Lithium ion battery non-aqueous electrolyte and lithium ion battery

By using a non-aqueous electrolyte containing lithium salts, non-aqueous organic solvents and silicon polynitrile compounds in lithium-ion batteries, the reaction problem of positive electrode materials and negative electrode materials at high voltage is solved, and a stable SEI film is formed, which significantly improves the The battery cycle and storage performance are achieved.

CN119069803APending Publication Date: 2024-12-03ZHANGJIAGANG HUASHENG CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411206605.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

At high voltage, the reaction of Co3+/4+ and O2- in the positive electrode material of lithium-ion batteries and the SEI film rupture and side reaction caused by the expansion of silicon-based negative electrode material affects the circulation and storage performance of the battery.

Method used

Using a nonaqueous electrolyte containing lithium salt, non-aqueous organic solvent and silicon-containing polynitrile compound, the silicon-containing polynitrile compound has a silicon body structure and a cyano group, which can complex cobalt ions on the positive electrode side and inhibit its activity. , and a high conductivity and tough SEI film is formed on the negative electrode side to avoid rupture of the SEI film.

Benefits of technology

The circulation and storage performance of lithium-ion batteries is significantly improved, especially under ultra-high voltage systems, which reduces the side reactions of the positive electrode materials and the structural instability of the negative electrode materials, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069803A_ABST
    Figure CN119069803A_ABST
Patent Text Reader

Abstract

The invention relates to a lithium ion battery non-aqueous electrolyte and a lithium ion battery. The non-aqueous electrolyte comprises a lithium salt, a non-aqueous organic solvent and an additive, the additive is a silicon-containing polynitrile compound, the silicon-containing polynitrile compound is one or more of a compound 1 and a compound with a chemical structural formula 1, the chemical structural formula of the compound 1 is # imgabs 0 #, the structural formula 1 is # imgabs 1 #, and Rf is a fluorine atom or fluoroalkyl. On one hand, the electrolyte can be complexed with cobalt ions, so that the side reaction of the positive electrode material is reduced, and the dissolution of cobalt ions and the escape of oxygen free radicals are inhibited; and on the other hand, an SEI film with high conductivity and toughness can be formed on the negative electrode, so that a series of side reactions caused by SEI film rupture due to silicon negative electrode expansion are avoided, and the cycle and storage performance of the battery can be effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery non-aqueous electrolyte and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are widely used because of their high energy density, high charge and discharge efficiency, low self-discharge, long service life and environmental friendliness. They have been applied to consumer electronics, aerospace, military, power tools and electric vehicles. With the development of technology, people have higher and higher requirements for the endurance of lithium-ion batteries in both the consumer field and the power battery field, and the development of high energy density (mass energy density and volume energy density) lithium batteries has become the key. The development of high energy density lithium batteries can start from two aspects. One is to develop new high-gram capacity positive and negative electrode materials; the other is to increase the charge and discharge voltage of lithium batteries. Increasing the charge and discharge voltage of lithium batteries can simultaneously increase the mass energy density and volume energy density of lithium batteries, and can also reduce the cost of lithium batteries, which has become a hot topic of research.

[0003] However, when studying high-voltage lithium batteries, people found that as the voltage of lithium batteries increases, the performance of the battery deteriorates significantly. For example, high-voltage (≥4.5V) lithium cobalt oxide (LCO), when LCO is charged to a voltage above 4.45V, it will undergo a harmful phase transition from the O3 hexagonal phase to the hybrid O1-O3 phase. This process is accompanied by sliding between lattice layers and partial collapse of the O3 lattice structure. Accompanied by the increase in the internal stress of LCO, it further leads to the formation of LCO cracks and particle breakage. In addition, due to the O 2- : The top of the 2p resonance band is related to the low-spin Co 3+ / 4+ :t2g resonance band overlap, so oxygen begins to undergo redox reaction under high voltage. 1- The ion mobility is higher than that of O 2- , O on the LCO surface 1- It is easy to convert into O2 and leave the LCO particles, which will destroy the cathode-electrolyte interface, resulting in interface instability. Therefore, slowing down the interfacial activity of LCO materials under high voltage and slowing down the decomposition of electrolyte will improve the cycle performance and storage performance of lithium-ion batteries under high voltage systems.

[0004] Similarly, when using silicon-based materials as negative electrode materials, there are the following advantages. 1. High theoretical specific capacity: Silicon-based negative electrode materials have extremely high theoretical specific capacity, reaching about 4200mAh / g, which is the highest among currently known materials. This means that in the same volume, silicon-based negative electrodes can store more charge, thereby providing longer battery life. 2. Lower lithium insertion potential: The lithium insertion potential of silicon-based negative electrodes is about 0.3Vvs.Li / Li +, compared with graphite anode (about 0.04Vvs.Li / Li + ) is slightly higher, but still suitable, and can avoid lithium plating on the surface of the material. 3. Safety: Due to the lower lithium insertion and extraction potential, the silicon-based negative electrode can avoid lithium deposition on the surface during charging, thereby reducing the risk of lithium dendrite formation, which helps to improve the overall safety of the battery. However, due to the extremely large expansion rate of silicon-based materials, it has the following disadvantages. 1. Lithium insertion and extraction: During the charging process of silicon-based negative electrode materials, lithium ions will be embedded in silicon atoms, causing the size of silicon atoms to change. When lithium ions are extracted from silicon atoms, these atoms will return to a smaller state, resulting in a volume change. This volume change can reach up to 280%. 2. Structural changes: When the silicon-based negative electrode reacts with lithium, it is not just a simple volume expansion, but also accompanied by changes in the material structure, such as changes in lattice parameters and adjustments in microstructure. 3. Mechanical stress: Due to volume expansion, large mechanical stresses will be generated between silicon particles and between silicon particles and electrode substrates. These stresses may cause the SEI (solid electrolyte interface) film on the surface of silicon particles to be destroyed, thereby affecting the performance and life of the battery. 4. Interface side reactions: During the charge and discharge process, due to the structural instability caused by volume expansion, interface side reactions may occur between the silicon-based negative electrode and the electrolyte, such as the crushing of silicon particles and the formation of unstable solid electrolyte interfaces, which will accelerate the failure of the battery. 5. Cycle stability issues: Long-term charge and discharge cycles will cause the volume expansion of silicon-based negative electrode materials to accumulate, leading to material cracks and even pulverization, ultimately affecting the capacity decay and cycle life of the battery.

[0005] Based on the above problems, in order to improve the battery performance of the high voltage lithium cobalt oxide / graphite composite silicon-based material negative electrode system, it is necessary to focus on solving the Co 3+ / 4+ With O 2- The reaction and the formation of a stable SEI on the graphite composite silicon-based material prevent a series of side reactions caused by the expansion of the silicon-based material. Summary of the invention

[0006] Technical problem to be solved: In view of the shortcomings of the prior art, the present invention provides a non-aqueous electrolyte for lithium-ion batteries and a lithium-ion battery. The electrolyte can improve the cycle and storage performance of the battery, and is particularly suitable for lithium-ion batteries under ultra-high voltage systems.

[0007] Technical solution: A non-aqueous electrolyte for lithium-ion batteries, the non-aqueous electrolyte comprising a lithium salt, a non-aqueous organic solvent and an additive; the additive is a silicon-containing polynitrile compound, the silicon-containing polynitrile compound is one or more of compound 1 and a compound having a chemical formula of structural formula 1,

[0008] The chemical structure of compound 1 is

[0009] Structural formula 1 is wherein Rf is a fluorine atom or a fluorinated alkyl group.

[0010] The compound having the chemical formula 1 is one or both of compound 2 and compound 3.

[0011] The chemical structure of compound 2 is

[0012] The chemical structure of compound 3 is

[0013] The above-mentioned lithium ion battery non-aqueous electrolyte contains the following components by weight: lithium salt: 10-20 parts; non-aqueous organic solvent: 60-80 parts; silicon-containing polynitrile compound: 0.1-5 parts.

[0014] The lithium salt described above is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium tetrafluorooxalatophosphate, lithium bis(trifluoromethylsulfonylimide), lithium bis(fluorosulfonylimide) and lithium 2-fluoromalonate difluoroborate.

[0015] The non-aqueous organic solvent described above is one or more of ethylene carbonate, fluoroethylene carbonate, ethyl difluoroacetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, butyl acetate, γ-butyrolactone, propyl propionate, ethyl propionate, ethyl acetate and ethyl butyrate.

[0016] The non-aqueous electrolyte mentioned above further comprises 0.2 to 15 parts by weight of an auxiliary agent.

[0017] The auxiliary agent described above is one or more of 2,2,2-trifluoromethyl ethyl carbonate, 2,2,2-trifluorodiethyl carbonate, vinylene carbonate, diethyl pyrocarbonate, 1,3-propane sultone, vinyl sulfate, 1,2-difluoroethylene carbonate, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-disulfate vinyl and 4,4-disulfate vinyl.

[0018] A lithium ion battery comprises a positive electrode, a negative electrode and the non-aqueous electrolyte mentioned above.

[0019] The positive electrode material described above is lithium cobalt oxide material, and the negative electrode material is a composite material of graphite and silicon oxide material, wherein the mass percentage of silicon oxide material in the negative electrode material is 3% to 50%.

[0020] The maximum charging voltage of the lithium-ion battery described above is 4.53V.

[0021] Compared with the prior art, the additives of the lithium ion battery non-aqueous electrolyte of the present invention include silicon-containing polynitrile compounds, which have both silicon structure and cyano groups. The cyano group can complex the cobalt ions on the positive electrode side during the formation stage, and it is speculated that the ability to complex cobalt ions is significantly better than the commonly used succinonitrile (SN), adiponitrile (ADN) and 1,3,6-hexanetrinitrile (HTCN). It can more stably complex the cobalt ions, inhibit the activity of cobalt ions, and avoid the Co in the positive electrode material from the root. 3+ / 4+ With O 2- The silicon-containing groups can form Li-rich x Si y O z The SEI film of the components has high ionic conductivity and toughness. It is not easy to break even when the silicon-based material expands. It can better cope with the SEI film rupture caused by mechanical stress when the silicon negative electrode expands, and inhibit the side reaction between the negative electrode material and the electrolyte. The fluorinated sulfonyl group in structural formula 1 can further form a LiF and Li-rich electrolyte at the negative electrode. x S y O z The SEI of the negative electrode can further increase the ionic conductivity and stability of the negative electrode SEI. Therefore, the addition of silicon-containing polynitrile compounds effectively solves the problem of Co in the positive electrode material from the root. 3+ / 4+ With O 2- The reaction leads to the generation of oxygen free radicals and a series of subsequent side reactions, and the stress generated by the expansion of silicon-carbon at the negative electrode leads to SEI rupture and a series of subsequent side reactions. It can significantly improve the cycle performance and storage performance of batteries with lithium cobalt oxide / graphite composite silicon-based material system, and is particularly suitable for batteries under ultra-high voltage systems.

[0022] Beneficial effects: The present invention provides a non-aqueous electrolyte for lithium ion batteries and a lithium ion battery, which have the following beneficial effects: during use, the lithium ion battery prepared using the non-aqueous electrolyte for lithium ion batteries of the present invention can, on the one hand, complex cobalt ions, reduce the side reactions of the positive electrode material, and inhibit the dissolution of cobalt ions and the escape of oxygen free radicals; on the other hand, it can form a high-conductivity, tough SEI film at the negative electrode, avoiding a series of side reactions caused by the rupture of the SEI film due to the expansion of the silicon negative electrode, and can effectively improve the battery's cycle and storage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the synthetic reaction equation of compound 1.

[0024] Figure 2 is the synthetic reaction equation of compound 2. DETAILED DESCRIPTION

[0025] An embodiment of the present invention provides a non-aqueous electrolyte for a lithium ion battery, the non-aqueous electrolyte comprising a lithium salt, a non-aqueous organic solvent and an additive; the additive is a silicon-containing polynitrile compound, the silicon-containing polynitrile compound is compound 1 or a compound having a chemical formula of structural formula 1,

[0026] The chemical structure of compound 1 is

[0027] Structural formula 1 is wherein Rf is a fluorine atom or a fluorinated alkyl group.

[0028] The compounds having the chemical formula of Structural Formula 1 include but are not limited to the following Compound 2, Compound 3 and combinations thereof.

[0029] The chemical structure of compound 2 is

[0030] The chemical structure of compound 3 is

[0031] The synthetic reaction equations of compound 1 and compound 2 are respectively as follows Figure 1 , Figure 2 The synthetic reaction equation of compound 3 is shown in Figure 2.

[0032]

[0033] Replace with (CAS: 421-85-2), and the remaining steps are the same as the synthesis method of compound 2.

[0034] The contents of the lithium salt, the non-aqueous organic solvent and the silicon-containing polynitrile compound are 10 to 20 parts, 60 to 80 parts and 0.1 to 5 parts respectively in parts by mass.

[0035] Preferably, the mass proportion of the silicon-containing polynitrile compound is 0.5 to 3 parts, specifically but not limited to 0.5 parts, 1 part, 2 parts, and 3 parts.

[0036] The mass proportion of the lithium salt is 10 to 20 parts, specifically but not limited to 10 parts, 11 parts, 12 parts, 14 parts, 16 parts, 18 parts, and 20 parts. The lithium salt is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium bisoxalatoborate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, lithium tetrafluoroborate, lithium tetrafluorooxalatophosphate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, and lithium 2-fluoromalonate difluoroborate.

[0037] Preferably, the lithium salt is a mixture of lithium difluorooxalate phosphate and lithium tetrafluorooxalate phosphate, a mixture of lithium hexafluorophosphate and lithium tetrafluoroborate, a mixture of lithium bisoxalate borate and lithium difluorooxalate borate, a mixture of lithium difluorooxalate borate and lithium difluoro oxalate phosphate, a mixture of lithium tetrafluorooxalate phosphate and lithium bistrifluoromethylsulfonyl imide, a mixture of lithium bistrifluoromethylsulfonyl imide and lithium bisfluorosulfonyl imide, a mixture of lithium tetrafluoroborate and lithium difluorophosphate, a mixture of lithium hexafluorophosphate and lithium difluorophosphate, a mixture of lithium bisfluorosulfonyl imide and lithium 2-fluoromalonate difluoroborate, a mixture of lithium 2-fluoromalonate difluoroborate and lithium bisoxalate borate, a mixture of lithium bisoxalate borate, lithium difluorooxalate borate and lithium difluoro oxalate phosphate.

[0038] The mass parts of the non-aqueous electrolyte are 60 to 80 parts, specifically but not limited to 60, 63, 66, 67, 69, 70, 71, 72, 73, 74, 77, and 80 parts. The non-aqueous organic solvent is one or more of ethylene carbonate, fluoroethylene carbonate, ethyl difluoroacetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, butyl acetate, γ-butyrolactone, propyl propionate, ethyl propionate, ethyl acetate, and ethyl butyrate.

[0039] The non-aqueous electrolyte further comprises 0.2 to 15 parts by weight of an auxiliary agent, which is one or more of 2,2,2-trifluoromethyl ethyl carbonate, 2,2,2-trifluorodiethyl carbonate, vinylene carbonate, diethyl pyrocarbonate, 1,3-propane sultone, vinyl sulfate, 1,2-difluoroethylene carbonate, tris(trimethylsilane)phosphate, tris(trimethylsilane)phosphite, 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-disulfate vinyl and 4,4-disulfate vinyl.

[0040] Preferably, the auxiliary agent is vinylene carbonate, 1,3-propane sultone, vinyl sulfate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-ethylene disulfate or 4,4-ethylene disulfate, and the content is 0.2-1.5 parts, 0.1-1.5 parts, 0.2-1.5 parts, 0.3-1.5 parts, 0.2-1.2 parts, 0.2-1.2 parts, 0.2-1.2 parts respectively.

[0041] Among them, vinylene carbonate (VC) has good high and low temperature performance and anti-flatulence function, which can improve the capacity and cycle life of the battery; tri(trimethylsilyl) phosphate and tri(trimethylsilyl) phosphite can adsorb free acid, thereby improving the cycle performance of the battery; 1,3-propane sultone can improve the cycle life and storage stability of the battery; vinyl sulfate can increase the content of sulfur and oxygen elements on the SEI film of the battery, accelerate the shuttle ability of lithium ions on the SEI film through the arc pairs of sulfur atoms and oxygen atoms, reduce the impedance of the SEI film, and thus improve the low-temperature discharge performance of the battery; 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-ethylene disulfate and 4,4-ethylene disulfate can effectively protect the negative electrode, which can not only prevent the reduction of battery capacity at high temperature, but also effectively improve the performance of the battery at low temperature.

[0042] An embodiment of the present invention further provides a lithium-ion battery, which includes a positive electrode, a negative electrode and the non-aqueous electrolyte described above, and the maximum charging voltage is 4.53 V. The positive electrode material is lithium cobalt oxide (including various lithium cobalt oxide materials doped and coated with lithium cobalt oxide as the main body), and the negative electrode material is a composite material of graphite and silicon oxide material, wherein the silicon oxide material accounts for 3% to 50%.

[0043] In order to better illustrate the purpose, technical scheme and beneficial effects of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be noted that the following implementation method is a further explanation of the present invention and should not be used as a limitation of the present invention.

[0044] Example 1

[0045] In order to detect the complexing ability of the electrolyte of the present invention for cobalt ions, bis(trifluoromethylsulfonyl)imide cobalt (Co(TFSI)2) was added during the preparation of the electrolyte in this embodiment. The bis(trifluoromethylsulfonyl)imide cobalt was prepared by reacting bis(trifluoromethylsulfonyl)imide and cobalt hydroxide.

[0046] The preparation process of the electrolyte is as follows:

[0047] In a glove box filled with nitrogen (O2 <1ppm, H2O <2ppm), ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) were mixed uniformly in a mass ratio of 3:3:4 to obtain 85.5g of a non-aqueous organic solvent, and then 500ppm of cobalt bistrifluoromethylsulfonyl imide (Co(TFSI)2) was added, and then 2g of compound 1 was added as an additive to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2h before being taken out. In a glove box filled with nitrogen (O2 <1ppm, H2O <2ppm), 12.5g of lithium hexafluorophosphate was slowly added to the mixed solution, and the electrolyte was prepared after mixing uniformly.

[0048] The preparation methods of Examples 2-3 and Comparative Examples 1-4 are the same as that of Example 1, but the electrolyte formulas are different, as shown in Table 1 below.

[0049] Table 1

[0050]

[0051] The above electrolytes were sealed, stored in a 45% oven for 10 days, and then taken out. The cobalt ion content in each group of electrolytes was tested using a cation chromatograph. The test results are shown in Table 2.

[0052] Table 2

[0053]

[0054]

[0055] As shown in Table 2, the cobalt ion content in the electrolyte of Comparative Examples 1-3 is much lower than that of Comparative Examples 1-4. This is because the additives of the lithium ion battery non-aqueous electrolyte of the present invention include silicon-containing polynitrile compounds, which have both silicon structure and cyano groups. The cyano group can complex the cobalt ions on the positive electrode side during the formation stage, and according to the experimental conclusion, the ability to complex the cobalt ions is significantly better than that of succinonitrile (SN), adiponitrile (ADN) and 1,3,6-hexanetrinitrile (HTCN) commonly used in the system.

[0056] Example 4

[0057] The preparation process of the electrolyte is as follows:

[0058] In a glove box filled with nitrogen (O2 <1ppm, H2O <2ppm), ethylene carbonate (EC), diethyl carbonate (DEC), propyl propionate (PP) and fluoroethylene carbonate (FEC) were mixed in a mass ratio of 2:2:5:1 to obtain 84g of a non-aqueous organic solvent, and 1g of compound 1 was added as an additive to obtain a mixed solution. The mixed solution was sealed and packaged and placed in a quick freezer (-4°C) for 2h before being taken out. In a glove box filled with nitrogen (O2 <1ppm, H2O <2ppm), 15g of lithium hexafluorophosphate was slowly added to the mixed solution, and the electrolyte was obtained after mixing evenly.

[0059] The preparation methods of Examples 4-18 and Comparative Examples 5-8 and Example 4 are the same as Example 1, but the electrolyte formulas are different, as shown in Table 3 below.

[0060] Table 3

[0061]

[0062]

[0063] Lithium cobalt oxide with a maximum charging voltage of 4.53V was used as the positive electrode material, natural graphite composite 20% SiOx was used as the negative electrode material, and the electrolytes of Examples 4 to 18 and Comparative Examples 5 to 8 were used to prepare lithium ion batteries according to the conventional lithium battery preparation method, and the room temperature cycle performance, high temperature cycle performance and high temperature storage performance tests were performed respectively, as follows:

[0064] 1. Normal temperature cycle performance test method

[0065] Place the lithium-ion battery in a 25°C environment, charge it to 4.53V at 1C constant current, then charge it at constant voltage until the current drops to 0.05C, then discharge it to 3.0V at 1C constant current, repeat this cycle, and record the discharge capacity of the first cycle and the discharge capacity of the last cycle. Calculate the capacity retention rate of high temperature cycles according to the following formula.

[0066] Capacity retention rate = discharge capacity of the last cycle / discharge capacity of the first cycle×100%.

[0067] 2. High temperature cycle performance test method

[0068] Place the lithium-ion battery in a 45°C environment, charge it at 1C constant current to 4.53V, then charge it at constant voltage until the current drops to 0.05C, then discharge it at 1C constant current to 3.0V, repeat this cycle, and record the discharge capacity of the first cycle and the discharge capacity of the last cycle. Calculate the capacity retention rate of high temperature cycles according to the following formula.

[0069] Capacity retention rate = discharge capacity of the last cycle / discharge capacity of the first cycle×100%.

[0070] 3. High temperature storage performance test

[0071] Place the lithium-ion battery in an environment of 25°C, charge it to 4.53V at a constant current of 0.5C, then charge it at a constant voltage until the current drops to 0.05C, then discharge it to 3.0V at a constant current of 0.5C, and record the discharge capacity at this time as C1; then charge the battery to 4.53V at a constant current of 0.5C, then charge it at a constant voltage until the current drops to 0.05C, and then place the battery at an extremely high temperature of 85°C for 8 hours, then take out the battery and place it at 25°C for 2 hours, and then discharge it to 3.0V at a constant current of 0.5C, and record the discharge capacity at this time as C2.

[0072] Capacity retention rate = C2 / C1×100%.

[0073] The test results are shown in Table 4 below.

[0074] Table 4

[0075]

[0076] It can be seen from the results in Table 4 that the room temperature cycle performance, high temperature cycle performance, and high temperature storage performance of Examples 4-18 are better than those of Comparative Examples 5-8. This is because the additives of the lithium ion battery non-aqueous electrolyte of the present invention include silicon-containing polynitrile compounds, which have both silicon structure and cyano groups. The cyano group can complex the cobalt ions on the positive electrode side during the formation stage, and according to the experimental conclusions, the ability to complex cobalt ions is significantly improved due to the commonly used succinonitrile (SN), adiponitrile (ADN) and 1,3,6-hexanetrinitrile (HTCN) in the system. It can more stably complex the cobalt ions, inhibit the activity of the cobalt ions, and avoid the Co in the positive electrode material from the root. 3+ / 4+ With O 2- The silicon-containing groups can form Li-rich x Si y O z The SEI film of the components has high ionic conductivity and toughness. It is not easy to break even when the silicon-based material expands. It can better cope with the SEI film rupture caused by mechanical stress when the silicon negative electrode expands, and inhibit the side reaction between the negative electrode material and the electrolyte. The fluorinated sulfonyl group in structural formula 1 can further form a LiF and Li-rich electrolyte at the negative electrode. x S y O z SEI can further increase the ionic conductivity and stability of the negative electrode SEI. Therefore, the addition of silicon-containing polynitrile compounds effectively solves the problem of Co in the positive electrode material from the root. 3+ / 4+ With O 2- The reaction leads to the generation of oxygen free radicals and a series of subsequent side reactions, and the stress generated by the expansion of silicon-carbon at the negative electrode leads to SEI rupture and a series of subsequent side reactions. It can significantly improve the cycle performance and storage performance of batteries with lithium cobalt oxide / graphite composite silicon-based material system, and is particularly suitable for batteries under ultra-high voltage systems.

[0077] It can be seen from the results in Table 4 that although the cycle and storage performance of Comparative Examples 6-8 are improved to a certain extent compared with that of Comparative Example 5, the improvement effect is obviously not as good as that of Examples 4-18. This is because the commonly used nitriles have a certain complexing effect on cobalt ions, but the complexing effect is obviously not as good as the silicon-containing polynitrile compounds described in the present invention, and the silicon-containing polynitrile compounds can also act on the negative electrode silicon material at the same time, further improving the cycle and storage performance.

[0078] It can be seen from the results in Table 4 that the cycle performance and storage performance of Examples 11-18 are better than those of Example 4. This is because Examples 11-18 add some additives on the basis of the silicon-containing polynitrile compound relative to Example 4, which further improves the cycle performance and storage performance of the lithium-ion battery.

[0079] The embodiments of the present invention are described in detail above. For those skilled in the art, according to the ideas of the embodiments of the present invention, there may be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A non-aqueous electrolyte for lithium-ion batteries, Features: The non-aqueous electrolyte comprises a lithium salt, a non-aqueous organic solvent and an additive; the additive is a silicon-containing polynitrile compound, the silicon-containing polynitrile compound is one or more of compound 1 and a compound having a chemical formula of structural formula 1, The chemical structure of compound 1 is , Structural formula 1 is , wherein Rf is a fluorine atom or a fluorinated alkyl group.

2. A lithium ion battery non-aqueous electrolyte according to claim 1, Features: The compound having the chemical formula of formula 1 is one or both of compound 2 and compound 3, The chemical structure of compound 2 is , The chemical structure of compound 3 is .

3. A lithium ion battery non-aqueous electrolyte according to claim 1, Features The non-aqueous electrolyte of the lithium ion battery contains the following components in parts by mass: 10 to 20 parts of lithium salt; 60 to 80 parts of non-aqueous organic solvent; and 0.1 to 5 parts of silicon-containing polynitrile compound.

4. A lithium ion battery non-aqueous electrolyte according to claim 1, Features: The lithium salt is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium difluorobis(oxalatophosphate), lithium tetrafluoroborate, lithium tetrafluorooxalatophosphate, lithium bis(trifluoromethylsulfonylimide), lithium bis(fluorosulfonylimide) and lithium 2-fluoromalonate difluoroborate.

5. A lithium ion battery non-aqueous electrolyte according to claim 1, Features: The non-aqueous organic solvent is one or more of ethylene carbonate, fluoroethylene carbonate, ethyl difluoroacetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, butyl acetate, γ-butyrolactone, propyl propionate, ethyl propionate, ethyl acetate and ethyl butyrate.

6. A lithium ion battery non-aqueous electrolyte according to claim 3, Features: The non-aqueous electrolyte further comprises 0.2 to 15 parts by weight of an auxiliary agent.

7. A lithium ion battery non-aqueous electrolyte according to claim 6, Features: The auxiliary agent is one or more of 2,2,2-trifluoromethyl ethyl carbonate, 2,2,2-trifluorodiethyl carbonate, vinylene carbonate, diethyl pyrocarbonate, 1,3-propane sultone, vinyl sulfate, 1,2-difluoroethylene carbonate, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, 4,4'-di-1,3-dioxolane-2,2'-dione, 3,3-disulfate vinyl and 4,4-disulfate vinyl.

8. A lithium ion battery, Features: The lithium ion battery comprises a positive electrode, a negative electrode and the non-aqueous electrolyte according to any one of claims 1 to 7.

9. A lithium ion battery according to claim 8, Features: The positive electrode material is lithium cobalt oxide material, and the negative electrode material is a composite material of graphite and silicon oxide material, wherein the mass percentage of silicon oxide material in the negative electrode material is 3% to 50%.

10. A lithium ion battery according to claim 8, Features: The maximum charging voltage of the lithium-ion battery is 4.53V.