Secondary battery and electric device
By introducing aluminum and niobium into the positive electrode active material of the secondary battery, and adding lithium difluoroxalate borate and fluorosolv to the electrolyte, the problem of poor cycling performance of the secondary battery at high voltage is solved, and excellent Cycling performance and low internal resistance growth rate.
Patent Information
- Application Number
- CN202411147235.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-12-03
AI Technical Summary
The existing secondary batteries have poor cycling performance under high voltages, and the unstable positive electrode oxygen release and electrolyte film formation lead to obvious internal resistance growth.
Aluminum and niobium are introduced simultaneously into the positive electrode active material, and lithium difluoroxalate borate and fluorosolv are added to the electrolyte to reasonably control their mass percentage to improve the film formation stability of the electrolyte and reduce the oxygen release of the positive electrode to form excellent Cycling performance and low internal resistance.
The secondary battery has excellent circulation performance and low internal resistance growth rate, reduced initial internal resistance, and small internal resistance growth rate during the cycle, which improves the overall performance of the battery.
Smart Images

Figure BDA0005002755890000121 
Figure BDA0005002755890000131 
Figure BDA0005002755890000132
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Art
[0002] Increasing the cut-off voltage of the battery is the most economical way to increase the battery energy density, but high voltage will also bring some problems, such as positive electrode phase change, cracks, oxygen release and electrolyte side reactions. Therefore, it is urgent to improve the overall performance of the battery from the positive electrode and electrolyte design. It is well known that the electrolyte is oxidatively unstable under high voltage, and ethylene carbonate (EC) will undergo side reactions such as oxidation and decomposition under the catalysis of transition metals, so it is necessary to improve the overall oxidation stability of the electrolyte. Summary of the invention
[0003] The purpose of the present application is to solve the problems in the prior art of poor cycle performance of secondary batteries and significant increase in internal resistance during the cycle caused by positive electrode oxygen release and unstable electrolyte film formation, and to provide a secondary battery and electrical device with excellent cycle stability and a low internal resistance growth rate during the cycle.
[0004] To achieve the above-mentioned object, in a first aspect of the present application, a secondary battery is provided, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material;
[0005] The electrolyte comprises lithium difluorooxalatoborate and a fluorinated solvent;
[0006] The positive electrode active material includes aluminum and niobium;
[0007] The secondary battery satisfies: 0.020≤Y≤0.48;
[0008] in,
[0009] C% is the mass percentage of lithium difluorooxalatoborate in the electrolyte;
[0010] W1% is the mass percentage of the fluorinated solvent in the electrolyte;
[0011] W2% is the mass percentage of aluminum element in the positive electrode active material;
[0012] W3% is the mass percentage of niobium element in the positive electrode active material.
[0013] As an embodiment of the present application, the mass percentage C of the lithium difluorooxalatoborate in the electrolyte is 0.1-5%.
[0014] As an embodiment of the present application, the mass percentage W1 of the fluorinated solvent in the electrolyte is 1-50%.
[0015] As an embodiment of the present application, the mass percentage W2 of the aluminum element in the positive electrode active material is 0.1-1%.
[0016] As an embodiment of the present application, the mass percentage W3 of the niobium element in the positive electrode active material is 0.1-1%.
[0017] As an implementation scheme of the present application, the ratio of W2 to W3 is (1-5):1.
[0018] As an embodiment of the present application, the ratio of C to W1 is (0.01-0.3):1.
[0019] As an embodiment of the present application, the ratio of C to W2 is (1-6):1.
[0020] As an embodiment of the present application, the fluorinated solvent includes at least one of fluorinated carbonates, fluorinated carboxylates, fluorinated ethers, and fluorinated nitriles having 3 to 20 carbon atoms.
[0021] As an embodiment of the present application, the electrolyte further includes a lithium salt, an organic solvent and an additive; based on the electrolyte, the mass percentage of the lithium salt is 8-20%, the mass percentage of the organic solvent is 80-90%, and the mass percentage of the additive is 0.5-10%.
[0022] As an embodiment of the present application, the lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate), lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide.
[0023] As an embodiment of the present application, the organic solvent includes at least two of ethylene carbonate, propylene carbonate, butylene carbonate, trifluoroethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, diphenyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, ethyl 2,2-difluoroacetate, methyl 2,2-difluoroacetate, methyl 2,3,3,3-tetrafluoropropionate, γ-butyrolactone, acetonitrile, and cyclopentane sulfone.
[0024] As an embodiment of the present application, the additive includes at least one of a silicon-containing additive, a sulfur-containing additive, and a cyclic carbonate additive.
[0025] As an embodiment of the present application, the positive electrode active material includes Li a Ni x Co y Mnz M b Al c Nb (1-x-y-z-c) At least one of the compounds shown in O2;
[0026] Among them, 0.9≤a≤1.1, 0<x<1, 0<y<1, 0 <z<1,0≤b≤0.1;
[0027] M is at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Y, Ti, In, La, Ce, Sr, Sb, and B.
[0028] As an implementation scheme of the present application, 0.5<x<0.8, x / y≥2.5.
[0029] In a second aspect of the present application, an electrical device is provided, comprising the secondary battery described above.
[0030] Compared with the prior art, the beneficial effects of this application are:
[0031] In the secondary battery provided in the present application, by simultaneously introducing aluminum and niobium into the positive electrode active material, simultaneously adding lithium difluorooxalate borate and a fluorinated solvent into the electrolyte, and by reasonably controlling the mass percentage of lithium difluorooxalate borate and the fluorinated solvent in the electrolyte, and the mass percentage of aluminum and niobium in the positive electrode active material, the secondary battery satisfies: It can effectively improve the electrolyte film formation stability and reduce positive electrode oxygen release, so that the obtained secondary battery has excellent cycle performance and a low internal resistance growth rate during the cycle; and can also simultaneously achieve a lower initial internal resistance of the secondary battery. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0033] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0034] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0035] The reagents or instruments used in this application without indicating the manufacturer are all conventional products that can be obtained through commercial purchase.
[0036] In one embodiment of the present application, the present application proposes a secondary battery, including a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet includes a positive electrode collector and a positive electrode active material layer disposed on at least one surface of the positive electrode collector, wherein the positive electrode active material layer includes a positive electrode active material;
[0037] The electrolyte comprises lithium difluorooxalatoborate and a fluorinated solvent;
[0038] The positive electrode active material includes aluminum and niobium;
[0039] The secondary battery satisfies: 0.020≤Y≤0.48;
[0040] in,
[0041] C% is the mass percentage of lithium difluorooxalatoborate in the electrolyte;
[0042] W1% is the mass percentage of the fluorinated solvent in the electrolyte;
[0043] W2% is the mass percentage of aluminum element in the positive electrode active material;
[0044] W3% is the mass percentage of niobium element in the positive electrode active material.
[0045] The present application has found that the addition of additives to the electrolyte has a significant effect on the film-forming ability of the electrolyte, and the type of element doping in the positive electrode active material will also affect the oxygen release and phase change of the positive electrode under high pressure, which will in turn affect the cycle performance of the secondary battery and the growth of the internal resistance during the cycle. The secondary battery provided by the present application, on the one hand, can effectively solve the problems of oxygen release and phase change of the positive electrode under high pressure by simultaneously adding aluminum doping and niobium coating to the positive electrode active material; on the other hand, the simultaneous addition of lithium difluorooxalate borate to the electrolyte can make the electrolyte film formation more stable; further, the present application reasonably controls the mass percentage of lithium difluorooxalate borate and fluorinated solvent in the electrolyte, and the mass percentage of aluminum and niobium in the positive electrode active material, so that the secondary battery meets the following requirements: It can effectively improve the CEI film formation stability and reduce the oxygen release of the positive electrode material and the dissolution of the transition metal, so that the obtained secondary battery has excellent cycle performance and a low internal resistance growth rate during the cycle; and the obtained secondary battery has a low initial internal resistance.
[0046] Exemplarily, the secondary battery satisfies 0.020≤Y≤0.48, wherein Y can be any point value or any two point range values within the range of 0.020≤Y≤0.48, such as 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, 0.21, 0.22, 0.23, 0.24, 0.25, 0.26, 0.27, 0.28, 0.29, 0.30, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.31, 0.32, 0.33, 0.34, 0.35, 0.36, 0.37, 0.38, 0.39, 0.4, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, or any two of them; when the Y value of the secondary battery is within the above range, the cycle performance of the obtained secondary battery is better, and the internal resistance growth rate of the secondary battery before and after the cycle is lower.
[0047] In one embodiment, the secondary battery satisfies 0.05≤Y≤0.28. For example, Y may be 0.05, 0.055, 0.06, 0.065, 0.07, 0.075, 0.085, 0.09, 0.095, 0.1, 0.105, 0.11, 0.115, 0.12, 0.125, 0.13, 0.135, 0.14, 0.145, 0.15, 0.155, 0.16, 0.165, 0.1 7. The range value of one or any two of 0.175, 0.18, 0.185, 0.19, 0.195, 0.2, 0.205, 0.21, 0.215, 0.22, 0.225, 0.23, 0.235, 0.24, 0.245, 0.25, 0.255, 0.26, 0.265, 0.27, 0.275, 0.28. The present application study found that when the secondary battery is further selected to satisfy 0.05≤Y≤0.28, the comprehensive performance of the obtained secondary battery is better.
[0048] In one embodiment, the mass percentage C of the lithium difluorooxalatoborate in the electrolyte is 0.1-5%.
[0049] It should be noted that the test method for the mass percentage of lithium difluorooxalatoborate in the electrolyte is: the electrolyte is extracted from the secondary battery with a syringe, then filtered with a filter membrane, and then tested on a GC-MS gas chromatography-mass spectrometer to calculate the mass percentage of lithium difluorooxalatoborate in the electrolyte.
[0050] Exemplarily, the mass percentage C of the lithium difluorooxalatoborate in the electrolyte can be any point value between 0.1-5% or any two point range values, for example, it can be 0.1%, 0.3%, 0.5%, 0.8%, 1.0%, 1.3%, 1.5%, 1.8%, 2.0%, 2.3%, 2.5%, 2.8%, 3.0%, 3.3%, 3.5%, 3.8%, 4.0%, 4.3%, 4.5%, 4.8%, 5.0%, etc.
[0051] The present application study found that lithium difluorooxalatoborate can form a solid electrolyte interface film of lithium oxalate and lithium fluoride at the positive electrode, thereby improving the stability of the interface and further slowing down the growth of the internal resistance of the secondary battery during the cycle process; at the same time, the addition of lithium difluorooxalatoborate can also effectively reduce the initial internal resistance of the secondary battery.
[0052] In one embodiment, the mass percentage C of the lithium difluorooxalatoborate in the electrolyte is 0.1-3%. For example, C can be 0.1%, 0.2%, 0.4%, 0.6%, 0.7%, 0.9%, 1.1%, 1.2%, 1.4%, 1.6%, 1.7%, 1.9%, 2.1%, 2.2%, 2.6%, 2.7%, 2.9%, 3.0%, or any two of them. The present application has found that when C is further selected to be 0.1-3%, the initial internal resistance of the secondary battery obtained is lower, and the internal resistance increases less during the cycle.
[0053] In one embodiment, the mass percentage W1 of the fluorinated solvent in the electrolyte is 1-50%.
[0054] It should be noted that the test method for the mass percentage of fluorinated solvents in the electrolyte is: the electrolyte is extracted from the secondary battery with a syringe, followed by filtering with a membrane, and then the mass percentage of the fluorinated solvent in the electrolyte is calculated after testing on a gas chromatograph-mass spectrometer (GC-MS) or an ion chromatograph-mass spectrometer (IC-MS) according to the type of fluorinated solvent selected.
[0055] Exemplarily, the mass percentage W1 of the fluorinated solvent in the electrolyte can be any point value or any two point range values between 1-50%, for example, 1%, 2%, 5%, 8%, 10%, 12%, 15%, 18%, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, etc.
[0056] The present application study found that fluorinated solvents are resistant to oxidation and can effectively reduce side reactions during the cycle process. Fluorinated solvents in an appropriate addition range can reduce the initial internal resistance of the secondary battery and reduce the growth of the internal resistance during the cycle while avoiding severe capacity loss caused by excessive viscosity, thereby improving the cycle stability of the secondary battery.
[0057] In one embodiment, the mass percentage W1 of the fluorinated solvent in the electrolyte is 5-30%. For example, W1 can be 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 21%, 23%, 25%, 27%, 29%, 30%, or any two of them. The present application found that when W1 is further selected to be 5-30%, the initial internal resistance of the obtained product is lower, the cycle stability of the secondary battery is better, and the internal resistance growth before and after the cycle is less.
[0058] In one embodiment, the mass percentage W2 of the aluminum element in the positive electrode active material is 0.1-1%.
[0059] It should be noted that the test method for the mass percentage of aluminum in the positive electrode active material is as follows: scrape the positive electrode active material on the positive electrode sheet and place it in a 100mL beaker, moisten it with a small amount of water and add 10mL of nitric acid, cover it with a watch glass and heat it on a 220℃ hot plate for 30 minutes to dissolve, then cool and filter it and transfer it to a 100mL volumetric flask to make up the volume, then test it on an ICP atomic emission spectrometer to obtain the element and concentration measurement values, and finally calculate the mass percentage of aluminum in the positive electrode active material.
[0060] Exemplarily, the mass percentage W2 of the aluminum element in the positive electrode active material can be any point value or any two point range values between 0.1-1%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, etc.
[0061] The present invention has found that the introduction of aluminum into the positive electrode material can effectively passivate the positive electrode interface, inhibit phase change and oxygen release, reduce crosstalk between the positive and negative electrodes, and inhibit side reactions, thereby improving the cycle stability of the secondary battery and reducing the growth of the internal resistance before and after the cycle; and the introduction of an appropriate amount of aluminum will not damage the capacity of the secondary battery, and can ensure that the power performance of the secondary battery is good.
[0062] In one embodiment, the mass percentage W2 of the aluminum element in the positive electrode active material is 0.25-0.75%. For example, it can be 0.25%, 0.28%, 0.32%, 0.34%, 0.36%, 0.38%, 0.42%, 0.44%, 0.46%, 0.48%, 0.52%, 0.54%, 0.56%, 0.58%, 0.62%, 0.64%, 0.66%, 0.68%, 0.72%, 0.75%, etc. The present invention has found that when the mass percentage of the aluminum element is further selected to be 0.25-0.75%, the comprehensive effect of the obtained product is better.
[0063] In one embodiment, the mass percentage W3 of the niobium element in the positive electrode active material is 0.1-1%.
[0064] It should be noted that the test method for the mass percentage of niobium in the positive electrode active material is as follows: scrape the positive electrode active material on the positive electrode sheet and place it in a 100mL beaker, moisten it with a small amount of water and add 10mL nitric acid, cover it with a watch glass and heat it on a 220℃ hot plate for 30 minutes to dissolve, then cool and filter it and transfer it to a 100mL volumetric flask to make up the volume, then test it on an ICP atomic emission spectrometer to obtain the element and concentration measurement values, and finally calculate the mass percentage of niobium in the positive electrode active material.
[0065] Exemplarily, the mass percentage W2 of the niobium element in the positive electrode active material can be any point value or any two point range values between 0.1-1%, such as 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, etc.
[0066] The present invention has found that the introduction of niobium into the positive electrode material can effectively relieve the internal strain, limit the lattice contraction, and thus inhibit the oxygen release of the positive electrode, and the introduction of niobium can form a fast ion conductor LiNbO3 protective layer to further inhibit side reactions and hinder the lattice oxygen release caused by the dissolution of transition metals; thereby, the cycle stability of the secondary battery can be effectively improved and the increase of the internal resistance before and after the cycle can be reduced; at the same time, the niobium element in a suitable addition range can also avoid the decrease in the capacity of the secondary battery, thereby maintaining the good kinetic performance of the secondary battery.
[0067] In one embodiment, the mass percentage W3 of the niobium element in the positive electrode active material is 0.25-0.75%. For example, it can be 0.25%, 0.28%, 0.32%, 0.34%, 0.36%, 0.38%, 0.42%, 0.44%, 0.46%, 0.48%, 0.52%, 0.54%, 0.56%, 0.58%, 0.62%, 0.64%, 0.66%, 0.68%, 0.72%, 0.75%, etc. The present invention has found that when the mass percentage of the niobium element in the positive electrode active material is further selected to be 0.25-0.75%, the comprehensive effect of the obtained product is better.
[0068] In one embodiment, the ratio of W2 to W3 is (1-5):1.
[0069] Exemplarily, the ratio of W2 and W3 can be any point value or any two points between (1-5):1, such as 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 2.0:1, 2.5:1, 3.0:1, 3.5:1, 4.0:1, 4.5:1, 5.0:1, etc.
[0070] In one embodiment, the ratio of C to W1 is (0.01-0.3):1.
[0071] Exemplarily, the ratio of C and W1 can be any point value or any two points between (0.01-0.3):1, such as 0.01:1, 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1, 0.28:1, 0.3:1, etc.
[0072] In one embodiment, the ratio of C to W2 is (1-6):1.
[0073] Exemplarily, the ratio of C to W2 may be any point value or any two points between (1-6):1, such as 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, etc.
[0074] The present invention has found that the mass percentage ratio of niobium element and aluminum element in the positive electrode active material, the mass percentage ratio of lithium difluorooxalatoborate and fluorinated solvent in the electrolyte, and the mass percentage ratio of lithium difluorooxalatoborate in the electrolyte to the mass percentage ratio of aluminum element in the positive electrode active material will also affect the comprehensive performance of the product. When the above ratio relationships are further selected, the secondary battery obtained has a lower initial internal resistance, better cycle performance, and a lower increase in internal resistance before and after the cycle.
[0075] In one embodiment, the fluorinated solvent includes at least one of fluorinated carbonates, fluorinated carboxylates, fluorinated ethers, and fluorinated nitriles having 3 to 20 carbon atoms.
[0076] In some embodiments, the fluorinated carbonate having 3-20 carbon atoms includes at least one of fluoroethylene carbonate and methyl trifluoroethyl carbonate.
[0077] In some embodiments, the fluorocarboxylic acid ester includes at least one of methyl trifluoropropionate and ethyl trifluoropropionate.
[0078] In some embodiments, the fluorinated ether includes at least one of tetrafluoroethyltetrafluoropropyl ether and difluoromethyl-2,2,2-trifluoroethyl ether.
[0079] In some embodiments, the fluoronitrile includes at least one of fluoroacetonitrile and trifluoropropionitrile.
[0080] In one embodiment, the electrolyte further comprises lithium salt, organic solvent and additives; based on the electrolyte, the mass percentage of lithium salt is 8-20%, the mass percentage of organic solvent is 80-90%, and the mass percentage of additives is 0.5-10%.
[0081] Exemplarily, based on the electrolyte, the mass percentage of the lithium salt can be any point value or any range value between 8-20%, for example, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc.; the mass percentage of the organic solvent can be any point value or any range value between 80-90%, for example, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, etc.; the mass percentage of the additive can be any point value or any range value between 0.5-10%, for example, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, etc.
[0082] In one embodiment, the lithium salt includes at least one of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorobis(oxalatophosphate) (LiDFOP), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).
[0083] Further preferably, the lithium salt comprises lithium hexafluorophosphate. The lithium salt has high conductivity, and the overall performance of the secondary battery obtained after being applied to the secondary battery is better.
[0084] In one embodiment, the organic solvent includes at least two of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), trifluoroethyl carbonate (FEMC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate (MPC), diphenyl carbonate (DPhC), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), ethyl 2,2-difluoroacetate (EDFA), methyl 2,2-difluoroacetate (MDFA), methyl 2,3,3,3-tetrafluoropropionate (M4FP), γ-butyrolactone (γ-GBL), acetonitrile (AN), and sulfolane (TMS).
[0085] In one embodiment, the additive includes at least one of a silicon-containing additive, a sulfur-containing additive, and a cyclic carbonate additive.
[0086] In one embodiment, the silicon-containing additive includes at least one of tris(trimethylsilyl)phosphite, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)borate, trimethylfluorosilane, and heptamethyldisilazane.
[0087] In one embodiment, the sulfur-containing additive includes at least one of 1,3-propane sultone, vinyl sulfate, and methylene methane disulfonate.
[0088] In one embodiment, the cyclic carbonate additive includes at least one of vinylene carbonate and vinyl ethylene carbonate.
[0089] In one embodiment, the positive electrode active material includes Li a Ni x Co y Mn z M b Al c Nb (1-x-y-z-c) At least one of the compounds shown in O2, wherein 0.9≤a≤1.1, 0<x<1, 0<y<1, 0 <z<1,0≤b≤1。
[0090] In one embodiment, the positive electrode active material satisfies 0.5<x<0.8.
[0091] In one embodiment, the positive electrode active material satisfies x / y≥2.5.
[0092] In one embodiment, the positive electrode active material satisfies y>0.2.
[0093] In one embodiment of the present application, the present application proposes an electrical device, and the electrical device includes the secondary battery described in the present application.
[0094] Exemplarily, the above-mentioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0095] Example 1
[0096] The present invention provides a secondary battery, wherein a method for preparing the secondary battery comprises the following steps:
[0097] (1) Preparation of electrolyte
[0098] At room temperature, in a glove box filled with argon (H2O<1ppm, O2<1ppm), an organic solvent (ethylene carbonate and ethyl methyl carbonate) and a fluorinated solvent (fluoroethylene carbonate) are uniformly mixed in a mass ratio of ethylene carbonate: fluoroethylene carbonate: ethyl methyl carbonate = 2:1:7, and water is removed with a 4A molecular sieve to obtain a mixed solvent, 1M LiPF6 lithium salt is added successively to the obtained mixed solvent, and the mixture is continuously stirred and cooled with dry ice to ensure that the temperature of the electrolyte does not rise by more than 2°C, and finally a colorless transparent liquid is obtained, and then additives (vinylene carbonate and lithium difluorooxalate borate) are added to obtain an electrolyte, wherein, based on the electrolyte, the mass percentage of vinylene carbonate is 1%, the mass percentage of lithium difluorooxalate borate is 0.5%, the mass percentage of lithium salt is 12.6%, and the sum of the mass percentages of the organic solvent and the fluorinated solvent is 85.9%;
[0099] (2) Preparation of positive electrode sheet
[0100] Add appropriate amount of Al(NO3) 3.9 H 20 C.C 10 H 25 NbO5 and H2NCONH2 were dissolved in anhydrous ethanol, and then the cathode precursor was added. The mixture was calcined at 300 °C for 4 h, and then calcined in an O2 atmosphere at 750 °C for 6 h to obtain the modified sample Li(Ni 0.6 Mn 0.3 Co 0.1 Al 0.02 Nb 0.005 )O2, then the modified positive electrode material, conductive agent acetylene black (Super P) and binder polyvinylidene fluoride (PVDF) are mixed evenly according to the mass ratio of NMC631:Super P:PVDF=94:3:3, and evenly dispersed in 1-methyl-2-pyrrolidone (NMP) to form a uniform black slurry, and the mass percentage of Al element in the positive electrode active material is calculated to be 0.5%, and the mass percentage of Nb element in the positive electrode active material is 0.5%. After coating the mixed black slurry on both sides of the aluminum foil, it is baked, rolled, and cut into pieces to obtain the positive electrode sheet;
[0101] (3) Preparation of negative electrode sheet
[0102] The negative electrode active material graphite, the conductive agent acetylene black (Super P) and the binder SBR are mixed evenly in a mass ratio of graphite:SuperP:SBR=94:3:3, and evenly dispersed in deionized water to form a uniform black slurry. The mixed slurry is coated on both sides of the copper foil, and then baked, rolled and cut into pieces to obtain the negative electrode sheet;
[0103] (4) Production of soft pack batteries
[0104] The prepared positive electrode sheet, separator, and negative electrode sheet are stacked in order, with the separator being located between the positive and negative electrode sheets, and bare cells are obtained through winding, hot pressing, and ear welding. The bare cells are placed in an outer packaging aluminum-plastic film and baked in an oven at 85±10°C for 24 hours. The prepared electrolyte is injected into the dried battery, allowed to stand, formed, and divided to obtain a secondary battery.
[0105] Embodiments 2 to 7
[0106] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the mass percentage of the fluorinated solvent in the electrolyte is changed by adjusting the addition amount of the fluorinated solvent.
[0107] Embodiments 8 to 13
[0108] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the mass percentage of the aluminum element in the positive electrode active material is changed by adjusting the addition amount of the substance containing the aluminum element.
[0109] Embodiments 14 to 19
[0110] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the mass percentage of the niobium element in the positive electrode active material is changed by adjusting the addition amount of the substance containing the niobium element.
[0111] Embodiments 20 to 24
[0112] The embodiment of the present application provides a secondary battery. The difference between the secondary battery and the embodiment 1 is that the mass percentage of lithium difluorooxalatoborate in the electrolyte is changed by adjusting the addition amount of lithium difluorooxalatoborate.
[0113] Embodiments 25-26
[0114] The embodiment of the present application provides a secondary battery, which is different from the embodiment 1 in that the change of Y is achieved by adjusting the addition amount of lithium difluorooxalatoborate, fluorinated solvent, aluminum-containing substance or niobium-containing substance.
[0115] Comparative Examples 1-2
[0116] The comparative example of the present application provides a secondary battery, which is different from Example 1 in that the change of Y is achieved by adjusting the addition amount of lithium difluorooxalatoborate, fluorinated solvent, aluminum-containing substance or niobium-containing substance.
[0117] In the secondary batteries provided in the embodiments and comparative examples, the mass percentages of lithium difluorooxalatoborate and fluorinated solvent in the electrolyte, and the mass percentages of aluminum and niobium in the positive electrode active material are shown in Table 1;
[0118] The tests of the initial internal resistance, cycle performance, and internal resistance growth rate before and after the cycle of the secondary batteries provided in the embodiments and comparative examples include the following:
[0119] 1) Normal temperature DCR test: At 25±2℃, charge the secondary battery 1C to 4.5V, then discharge it at 1C capacity for 30min, adjust it to 50% SOC, discharge it at 10C constant current pulse for 10s, modulate it to 50% SOC according to the above SOC adjustment method, and charge it for 10s, calculate DCR = (voltage before pulse discharge - voltage after pulse discharge) / discharge current * 100%. After 500 cycles, test DCR again, DCR change rate = (DCR of 500 cycles - initial DCR) / initial DCR * 100%, and the recorded results are shown in Table 2;
[0120] 2) Normal temperature cycle performance test: At 25±2℃, the secondary battery is subjected to charge and discharge cycle test at a charge and discharge rate of 1C / 2C in the range of 2.8~4.5V, and the battery's first week discharge capacity and the discharge capacity after 500 cycles are recorded. 500-week capacity retention rate = 500-week discharge capacity / first week discharge capacity*100%, recorded data see Table 2;
[0121] Table 1
[0122]
[0123]
[0124] Table 2
[0125]
[0126]
[0127] As can be seen from Table 2, this application controls the secondary battery to meet When the secondary battery is subjected to the above conditions, the obtained secondary battery has a low internal resistance, excellent cycle performance, and a low internal resistance growth rate before and after the cycle; specifically, the initial DCR of the obtained secondary battery is below 17.8 mΩ, the cycle retention rate is above 82%, and the internal resistance growth rate is below 27.1%;
[0128] The results of Examples 1 to 25 and Comparative Examples 1 to 2 of the present application also show that when the value of Y is not within the range given in the present application, the overall performance of the obtained secondary battery is poor.
[0129] Finally, it should be noted that the above embodiments are intended to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, a person of ordinary skill in the art should understand that the technical solution of the present application may be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A secondary battery comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material; The electrolyte comprises lithium difluorooxalatoborate and a fluorinated solvent; The positive electrode active material includes aluminum and niobium; The secondary battery satisfies: 0.020≤Y≤0.48; in, C% is the mass percentage of lithium difluorooxalatoborate in the electrolyte; W1% is the mass percentage of the fluorinated solvent in the electrolyte; W2% is the mass percentage of aluminum in the positive electrode active material; W3% is the mass percentage of niobium element in the positive electrode active material.
2. The secondary battery according to claim 1, wherein At least one of the following is met: a. The mass percentage C of the lithium difluorooxalatoborate in the electrolyte is 0.1-5%; b. The mass percentage W1 of the fluorinated solvent in the electrolyte is 1-50%; c. The mass percentage W2 of the aluminum element in the positive electrode active material is 0.1-1%; d. The mass percentage W3 of the niobium element in the positive electrode active material is 0.1-1%.
3. The secondary battery according to claim 1, wherein The ratio of W2 to W3 is (1-5):
1.
4. The secondary battery according to claim 1, wherein The ratio of C and W1 is (0.01-0.3):
1.
5. The secondary battery according to claim 1, wherein The ratio of C and W2 is (1-6):
1.
6. The secondary battery according to claim 1, wherein The fluorinated solvent includes at least one of fluorinated carbonates, fluorinated carboxylates, fluorinated ethers, and fluorinated nitriles having 3 to 20 carbon atoms.
7. The secondary battery according to claim 1, wherein The electrolyte also includes lithium salt, organic solvent and additives; based on the electrolyte, the mass percentage of the lithium salt is 8-20%, the mass percentage of the organic solvent is 80-90%, and the mass percentage of the additive is 0.5-10%.
8. The secondary battery according to claim 7, wherein: The lithium salt includes at least one of lithium hexafluorophosphate, lithium difluorophosphate, lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate), lithium bis(fluorosulfonyl)imide, and lithium bis(trifluoromethylsulfonyl)imide; and / or the organic solvent comprises at least two of ethylene carbonate, propylene carbonate, butylene carbonate, trifluoroethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, methylpropyl carbonate, diphenyl carbonate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, ethyl 2,2-difluoroacetate, methyl 2,2-difluoroacetate, methyl 2,3,3,3-tetrafluoropropionate, γ-butyrolactone, acetonitrile, and sulfolane; And / or, the additive includes at least one of a silicon-containing additive, a sulfur-containing additive, and a cyclic carbonate additive.
9. The secondary battery according to claim 1, wherein The positive electrode active material includes Li a Ni x Co y Mn z M b Al c Nb (1-x-y-z-c) At least one of the compounds shown in O2; Among them, 0.9≤a≤1.1, 0<x<1, 0<y<1, 0<z<1, 0≤b≤0.1; M is at least one of Zr, Zn, Cu, Cr, Mg, Fe, V, Y, Ti, In, La, Ce, Sr, Sb, and B.
10. The secondary battery according to claim 9, wherein 0.5<x<0.8, x / y≥2.
5.
11. An electrical device, characterized in that: The secondary battery comprises the secondary battery according to any one of claims 1 to 10.
Citation Information
Patent Citations
Secondary battery, method for manufacturing secondary battery, battery module, battery pack, and power device
CN116111177A
Lithium ion battery, battery and electric device
CN117154188A
Secondary battery, battery module, battery pack, and electric device
CN117203809A
Secondary battery and device
CN117393861A
Secondary battery, battery pack and electric equipment
CN118336079A