Electrolyte and sodium metal battery
By using phosphoryl ester as the solvent body of the electrolyte in sodium ion batteries, combining sodium hexafluorophosphate and other sodium salts, the problems of low energy density and insufficient safety of sodium ion batteries are solved, and higher energy density and more Optimal safety and longer cycle life.
Patent Information
- Application Number
- CN202411363243.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing sodium ion batteries have low energy density due to the use of hard carbon as the negative electrode material, and the flame retardant additives in conventional electrolytes have limited safety improvements, which ignition and explosion risk and cycle life attenuation problems.
Using 70-100% wt of phosphoryl ester compound as the solvent main body of the electrolyte, combining sodium hexafluorophosphate and other sodium salts, the flame retardancy and solubility are improved through the structural design of phosphoryl ester compound, and auxiliary salts and additives are added To improve the stability of the electrolyte and the wettability of the membrane.
It achieves higher energy density, better safety and longer cycle life of sodium metal batteries, while significantly improving the flame retardant effect of the electrolyte and the wettability of the diaphragm, reducing combustion risks.
Smart Images

Figure CN119069813A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery manufacturing, and in particular to an electrolyte and a sodium metal battery. Background Art
[0002] As the energy crisis and environmental crisis continue to ferment, the development of sustainable energy has become an important trend in current energy development. Sodium-ion batteries have become one of the important electrochemical energy storage candidates due to their abundant raw material resources and low cost.
[0003] Currently, sodium-ion batteries mainly use hard carbon as the negative electrode material, but the gram capacity of hard carbon itself is low, less than 300mAh / g, and the upper limit of compaction density is low, usually less than 1.0. The graphite negative electrode material in lithium-ion batteries can achieve a gram capacity of 360mAh / g, and the compaction density can exceed 1.6. In addition, the hard carbon material itself has a large specific surface area and many surface defects, resulting in low initial charge and discharge efficiency of the battery. Limited by the low capacity, low compaction and low initial efficiency of hard carbon, the energy density of sodium-ion batteries is usually less than 140Wh / kg.
[0004] Therefore, it is necessary to develop a new negative electrode material system to improve the energy density of sodium-ion batteries. One solution is to build a negative electrode-free sodium metal battery, using the dissolution and deposition reaction of sodium as the negative electrode reaction to achieve extremely high energy density.
[0005] However, the safety of negative electrode-free sodium metal batteries is greatly affected due to the high activity of sodium. Conventional carbonate and ether solvents have great safety risks when matched with sodium metal batteries. Therefore, it is of great significance to develop an intrinsically safe electrolyte system to solve the risk of explosion of negative electrode-free sodium metal batteries.
[0006] At present, the conventional practice to improve the safety of electrolytes is to add flame retardant additives, such as phosphate compounds, to conventional carbonate and ether electrolytes. However, conventional phosphate compounds have poor solubility in conventional sodium salts (such as sodium hexafluorophosphate), so the content of these additives is usually less than 10%. When the electrolyte is exposed to flames or high temperatures, once the phosphate flame retardant is consumed, the remaining electrolyte will be ignited, and the safety of the electrolyte will be limited. In addition, common phosphate compounds have high LUMO energy levels, poor reduction stability, high polarity, strong interaction with sodium ions, and a high proportion inside the solvation shell. When charging, the solvated sodium ions migrate to the negative electrode for reduction. When the solvation structure is removed, the phosphate solvation shell is easily decomposed. Therefore, excessive addition of phosphates will also lead to rapid decay of the battery cycle life. Moreover, due to their high polarity, phosphate compounds have poor wettability with ordinary PP and PE separators. Therefore, the current addition of phosphates is relatively low, and the flame retardant effect is limited.
[0007] In view of this, the present invention is proposed. Summary of the invention
[0008] The object of the present invention is to provide an electrolyte and a sodium metal battery, aiming to improve at least one of the problems mentioned in the background technology.
[0009] The present invention is achieved in that:
[0010] In a first aspect, the present invention provides an electrolyte comprising a sodium salt and a solvent;
[0011] Sodium salts include main salts, and main salts include sodium hexafluorophosphate;
[0012] The solvent includes 70 to 100% wt of a phosphoryl ester compound, and the phosphoryl ester compound has the structural formula:
[0013]
[0014] Among them, R 1 , R 2 , R 3 , R 4 Each of them is one of C1 to C4 alkane groups.
[0015] In an optional embodiment, the concentration of sodium hexafluorophosphate in the electrolyte is 0.5 to 2 mol / L.
[0016] In an alternative embodiment, the primary salt further comprises sodium nitrate.
[0017] In an optional embodiment, the concentration of sodium nitrate in the electrolyte is 0.1-0.8 mol / L.
[0018] In an optional embodiment, the sodium salt further comprises a secondary salt selected from NaFSI, sodium nitrate, NaBF 4 , sodium trifluoroacetate, sodium perchlorate, sodium methanesulfonate, sodium difluorooxalatoborate and sodium difluorophosphate.
[0019] In an optional embodiment, the concentration of the auxiliary salt in the electrolyte is 0.01-0.2 mol / L.
[0020] In an optional embodiment, an additive is further included, and the additive is selected from at least one of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, ethylene carbonate and propylene carbonate.
[0021] In an optional embodiment, the mass concentration of the additive in the electrolyte is 0.01-0.5 mol / L.
[0022] In an optional embodiment, the solvent consists of 70-100%wt of the phosphoryl ester compound and 0-30%wt of a common solvent;
[0023] The common solvent is selected from at least one of carbonate solvents, saturated monobasic ester solvents and ether solvents;
[0024] The carbonate solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate;
[0025] The saturated monobasic ester solvent is selected from at least one of ethyl acetate, propyl acetate and ethyl propionate;
[0026] The ether solvent is selected from at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, 1,4-dioxolane and ethylene glycol diethyl ether.
[0027] In a second aspect, the present invention provides a sodium metal battery, comprising the electrolyte according to any one of the aforementioned embodiments.
[0028] The present invention has the following beneficial effects:
[0029] Half of the molecular structure of phosphoryl compounds contains phosphoric acid functional groups, which provide flame retardancy; the other half is carbonate functional groups, which provide solubility for sodium salts such as sodium hexafluorophosphate. Therefore, using phosphoryl esters as the main solvent can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect;
[0030] Compared with phosphate solvents, phosphoryl compounds have lower LUMO energy levels, lower polarity, and better reduction stability. In addition, phosphoryl molecules have large steric hindrance, weak coordination with sodium ions, and are easy to form anion-rich solvation shells. Therefore, when the electrolyte provided by the present invention is used in a sodium metal battery, it has good stability with the sodium metal negative electrode.
[0031] Compared with phosphate solvents, phosphoryl compounds have carbonate functionality, which improves the wetting effect of the solvent on the diaphragm.
[0032] Therefore, the electrolyte provided by the embodiment of the present invention mainly uses phosphoryl compounds as solvents, which can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect. In addition, it also has better reduction stability, better stability with the sodium metal negative electrode, and better wetting effect on the diaphragm. The negative electrode-free sodium metal battery made of the electrolyte has better safety. DETAILED DESCRIPTION
[0033] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0034] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0035] An electrolyte provided by an embodiment of the present invention includes a sodium salt and a solvent;
[0036] Sodium salts include main salts, and main salts include sodium hexafluorophosphate;
[0037] The solvent includes 70 to 100% wt of a phosphoryl ester compound, and the phosphoryl ester compound has the structural formula:
[0038]
[0039] Among them, R 1 , R 2 , R 3 , R 4 Each of them is one of C1 to C4 alkane groups.
[0040] Half of the molecular structure of phosphoryl compounds contains phosphoric acid functional groups, which provide flame retardancy; the other half is carbonate functional groups, which provide solubility for sodium hexafluorophosphate. Therefore, using phosphoryl esters as the main solvent can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect.
[0041] The phosphoryl compounds of the above structure have lower LUMO energy levels, lower polarity, and better reduction stability than phosphate solvents. In addition, phosphoryl molecules have large steric hindrance, weak coordination with sodium ions, and are easy to form a solvation shell rich in anions. Therefore, when the electrolyte provided by the present invention is used in a sodium metal battery, it has good stability with the sodium metal negative electrode.
[0042] Compared with phosphate ester solvents, the phosphoryl compound of the above structure has a carbonate function, which improves the wetting effect of the solvent on the diaphragm.
[0043] Therefore, the electrolyte provided in the embodiment of the present invention mainly uses phosphoryl compounds as solvents, which can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect. In addition, it also has better reduction stability, better stability with the sodium metal negative electrode, and better wetting effect on the diaphragm.
[0044] Optionally, the concentration of sodium hexafluorophosphate in the electrolyte is 0.5 to 2 mol / L (eg, 0.5 mol / L, 1 mol / L or 2 mol / L).
[0045] Optionally, the main salt further comprises sodium nitrate. Optionally, the concentration of sodium nitrate in the electrolyte is 0.1-0.8 mol / L.
[0046] Optionally, the sodium salt further comprises an auxiliary salt selected from NaFSI, sodium nitrate, NaBF4 , sodium trifluoroacetate, sodium perchlorate, sodium methanesulfonate, sodium difluorooxalatoborate and sodium difluorophosphate.
[0047] Optionally, the concentration of the auxiliary salt in the electrolyte is 0.01-0.2 mol / L.
[0048] Optionally, the additive is selected from at least one of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, ethylene carbonate and propylene carbonate.
[0049] Optionally, the mass concentration of the additive in the electrolyte is 0.01 to 0.5 mol / L (eg, 0.01 mol / L, 0.1 mol / L, 0.2 mol / L or 0.5 mol / L).
[0050] Optionally, the solvent consists of 70-100% wt of the phosphoryl ester compound and 0-30% wt of a common solvent.
[0051] Specifically, the common solvent is selected from at least one of carbonate solvents, saturated monobasic ester solvents and ether solvents.
[0052] Furthermore, the carbonate solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; the saturated monoester solvent is selected from at least one of ethyl acetate, propyl acetate and ethyl propionate; the ether solvent is selected from at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, 1,4-dioxolane and ethylene glycol diethyl ether.
[0053] A sodium metal battery provided by an embodiment of the present invention includes the electrolyte provided by an embodiment of the present invention.
[0054] The sodium metal battery has better safety because the electrolyte provided by the present invention is used as the electrolyte.
[0055] Example 1
[0056] This embodiment provides an electrolyte, and its specific formula is as follows:
[0057] The solvent of the electrolyte is composed of 70%wt of phosphoryl compound and 30%wt of ethylene carbonate;
[0058] In phosphoryl compounds, R1 is -CH 3 , R2 is -CH 3 , R3 is -CH 3 , R4 is -CH 3 .
[0059] The sodium salts and their concentrations in the electrolyte are: sodium hexafluorophosphate 0.5 mol / L, sodium nitrate 0.1 mol / L, and NaFSI 0.01 mol / L.
[0060] The additive and its concentration in the electrolyte are: 0.1 mol / L of fluoroethylene carbonate.
[0061] Example 2
[0062] This embodiment provides an electrolyte, and its specific formula is as follows:
[0063] The solvent of the electrolyte consists of 80%wt of phosphoryl compound, 10%wt of propylene carbonate and 10%wt of ethylene glycol dimethyl ether;
[0064] In phosphoryl compounds, R1 is -CH 3 , R2 is -CH 2 -CH 3 , R3 is -CH 2 -CH 2 -CH 3 , R4 is -CH 2 -CH 3 .
[0065] The sodium salts and their concentrations in the electrolyte are: sodium hexafluorophosphate 2 mol / L, sodium nitrate 0.8 mol / L, sodium methanesulfonate 0.2 mol / L.
[0066] The additives and their concentrations in the electrolyte are: 0.05 mol / L vinylene carbonate, 0.05 mol / L vinyl sulfate.
[0067] Example 3
[0068] This embodiment provides an electrolyte, and its specific formula is as follows:
[0069] The electrolyte solvent consists of 90%wt of phosphoryl compound and 10%wt of propylene carbonate;
[0070] In phosphoryl compounds, R1 is -CH 2 -CH 3 , R2 is -CH 2 -CH 2 -CH 3 , R3 is -CH 3 , R4 is -CH 2 -CH 3 .
[0071] The sodium salts and their concentrations in the electrolyte are: sodium hexafluorophosphate 1 mol / L, sodium nitrate 0.5 mol / L, sodium perchlorate 0.1 mol / L.
[0072] The additives and their concentrations in the electrolyte are: vinyl sulfate 0.05 mol / L, vinylene carbonate 0.05 mol / L.
[0073] Example 4
[0074] This embodiment provides an electrolyte, and its specific formula is as follows:
[0075] The solvent of the electrolyte consists of 100%wt of phosphoryl compound;
[0076] In phosphoryl compounds, R1 is -CH 2 -CH 2 -CH 2 -CH 3 , R2 is -CH 3 , R3 is -CH 3 , R4 is -CH 2 -CH 3 .
[0077] The sodium salts and their concentrations in the electrolyte are: sodium hexafluorophosphate 1 mol / L, sodium nitrate 0.5 mol / L, sodium nitrate 0.1 mol / L.
[0078] The additive and its concentration in the electrolyte are: 1,3-propane sultone 0.1 mol / L.
[0079] Comparative Example 1
[0080] This comparative example is basically the same as Example 1, except that the solvent of the electrolyte in Example 1 is completely replaced by an equal volume, and the solvent composition of this comparative example is:
[0081] 90%wt propylene carbonate, 10%wt trimethyl phosphate.
[0082] Comparative Example 2
[0083] This comparative example is basically the same as Example 1, except that the solvent of the electrolyte in Example 1 is completely replaced by an equal volume, and the solvent composition of this comparative example is:
[0084] 80%wt propylene carbonate, 20%wt triethyl phosphate.
[0085] Comparative Example 3
[0086] This comparative example is basically the same as Example 1, except that the solvent of the electrolyte in Example 1 is completely replaced by an equal volume, and the solvent composition of this comparative example is:
[0087] The invention is composed of 60%wt of phosphoryl compounds and 40%wt of propylene carbonate.
[0088] Comparative Example 4
[0089] This comparative example is basically the same as Example 1, except that the solvent of the electrolyte in Example 1 is completely replaced by an equal volume, and the solvent composition of this comparative example is:
[0090] 70%wt diethyl carbonate, 30% ethylene carbonate.
[0091] Experimental example
[0092] (1) The electrolytes of the various embodiments and comparative examples were prepared into sodium metal batteries, and the preparation method was as follows:
[0093] S1. Sodium iron pyrophosphate, carbon black and PVDF are homogenized in a NMP solution at a mass ratio of 94:3:3, and coated on an aluminum foil, and dried to form a positive electrode sheet.
[0094] S2, NaPF 6 Dissolved in diethylene glycol dimethyl ether as the electrolyte, the electrode prepared in the above embodiment is used as the negative electrode, the positive electrode prepared in S1, and a 20 μm thick polypropylene separator are assembled into a single-chip soft-pack battery in a glove box filled with argon.
[0095] (2) The electrolytes of Example 1 and Comparative Example 1 were prepared into sodium ion batteries, and the preparation method was as follows:
[0096] S1. Sodium iron pyrophosphate, carbon black and PVDF are homogenized in a NMP solution at a mass ratio of 94:3:3, and coated on an aluminum foil, and dried to form a positive electrode sheet.
[0097] S2. Hard carbon, carbon black and PVDF are homogenized in a NMP solution at a mass ratio of 94:3:3, and coated on an aluminum foil, and dried to form a negative electrode sheet.
[0098] S3. The positive and negative electrodes prepared in S1 and S2, a 20 μm thick polypropylene separator, and the electrolyte in the above embodiment are assembled into a single-chip soft-pack battery in a glove box filled with argon.
[0099] (3) Conducting battery performance test on the prepared battery:
[0100] First coulombic efficiency test of the battery: charge the assembled battery to 3.4V at 0.1C, then discharge it to 2.0V at 0.1C, and calculate the ratio of the battery discharge capacity to the charge capacity as Q;
[0101] Cycle life test: Charge the assembled battery to 3.4V at 0.5C at 25℃, then discharge it to 2.0V at 1C, cycle 100 times, and record the capacity retention rate;
[0102] Flame retardancy test: Cut the prepared battery in half, point the cut end at the flame of a lighter, and observe the second at which the battery starts to burn. If the battery does not catch fire, place it above the flame for 30 seconds; if the battery catches fire, remove the battery and observe the second at which the battery flame goes out.
[0103] Record the test results in Table 1.
[0104] Table 1 Electrochemical properties of the batteries prepared in various embodiments and comparative examples
[0105]
[0106] It can be seen from the test data in Table 1 that the sodium metal batteries prepared in the various embodiments provided by the present invention have better flame retardancy and electrochemical properties, and the flame retardancy of each embodiment is significantly more significant than that of Comparative Example 4.
[0107] The performance of sodium metal batteries made from the electrolytes provided in Example 1, Comparative Example 1 and Comparative Example 4 is compared. The electrolyte formula of Comparative Example 1 is a conventional carbonate solvent in which phosphate ester is added to improve flame retardancy. Although Comparative Example 1 has better flame retardancy than Comparative Example 4, its flame retardancy and cycle performance are significantly worse than those of Example 1.
[0108] The performance of the sodium metal battery made of the electrolyte provided in Comparative Example 1 and Comparative Example 2 is compared. The electrolyte formula of Comparative Example 2 is based on the conventional carbonate solvent and the phosphate ester formula is added to increase the amount of phosphate ester. From the data in Table 1, it can be seen that the cycle performance of Comparative Example 2 is worse, indicating that the cycle life of the battery is worse due to the higher phosphate ester content;
[0109] Comparing the performance of the sodium metal battery made of the electrolyte provided in Comparative Example 3 with that in Example 1, Comparative Example 3 failed to completely suppress combustion and the cycle performance was also reduced, indicating that reducing the content of phosphoryl compounds in the solvent will make the flame retardancy of the electrolyte lower and the cycle performance worse.
[0110] The performance of sodium metal batteries made of the electrolyte provided in Examples 1, 2, 3, and 4 was compared with that of the comparative example 1. Examples 1, 2, 3, and 4 all had complete flame retardancy and were not flammable when exposed to flames. The performance of sodium ion batteries made of the electrolyte provided in Example 1 was compared with that of the comparative example 1. Example 1 had complete flame retardancy and was not flammable when exposed to flames.
[0111] (4) Testing the wettability of the electrolyte provided in each embodiment and comparative example to the diaphragm, the testing method is as follows:
[0112] Take a 20 cm long and 10 cm wide separator and straighten it horizontally, drop 100 uL of the electrolyte in the above embodiment and comparative example on one side of the separator, and record the time t required for the electrolyte to diffuse to the other side. The electrolyte infiltration rate is calculated to be 20 / t.
[0113] Record the test results in Table 2.
[0114] Table 2 Wettability of the electrolytes of the embodiments and comparative examples on the diaphragm
[0115]
[0116] It can be seen from the data in Table 2 that the comparative examples of the present invention have better wettability to the diaphragm than comparative examples 1 and 2.
[0117] In summary, the electrolyte provided by the embodiment of the present invention has the following characteristics:
[0118] 1. Half of the molecular structure of phosphoryl compounds contains phosphoric acid functional groups, which provide flame retardancy; the other half is carbonate functional groups, which provide solubility for sodium hexafluorophosphate. Therefore, using phosphoryl esters as the main solvent can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect.
[0119] 2. Phosphoryl compounds have lower LUMO energy level, lower polarity and better reduction stability than phosphate solvents. In addition, phosphoryl molecules have large steric hindrance, weak coordination with sodium ions, and are easy to form a solvation shell rich in anions. Therefore, when the electrolyte provided by the present invention is used in a sodium metal battery, it has good stability with the sodium metal negative electrode.
[0120] 3. Compared with phosphate solvents, phosphoryl compounds have carbonate functionality, which improves the wetting effect of the solvent on the diaphragm.
[0121] Therefore, the electrolyte provided by the embodiment of the present invention mainly uses phosphoryl compounds as solvents, which can not only meet the solubility requirements of sodium salts, but also improve the flame retardant effect. In addition, it also has better reduction stability, better stability with the sodium metal negative electrode, and better wetting effect on the diaphragm. The negative electrode-free sodium metal battery made of the electrolyte has better safety.
[0122] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An electrolyte, characterized in that: including sodium salt and solvent; The sodium salt includes a main salt, and the main salt includes sodium hexafluorophosphate; The solvent comprises 70 to 100% wt of a phosphoryl ester compound, and the phosphoryl ester compound has the structural formula: Wherein, R1, R2, R3, and R4 are each one of C1 to C4 alkane groups.
2. The electrolyte according to claim 1, characterized in that The concentration of the sodium hexafluorophosphate in the electrolyte is 0.5 to 2 mol / L.
3. The electrolyte according to claim 1, characterized in that The main salt also includes sodium nitrate.
4. The electrolyte according to claim 3, characterized in that The concentration of the sodium nitrate in the electrolyte is 0.1-0.8 mol / L.
5. The electrolyte according to claim 1, characterized in that The sodium salt also includes an auxiliary salt, and the auxiliary salt is selected from at least one of NaFSI, sodium nitrate, NaBF4, sodium trifluoroacetate, sodium perchlorate, sodium methanesulfonate, sodium difluorooxalatoborate and sodium difluorophosphate.
6. The electrolyte according to claim 5, characterized in that The concentration of the auxiliary salt in the electrolyte is 0.01-0.2 mol / L.
7. The electrolyte according to claim 1, characterized in that The invention also includes an additive, wherein the additive is selected from at least one of fluoroethylene carbonate, vinylene carbonate, vinyl sulfate, 1,3-propane sultone, ethylene carbonate and propylene carbonate.
8. The electrolyte according to claim 7, characterized in that The concentration of the additive in the electrolyte is 0.01-0.5 mol / L.
9. The electrolyte according to claim 1, characterized in that The solvent is composed of 70-100%wt of the phosphoryl ester compound and 0-30%wt of a common solvent; The common solvent is selected from at least one of carbonate solvents, saturated monobasic ester solvents and ether solvents; The carbonate solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate; The saturated monobasic ester solvent is selected from at least one of ethyl acetate, propyl acetate and ethyl propionate; The ether solvent is selected from at least one of ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, tetrahydrofuran, 1,4-dioxolane and ethylene glycol diethyl ether.
10. A sodium metal battery, characterized in that: The invention comprises the electrolyte as claimed in any one of claims 1 to 9.