Anti-overcharge electrolyte additive and application thereof in sodium ion battery

By using compound fluoroanisole as an electrolyte additive in sodium ion batteries, the proportion in the electrolyte is optimized, and the interface and electrochemical reactions of protective solid electrolyte are formed, and the problem of overcharge safety of sodium ion batteries is solved. Improves battery safety and performance, reducing cost and complexity.

CN119069808AActive Publication Date: 2024-12-03ZHEJIANG SHANGAO NEW ENERGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411462669.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-19
Publication Date
2024-12-03
Estimated Expiration
2044-10-19

AI Technical Summary

Technical Problem

There are safety hazards during the overcharge process of sodium ion batteries, which may lead to thermal runaway and short circuits. The prior art prevents overcharge through external systems or modified electrolytes, but increases costs and complexity, and the effect is not reliable enough.

Method used

Combined ortho-interpoly-p-fluoroanisole (FA) is used as the electrolyte additive. By optimizing the proportion of different additives in the electrolyte, the voltage of sodium ion batteries is prevented from rising continuously during charging, forming a protective solid electrolyte interface and electrochemistry. Response to reduce the risk of overcharge.

Benefits of technology

Improves the electrochemical performance and safety of sodium ion batteries, reduces the cost increase and complexity caused by external overcharge construction, and provides an efficient and reliable self-protection mechanism to prevent thermal runaway caused by overcharge and Short circuit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005092298740000071
    Figure BDA0005092298740000071
  • Figure BDA0005092298740000081
    Figure BDA0005092298740000081
  • Figure BDA0005092298740000082
    Figure BDA0005092298740000082
Patent Text Reader

Abstract

The invention discloses an anti-overcharge electrolyte additive and application thereof in a sodium ion battery, and relates to the technical field of sodium ion batteries. The method comprises the following specific steps: preparing a traditional electrolyte with a sodium salt concentration of 0.7-1.4 M, selecting two or more than two of electrolytes EC, PC and EMC for preparation, and naming the traditional electrolyte as a basic electrolyte; an anti-overcharge electrolyte additive A and an anti-overcharge electrolyte additive B with different concentrations are respectively added into a basic electrolyte to serve as electrolyte additives, and the sodium-ion battery electrolyte containing the additives with different concentrations is prepared. According to the method, the safety and the electrochemical performance of the sodium ion battery are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion batteries, in particular to an overcharge-preventing electrolyte additive and application thereof in sodium ion batteries. Background Art

[0002] Overcharging seriously threatens the safety of sodium-ion batteries. During the overcharging process, sodium ions are deintercalated from the positive electrode and gain electrons at the negative electrode. The over-deposited sodium forms sodium dendrites at the negative electrode, which may pierce the diaphragm and cause a short circuit in the battery. The over-deionized positive electrode material has extremely high reactivity in the sodium-ion electrolyte and is prone to thermal decomposition and release heat at high temperatures. Regardless of the mechanism, a large amount of heat will be released, causing thermal runaway of the sodium-ion battery and leading to safety accidents. In order to prevent sodium-ion batteries from being overcharged during use, the methods currently used in the market are mainly divided into two categories: (1) introducing external components for voltage monitoring. (2) developing overcharge-proof and flame-retardant electrolytes for sodium-ion batteries. The external protection methods mainly include installing a positive temperature coefficient element (PTC), a current interrupter, an external overcharge safety protection circuit or an explosion-proof safety valve inside the battery. However, introducing an external system to prevent battery overcharging will increase the weight and volume of the battery module, thereby increasing the cost and complexity of the battery. Once the external system fails, the battery will be in danger. By modifying the electrolyte, a self-protection mechanism can be established inside the battery, which can not only simplify the battery production process and reduce the manufacturing cost of the battery, but also this method of essentially improving battery safety has higher reliability.

[0003] As an anti-overcharge additive for sodium-ion batteries, it is necessary to have the following characteristics: (1) Good solubility of engine oil in organic solvents of electrolyte and fast diffusion speed. (2) Good stability within the temperature and voltage range of battery operation, and no side effects on the normal use of sodium-ion batteries. (3) Strong protective effect on batteries within the high voltage range. According to the mechanism of action of sodium-ion battery anti-overcharge electrolyte, it can be divided into two categories, redox additives and electropolymerization additives. When the battery is overcharged to the redox reaction potential, the redox additives are oxidized at the positive electrode of the battery and diffuse to the negative electrode of the battery to be reduced. The reduction product then passes through the diaphragm back to the positive electrode and is oxidized again. In the process of repeated cycles, the excess charge in the overcharge process is consumed, playing a role in overcharge protection. When the lithium-ion battery is overcharged, the polymerizable monomers of the electropolymerization additives will undergo electropolymerization reaction. The generated electropolymerization products can increase the internal resistance of the battery, limit the current and consume the overcharged electrical energy.

[0004] In this work, the (ortho-para)fluoroanisole (FA) electrolyte additive is introduced to enable the additive to act under a certain potential, thereby preventing the voltage of the sodium-ion battery from continuing to rise during the charging process and exceeding the safety critical value, thereby fundamentally solving the problem of overcharge safety of sodium-ion batteries. At the same time, the electrolyte additive has the characteristics of small amount and high efficiency, which can reduce the cost increase caused by the introduction of external anti-overcharge structure, while reducing the complexity of the battery system. Summary of the invention

[0005] The object of the present invention is to provide an anti-overcharge electrolyte additive and a method for using the same in a sodium ion battery, by combining and optimizing the proportions of different additives in the electrolyte, to prevent the voltage of the sodium ion battery from continuing to rise during charging, thereby improving the electrochemical performance and safety of the sodium ion battery.

[0006] To achieve the above object, the present invention adopts the following technical solutions:

[0007] An overcharge-preventing electrolyte additive and its application in a sodium ion battery, characterized in that the electrolyte comprises: a sodium salt, an electrolyte, an additive A and an additive B.

[0008] Preferably, the additive A is selected from the group consisting of o-fluoroanisole (2-FA), m-fluoroanisole (3-FA), and p-fluoroanisole (4-FA).

[0009] Preferably, the preparation method of the additive B is:

[0010] According to weight, 16-32 parts of 3,4-difluoro-2-methoxyaniline, CAS: 114076-35-6; 6-12 parts of N-allyl-2-pyrimidinamine; 0.002-0.03 parts of 1-allyl-3-methylimidazolium tetrafluoroborate, CAS: 851606-63-8; 3-6 parts of sodium ethoxide, 200-300 parts of toluene, and 3-7 parts of sodium hydroxide are added, and the reaction is stirred at 60-70°C for 100-150 minutes, and the toluene is removed by distillation to obtain additive B.

[0011] Preferably, the additive A and the additive B account for 1-20% of the total mass of the electrolyte.

[0012] Preferably, the sodium salt is sodium hexafluorophosphate (NaPF 6 ), sodium perchlorate (NaClO 4 ).

[0013] Preferably, the electrolyte includes a cyclic organic solvent and a chain organic solvent, the cyclic organic solvent includes one or more of ethylene carbonate, propylene carbonate and butylene carbonate, and the chain organic solvent includes one or more of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

[0014] Preferably, the positive electrode active material of the sodium ion battery is NaFe 0.5 Mn 0.5 O 2 、NaNi 0.3 Fe 0.4 Mn 0.3 O 2 、NaNi 0.33 Fe 0.34 Mn 0.33 O 2 、NaNi 0.25 Fe 0.5 Mn 0.25 O 2 、NaNi 0.2 Cu 0.1 Fe 0.4 Mn 0.3 O 2 、NaNi 0.25 Fe 0.4 Co 0.1 Mn 0.25 O 2 、NaNi 0.5 Fe 0.4 Mn 0.4 O 2.4 or NaNi 0.4 Fe 0.2 Mn 0.3 O 1.8 One or a combination of at least two of the following.

[0015] Preferably, the preparation method of the electrolyte is:

[0016] (1) preparing a conventional electrolyte with a sodium salt concentration of 0.7-1.4 M, selecting two or more of the electrolytes EC, PC, and EMC for preparation, and naming it as a basic electrolyte;

[0017] (2) Different concentrations of anti-overcharge electrolyte additive A and additive B were added to the basic electrolyte as electrolyte additives to prepare sodium ion battery electrolytes containing additives of different concentrations.

[0018] Preparation mechanism of the additive B:

[0019] The 3,4-difluoro-2-methoxyaniline undergoes an amine-olefin addition reaction with N-allyl-2-pyrimidinamine and 1-allyl-3-methylimidazolium tetrafluoroborate to obtain a synergist containing difluoromethoxybenzene, pyrimidinamine and tetrafluoroborate, which is used to assist fluoroanisole as an overcharge prevention additive for sodium ion electrolyte;

[0020] Technical effect of the additive B:

[0021] 1. Formation of a protective solid electrolyte interface

[0022] Chemical stability: These additives can form a stable solid electrolyte interface (SEI) on the electrode surface, which can effectively prevent the further decomposition of the electrolyte under high voltage, thereby preventing the battery from degrading under overcharge. Selective permeability: The formed SEI membrane allows sodium ions to pass through, but prevents larger organic molecules or dissociated ions from passing through, thereby ensuring the cycle efficiency and service life of the battery.

[0023] 2. Promote thermal stability

[0024] Improve heat capacity: The presence of additives can increase the heat capacity of battery components, slow down the rate of temperature rise in overcharge state, and provide time for the activation of protection measures. Heat dissipation performance: Among them, tetrafluoroborate is particularly known for its high thermal stability. It can remain stable at high temperatures, which helps prevent thermal runaway of the battery due to overheating.

[0025] 3. Electrochemical activity and consumable protection

[0026] Potential regulation: These additives can react electrochemically at a specific voltage to form a protective layer or change the internal resistance of the battery to limit the flow of current before the battery reaches a dangerous charge level. Sacrificial agent effect: In the electrochemical reaction, these additives can be oxidized or reduced first, thereby sacrificing themselves to protect key electrode materials from damage by overcharging.

[0027] 4. Influence on the properties of electrolyte

[0028] Solubility and compatibility: The addition of additives improves the solubility of the electrolyte and the compatibility of the electrode materials, which helps stabilize the properties of the electrolyte and reduce the generation of harmful chemicals under overcharge conditions. Increased ion mobility: In particular, tetrafluoroborate, as an ionic liquid or additive, can enhance the overall ion mobility of the electrolyte and reduce the heat accumulation of the battery under high load.

[0029] Together, these mechanisms work together to make sodium-ion batteries more stable and safer under overcharge conditions. It will be important to continue exploring the application of these compounds in different battery systems.

[0030] Technical mechanism of the above scheme:

[0031] The present invention provides an anti-overcharge electrolyte additive and a method for using it in a sodium ion battery. During the overcharge process of the battery, FA undergoes an electropolymerization reaction, and the generated polymer is first evenly deposited on the surface of the positive electrode material and the diaphragm. As the reaction progresses, the deposited polymer increases, further grows along the small holes on the diaphragm, and finally penetrates the diaphragm to form a conductive bridge between the positive and negative electrodes, causing a micro short circuit inside the battery, reducing the battery voltage, and improving the overcharge safety of the sodium ion battery.

[0032] Technical effects:

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The present invention provides a method for improving battery safety. By optimizing the proportion of additives in the electrolyte, an anti-overcharge electrolyte additive and a method for using it in a sodium ion battery are provided. During the overcharging process of the battery, FA undergoes an electropolymerization reaction, and the generated polymer is first evenly deposited on the surface of the positive electrode material and the diaphragm. As the reaction progresses, the deposited polymer increases, further grows along the small holes on the diaphragm, and finally penetrates the diaphragm to form a conductive bridge between the positive and negative electrodes, causing a micro-short circuit inside the battery, reducing the battery voltage, and improving the overcharge safety of the sodium ion battery.

[0035] (2) The preparation process provided by the present invention is relatively simple, the dosage is small, and the overall performance of the sodium ion battery is improved with a small amount of additives. The product performance is relatively good and has certain competitive advantages. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with specific embodiments. The following embodiments are only used to illustrate the present invention and are not intended to limit the scope of application of the present invention. Without departing from the spirit and essence of the present invention, modifications or replacements made to the inventive method, steps or conditions all belong to the scope of the present invention.

[0037] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the materials and reagents used are reagents and materials that can be obtained from commercial channels unless otherwise specified.

[0038] Example 1

[0039] The present invention provides a method for improving battery safety, comprising the following components:

[0040] This embodiment provides a sodium ion battery electrolyte, the formula of which is: 20g ethylene carbonate (EC) solvent, 20g propylene carbonate (PC) solvent, 20g ethyl methyl carbonate (EMC), and 10.08g sodium hexafluorophosphate. Then, different contents of additives o-fluoroanisole (2-FA) and additive B are prepared according to Table 1. The raw materials are mixed evenly to prepare an electrolyte.

[0041] The preparation method of the additive B is:

[0042] 16 g of 3,4-difluoro-2-methoxyaniline, CAS: 114076-35-6; 6 g of N-allyl-2-pyrimidinamine; 0.002 g of 1-allyl-3-methylimidazolium tetrafluoroborate, CAS: 851606-63-8; 3 g of sodium ethoxide, 200 g of toluene, and 3 g of sodium hydroxide were stirred and reacted at 60° C. for 100 min, and the toluene was removed by distillation to obtain additive B.

[0043] Table 1

[0044] Recipe Name Propylene carbonate Ethyl methyl carbonate Ethylene carbonate <![CDATA[NaPF 6 ]]> 2-FA Additive B Recipe 1 20g 20g 20g 10.08g 3ml 0.05g Recipe 2 20g 20g 20g 10.08g 6ml 0.1g Recipe 3 20g 20g 20g 10.08g 9ml 0.25g Recipe 4 20g 20g 20g 10.08g 12ml 0.4g

[0045] Example 2

[0046] The present invention provides a method for improving battery safety, comprising the following components:

[0047] This embodiment provides a sodium ion battery electrolyte, the formula of which is: 20g propylene carbonate (PC) solvent, 20g ethyl methyl carbonate (EMC), 10.08g sodium hexafluorophosphate. Then, different contents of additive m-fluoroanisole (3-FA) and additive B are taken. The electrolyte is prepared according to Table 2. The raw materials are mixed evenly to form an electrolyte.

[0048] The preparation method of the additive B is:

[0049] 24 g of 3,4-difluoro-2-methoxyaniline, CAS: 114076-35-6; 9 g of N-allyl-2-pyrimidinamine; 0.015 g of 1-allyl-3-methylimidazolium tetrafluoroborate, CAS: 851606-63-8; 4.5 g of sodium ethoxide, 250 g of toluene, and 5 g of sodium hydroxide were stirred and reacted at 65° C. for 125 min, and the toluene was removed by distillation to obtain Additive B.

[0050] Table 2

[0051] Recipe Name Propylene carbonate Ethyl methyl carbonate Ethylene carbonate <![CDATA[NaPF 6 ]]> 3-FA Additive B Recipe 1 20g 20g 20g 10.08g 3ml 0.05g Recipe 2 20g 20g 20g 10.08g 6ml 0.1g Recipe 3 20g 20g 20g 10.08g 9ml 0.25g Recipe 4 20g 20g 20g 10.08g 12ml 0.4g

[0052] Example 3

[0053] The present invention provides a method for improving battery safety, comprising the following components:

[0054] This embodiment provides a sodium ion battery electrolyte, the formula of which is: 20g propylene carbonate (PC) solvent, 20g ethyl methyl carbonate (EMC), 10.08g sodium hexafluorophosphate. Then, different contents of additives p-fluoroanisole (4-FA) and additive B are prepared according to Table 3. The raw materials are mixed evenly to prepare an electrolyte.

[0055] The preparation method of the additive B is:

[0056] 32 g of 3,4-difluoro-2-methoxyaniline, CAS: 114076-35-6; 12 g of N-allyl-2-pyrimidinamine; 0.03 g of 1-allyl-3-methylimidazolium tetrafluoroborate, CAS: 851606-63-8; 6 g of sodium ethoxide, 300 g of toluene, and 7 g of sodium hydroxide were stirred and reacted at 70° C. for 150 min, and the toluene was removed by distillation to obtain additive B.

[0057] Table 3

[0058] Recipe Name Propylene carbonate Ethyl methyl carbonate Ethylene carbonate <![CDATA[NaPF 6 ]]> 4-FA Additive B Recipe 1 20g 20g 20g 10.08g 3ml 0.05g Recipe 2 20g 20g 20g 10.08g 6ml 0.1g Recipe 3 20g 20g 20g 10.08g 9ml 0.25g Recipe 4 20g 20g 20g 10.08g 12ml 0.4g

[0059] Comparative Example 1

[0060] The present invention provides a method for improving battery safety, comprising the following components:

[0061] This embodiment provides a sodium ion battery electrolyte, the formula of which is: 20g ethylene carbonate (EC) solvent, 20g propylene carbonate (PC) solvent, 20g ethyl methyl carbonate (EMC), and 10.08g sodium hexafluorophosphate. The raw materials are mixed evenly to prepare the electrolyte.

[0062] Test Example 1: Electrochemical Performance Test

[0063] Battery assembly: The positive electrode materials of Examples 1-3 and Comparative Example 1 are respectively Prussian blue (PB) positive electrodes, the positive electrode being composed of PB, polyvinylidene fluoride (PVDF) binder, carbon nanotubes and Super P conductive agent in a mass ratio of 90.0:4.0:1.5:4.5, N-methylpyrrolidone (NMP) is added to prepare a viscous glue, which is coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a positive electrode sheet.

[0064] Hard carbon negative electrode material is used as the active material. The negative electrode is composed of HC, sodium alginate binder and Super P conductive agent in a mass ratio of 92:5:3. N-methylpyrrolidone (NMP) is added to make a viscous glue, which is coated on aluminum foil and baked in a vacuum drying oven at 120°C for 12 hours to obtain a negative electrode sheet.

[0065] PE film is used as separator.

[0066] The Prussian blue (PB)-HC battery was tested in the voltage range of 1.5V-4.5V, first discharged at a rate of 0.1C to a voltage of 1.5, and then charged at 0.1C to 4.5V.

[0067] Test Example 2: LSV

[0068] Transfer the assembled battery out of the glove box, let it stand at room temperature for 2-3 hours, and then use the Chenhua electrochemical workstation to perform a linear sweep voltammetry test. The voltage range of the half-cell scan without adding active materials is 1.5-6.0V, and the scan rate is 0.5mV / s. Then use different scan rates of 0.1, 0.2, 0.5, and 1mV / s to scan the same sodium manganate-HC battery with an electrolyte system of 5% 3FA, and the scan voltage is 1.5-6.0V. For the same half-cell, perform a low-rate scan first, and then a high-rate scan in sequence.

[0069] Test Example 3: Thermal Stability Test

[0070] The fully discharged Prussian blue (PB)-HC battery was disassembled in a glove box to obtain the sodium manganate positive electrode and HC negative electrode. Then the sodium manganate positive electrode, HC negative electrode, electrolyte containing (o-m-p)fluoroanisole (FA) and two groups of basic electrolytes were taken out and DSC test was immediately performed with a test temperature range of -50-400℃ and a heating rate of 5℃ / s. The exothermic energy was observed.

[0071] Test Example 4: Normal Temperature Process Safety Test

[0072] In order to explore the anti-overcharge effect of (ortho-p-)fluoroanisole (FA) as an anti-overcharge electrolyte additive for sodium ion batteries, we used a Prussian blue (PB) full battery system to conduct a battery overcharge safety test at room temperature to detect the effect of 3FA under actual action. The assembled Prussian blue (PB)-HC battery was left to stand until the electrolyte fully infiltrated the active material. A battery charge and discharge cycler was used to pre-charge and discharge 3 cycles in the range of 1.5-4.0V at a charge and discharge rate of 0.2C, and then the battery was quickly overcharged to 4.5V at a rate of 0.2C to observe the changes in the charge and discharge platform after the introduction of the additive. During the preparation process, a pipette was used to ensure that the same volume of electrolyte was added to each half-cell and that the electrolyte did not leak out during the entire experimental operation.

[0073] Test results:

[0074] Embodiment 1:

[0075]

[0076] Embodiment 2:

[0077]

[0078] Embodiment 3:

[0079]

[0080] Comparative Example:

[0081]

[0082] It can be seen from the test data of the above embodiments and test examples that the present method is effective in improving the safety and electrochemical performance of sodium ion batteries.

[0083] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An electrolyte additive for preventing overcharge and its application in sodium ion batteries, characterized in that: The electrolyte comprises: sodium salt, electrolyte, additive A and additive B.

2. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The additive A is selected from the compounds o-fluoroanisole (2-FA), m-fluoroanisole (3-FA), and p-fluoroanisole (4-FA).

3. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The preparation method of the additive B is: According to weight, 16-32 parts of 3,4-difluoro-2-methoxyaniline, 6-12 parts of N-allyl-2-pyrimidinamine, 0.002-0.03 parts of 1-allyl-3-methylimidazolium tetrafluoroborate, 3-6 parts of sodium ethoxide, 200-300 parts of toluene, and 3-7 parts of sodium hydroxide are added, and the reaction is stirred at 60-70° C. for 100-150 minutes, and the toluene is removed by distillation to obtain additive B.

4. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The additive A and the additive B account for 1-20% of the total mass of the electrolyte.

5. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The sodium salt is sodium hexafluorophosphate (NaPF6) or sodium perchlorate (NaClO4).

6. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The electrolyte includes a cyclic organic solvent and a chain organic solvent, wherein the cyclic organic solvent includes one or more of ethylene carbonate, propylene carbonate and butylene carbonate, and the chain organic solvent includes one or more of dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

7. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The positive electrode active material of the sodium ion battery is NaFe 0.5 Mn 0.5 O2、NaNi 0.3 Fe 0.4 Mn 0.3 O2、NaNi 0.33 Fe 0.34 Mn 0.33 O2、NaNi 0.25 Fe 0.5 Mn 0.25 O2、NaNi 0.2 Cu 0.1 Fe 0.4 Mn 0.3 O2、NaNi 0.25 Fe 0.4 Co 0.1 Mn 0.25 O2、NaNi 0.5 Fe 0.4 Mn 0.4 O 2.4 or NaNi 0.4 Fe 0.2 Mn 0.3 O 1.8 One or a combination of at least two of the following.

8. The electrolyte additive for preventing overcharge and its use in sodium ion batteries according to claim 1, characterized in that: The preparation method of the electrolyte: (1) preparing a conventional electrolyte with a sodium salt concentration of 0.7-1.4 M, selecting two or more of the electrolytes EC, PC, and EMC for preparation, and naming it as a basic electrolyte; (2) Different concentrations of anti-overcharge electrolyte additive A and additive B were added to the basic electrolyte as electrolyte additives to prepare sodium ion battery electrolytes containing additives of different concentrations.

Citation Information

Patent Citations

  • Non-aqueous electrolyte and non-aqueous electrolyte secondary battery

    CN108346824A

  • Lithium secondary battery electrolyte solution and lithium secondary battery containing lithium secondary battery electrolyte solution

    CN108539257A

  • Method for inhibiting overcharge of sodium secondary battery

    CN118281319A

  • Sodium-ion battery electrolyte capable of reducing solvated sodium ions and application of sodium-ion battery electrolyte

    CN118352624A

  • Overcharging preventive electrolyte and lithium-ion battery

    US20170018803A1