluorophenyl group introduced by Compound 3 effectively increases the wetting effect of the electrolyte on the electrode material, reduces the concentrated polarization internal resistance of the electrode, and further improves the capacity retention rate of the battery after high-temperature cycling.
[0159] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those described herein, for example.
[0160] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An electrolyte additive, characterized in that: The electrolyte additive has a structure shown in the following formula I: Wherein, R1, R2, R3, R4, and R5 are each independently selected from a substituted or unsubstituted C1-C5 straight-chain or branched hydrocarbon group, a substituted or unsubstituted C6-C10 aryl group, a cyano group, or a C1-C5 cyano hydrocarbon group.
2. The electrolyte additive according to claim 1, characterized in that: R1 and R2 are each independently selected from a C1-C4 straight chain or branched hydrocarbon group, a cyano group or a C1-C5 cyano hydrocarbon group, and R3, R4, and R5 are each independently selected from a C1-C4 straight chain or branched hydrocarbon group, a substituted or unsubstituted C6-C8 aromatic group.
3. The electrolyte additive according to claim 1 or 2, characterized in that: The straight-chain or branched hydrocarbon group of C1 to C5 is any one of the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, vinyl, propenyl, 1-butenyl, 2-butenyl, 3-butenyl, 1-pentenyl, and 1-methyl-2-butenyl; the aromatic group of C6 to C10 is phenyl; the cyano hydrocarbon group of C1 to C5 is any one of the group consisting of methylcyano, ethylcyano, propionylano, and benzylcyano.
4. The electrolyte additive according to any one of claims 1 to 3, characterized in that When the C1-C5 straight or branched hydrocarbon group and the C6-C10 aryl group have substituents, the substituents independently include halogens; Preferably, the substituents are each independently fluorine.
5. The electrolyte additive according to any one of claims 1 to 4, characterized in that R1 and R2 are each independently selected from any one of ethyl, cyano, vinyl and tert-butyl, and R3, R4 and R5 are each independently selected from any one of methyl, ethyl, vinyl, tert-butyl, trifluoromethyl, phenyl and fluorophenyl.
6. The electrolyte additive according to claim 1, characterized in that: The electrolyte additive is any one of the following compounds 1 to 5:
7. A non-aqueous electrolyte comprising a lithium salt and an organic solvent, characterized in that: The non-aqueous electrolyte further comprises at least one of the electrolyte additives described in any one of claims 1 to 6, and the mass fraction of the electrolyte additive in the non-aqueous electrolyte is 0.1% to 4%, preferably 0.1% to 2.5%.
8. The non-aqueous electrolyte according to claim 7, characterized in that The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium trifluoromethylsulfonate, lithium methanesulfonate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium tetrafluorooxalatophosphate, lithium bis(trifluoromethylsulfonylimide) and lithium bis(fluorosulfonylimide); preferably lithium hexafluorophosphate; Preferably, the mass fraction of the lithium salt in the non-aqueous electrolyte is 6% to 25%, more preferably 10% to 20%.
9. The non-aqueous electrolyte according to claim 7 or 8, characterized in that The organic solvent is selected from one or more of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl carbonate, butylene carbonate, methyl acetate, ethyl acetate, propyl acetate, propyl propionate, γ-butyrolactone, 1,3-dioxolane, crown ether, dimethoxymethane, diethoxymethane, ethoxymethoxymethane and fluoroethylene carbonate; Preferably, the mass fraction of the organic solvent in the non-aqueous electrolyte is 65% to 85%.
10. The non-aqueous electrolyte according to any one of claims 7 to 9, characterized in that The non-aqueous electrolyte also includes an auxiliary agent, and the auxiliary agent is selected from one or more of vinylene carbonate, vinylene carbonate, fluoroethylene carbonate, 1,3-propane sultone, vinyl sulfate, 1,4-butane sultone, maleic anhydride, 2-methylmaleic anhydride, methylene methanedisulfonate, tris(trimethylsilyl)borate, tris(trimethylsilyl)phosphate, adiponitrile, succinonitrile, 1,3,6-hexanetrinitrile and tripropargyl phosphate; Preferably, the auxiliary agent is selected from one or more of vinylene carbonate, fluoroethylene carbonate and 1,3-propane sultone.
11. The non-aqueous electrolyte according to claim 10, characterized in that The mass fraction of the auxiliary agent in the non-aqueous electrolyte is 0.1% to 4%.
12. A lithium ion battery comprising a positive electrode, a negative electrode and an electrolyte, characterized in that: The electrolyte is the non-aqueous electrolyte according to any one of claims 7 to 11.
13. The lithium ion battery according to claim 12, characterized in that: The positive electrode includes a positive electrode material, and the positive electrode material is selected from one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate and lithium nickel cobalt manganese oxide, and the molecular formula of the lithium nickel cobalt manganese oxide is LiNi x Co y Mn (1-x-y) O2, of which 0.5 <x<0.9,x+y≤1; Preferably, the positive electrode material is a ternary material of lithium nickel cobalt manganese oxide LiNi 0.8 Co 0.1 Mn 0.1 O2.
14. The lithium ion battery according to claim 12 or 13, characterized in that: The negative electrode includes a negative electrode material, and The negative electrode material is selected from one or more of graphite, hard carbon, lithium titanate and silicon-carbon composite material, preferably artificial graphite.