Winding type lithium ion battery
By adjusting the particle size of the ternary material and the width of the negative electrode groove, combining the positive electrode hole structure and lithium supplementation agent, the problems of poor circulation performance of the ternary material and large expansion of the silicon negative electrode in lithium-ion batteries are solved, and the circulation performance and energy of the battery are improved Density reduces the risk of lithium arc evolution of the battery.
Patent Information
- Application Number
- CN202411371154.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-03
AI Technical Summary
The ternary material has poor circulation performance in lithium-ion batteries, and the silicon negative electrode material expands, resulting in poor circulation performance of the battery and easy to produce black spots.
By adjusting the particle size of the ternary material and the first groove width on the negative electrode active material layer, combining the pore structure and lithium supplement agent on the positive electrode active material layer, the distribution and structure of the electrode material are optimized to improve the cycling performance and energy of the battery. density.
It effectively improves the circulation performance and energy density of lithium-ion batteries, reduces the battery arc lithium-ion problem, reduces the loss of active substances, and improves the liquid retention ability of the electrolyte and the long circulation performance of the battery.
Smart Images

Figure CN119069828A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of batteries, and in particular to a wound lithium-ion battery. Background Art
[0002] In the current power battery material system, ternary materials have gradually become the mainstream positive electrode materials due to their obvious advantages over lithium manganese oxide and lithium iron phosphate in terms of energy density. Silicon negative electrode materials have also become an important development direction for lithium battery negative electrode materials due to their ultra-high theoretical specific capacity (4200mAh / g).
[0003] However, the cycling performance of ternary materials is poor, and the silicon negative electrode system expands greatly, which makes it easier for black spots to form at the arc of the silicon negative electrode ternary battery during the cycle process, which also leads to poor cycling performance.
[0004] Based on this, how to improve the cycle performance of ternary-silicon system batteries and reduce expansion is a technical problem that needs to be solved urgently. Summary of the invention
[0005] The present application provides a wound lithium-ion battery, which alleviates the problem of arc lithium deposition in the battery and improves the battery cycle performance by adjusting the particle size of the ternary material and the width of the first groove.
[0006] The present invention provides a wound lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator located between the positive electrode sheet and the negative electrode sheet;
[0007] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises a ternary material;
[0008] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a carbon material and a silicon-based material;
[0009] The negative electrode active material layer is evenly provided with a plurality of first grooves on the entire surface, and the width L1 of the first groove and the particle size Dv50 of the ternary material satisfy the formula: 1+0.25 / Dv50≤L1≤9+4000 / Dv50;
[0010] L1 is 1~500μm, and Dv50 is 5μm~15μm.
[0011] In a possible implementation manner, the depth h2 of the first groove is approximately equal to the particle size Dv50 of the carbon material. (1) Satisfy the formula: 4≤0.05*h2*Dv50 (1) ≤18.75, Dv50(1) The units of and h2 are both μm.
[0012] In a possible implementation, the positive electrode active material layer is provided with holes, and a lithium supplement agent is provided in the holes;
[0013] In a possible implementation, the depth of the pores is 1 μm to 20 μm, the pore diameter is 20 to 100 μm, and the pore spacing is 10 to 400 μm;
[0014] In a possible implementation, the depth of the pores is 50 μm to 200 μm, the pore diameter is 1 to 10 μm, and the pore spacing is 2 to 400 μm;
[0015] In a possible implementation, the lithium supplement is at least one of a binary lithium-containing compound and a ternary lithium-containing compound, preferably Li6CoO4 or Li5FeO4;
[0016] In a possible implementation, based on the mass of the positive electrode active material, the content y1wt% of the lithium supplement agent satisfies 0.1wt%≤y1wt%≤2.0wt%, preferably 0.1wt%≤y1wt%≤1.0wt%.
[0017] In a possible implementation, the thickness H1 of the positive electrode active material layer, the content y1 of the lithium supplement agent and the particle size Dv50 of the ternary material satisfy the formula Dv50*H1 / 4000≤y1≤Dv50*H1 / 2000+1; H1≤300 μm.
[0018] In a possible implementation manner, a second groove area is provided in the arc region of the positive electrode plate;
[0019] In a possible implementation manner, the width of the second groove area is 5 mm to 20 mm;
[0020] In a possible implementation manner, a depth h1 of the second groove region is 1 μm to 45 μm.
[0021] In a possible implementation manner, the depth h1 of the second groove area and the particle size Dv50 of the ternary material satisfy the formula: 20 / Dv50≤h1≤10+350 / Dv50.
[0022] In a possible implementation manner, the proportion y2 of the silicon-based material in the negative electrode active material satisfies 5wt%≤y2≤20wt%; the proportion y3 of the carbon material in the negative electrode active material satisfies 80%≤y3≤95%;
[0023] In a possible implementation, the silicon-based material includes a silicon-carbon material and a silicon-oxygen material;
[0024] In a possible implementation, the proportion y2(1) of the silicon-carbon material in the silicon-based material and the proportion y2(2) of the silicon-oxygen material in the silicon-based material satisfy: 0.4≤y2(1) / y2(2)≤2.
[0025] In a possible embodiment, the particle size of the carbon material is 8 μm ≤ Dv50 (1) ≤23μm, particle size of silicon carbon material 4μm≤Dv50 (2) ≤16μm, particle size of silicon oxide material 3μm≤Dv50 (3) ≤10μm;
[0026] The carbon material Dv50 (1) , Dv50 of silicon carbon material (2) And Dv50 of silicon oxide material (3) Meets: Dv50 (1) ≤Dv50 (2) +Dv50 (3) ≤2*Dv50 (1) .
[0027] In a possible implementation manner, the thickness H2 of the negative electrode active material layer is about the same as the thickness Dv50 of the carbon material. (1) Satisfy: 0.1*H2≤9*Dv50 (1) +10≤H2; thickness of negative electrode active material layer H2≤300μm;
[0028] In a possible implementation manner, the interval between two adjacent first grooves is 0.5 mm to 2 mm;
[0029] In a possible implementation manner, a depth h2 of the first groove is 0.3 μm to 45 μm.
[0030] In a possible implementation, the electrolyte includes additive A, and the additive A is a nitrile and / or ether nitrile additive;
[0031] In a possible implementation manner, the content w1 of the additive A in the electrolyte satisfies: 2%≤w1≤13%;
[0032] In a possible embodiment, the additive A is selected from one or more of ethylene glycol di(2-cyanoethyl) ether, ethylene glycol di(4-cyanobutyl) ether, 1,2,3-tri(cyanoethoxy)propane, diethylene glycol di(2-cyanoethyl) ether, tetraethylene glycol di(2-cyanoethyl) ether and ethylene glycol (bis) propionitrile ether;
[0033] In a possible implementation, the electrolyte includes additive B, and additive B is a negative electrode film-forming additive;
[0034] In a possible implementation, the additive B is selected from one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC) and an organic silane compound;
[0035] In a possible implementation manner, the content w2 of the additive B in the electrolyte satisfies: 0.1%≤w2≤5%.
[0036] The length direction of the first groove is parallel to the width direction of the negative electrode sheet.
[0037] The technical solution of this application has the following advantages:
[0038] The lithium-ion battery of the present invention comprises a positive electrode plate, a negative electrode plate, an electrolyte and a separator located between the positive electrode plate and the negative electrode plate; the positive electrode plate comprises a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises a ternary material; the negative electrode plate comprises a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector, the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a carbon material and a silicon-based material; a plurality of first grooves are uniformly arranged on the entire surface of the negative electrode active material layer, and the width L1 of the first groove and the particle size Dv50 of the ternary material satisfy the formula: 1+0.25 / Dv50≤L1≤9+4 / Dv50; L1 is 1 to 500 μm, and Dv50 is 5 μm to 15 μm. The combination of the ternary positive electrode and the silicon negative electrode, while bonding the wires, can improve the expansion and interface problems of the silicon negative electrode while increasing the energy density, ultimately achieving high energy density and high cycle performance. The particle size of the ternary material and the width of the first groove are adjusted to alleviate the arc lithium precipitation problem of the battery cell and improve the battery cycle performance. As the particle size of the ternary material increases, the consumption of electrolyte is reduced, the arc interface problem will be weakened, and the width of the first groove can be appropriately reduced without causing excessive loss of active materials.
[0039] Additional aspects and advantages of the embodiments of the present application will be described and shown in part in the subsequent description, or explained through the implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0041] Figure 1 Schematic diagram of the lithium supplementation structure in the positive electrode plate;
[0042] Figure 2 The front view (top) and top view (bottom) of the negative electrode sheet;
[0043] Figure 3 The front view (top) and top view (bottom) of the positive electrode.
[0044] The reference numerals are described as follows:
[0045] 1-lithium supplement; 2-first groove; 3-second groove area. DETAILED DESCRIPTION
[0046] The following examples are provided for a better understanding of the present application, but are not limited to the best implementation mode described, and do not limit the content and protection scope of the present application. Any product identical or similar to the present application obtained by anyone under the inspiration of the present application or by combining the features of the present application with other prior arts shall fall within the protection scope of the present application.
[0047] In the description of the present application, it should be noted that the terms "inside", "outside", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0048] The present invention provides a wound lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator located between the positive electrode sheet and the negative electrode sheet;
[0049] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises a ternary material;
[0050] The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a carbon material and a silicon-based material;
[0051] The negative electrode active material layer is evenly provided with a plurality of first grooves on the entire surface, and the width L1 of the first groove and the particle size Dv50 of the ternary material satisfy the formula: 1+0.25 / Dv50≤L1≤9+4000 / Dv50;
[0052] L1 is 1~500μm, and Dv50 is 5μm~15μm.
[0053] The ternary system with a silicon-based negative electrode can improve the energy density of the system, reduce the coating surface density and compaction, and improve the system dynamics. However, the lithium storage mechanism of the silicon-based negative electrode is an alloying reaction mechanism, which will cause severe volume expansion during the charging process, which is easy to increase the risk of cracking and leakage of the battery cell. In addition, the repeated volume changes during the battery charging and discharging process will accelerate the structural collapse of the electrode material and the continuous side reactions on the negative electrode side (accelerate the consumption of the electrolyte), reduce the initial coulomb efficiency of the battery and affect the cycle life. Therefore, when introducing the silicon-based negative electrode, it is necessary to consider solving the problem of its large expansion. Based on this, by evenly setting the first groove on the entire surface of the negative electrode, adjusting the pore structure of the negative electrode pole piece, and setting up sufficient buffer margin for the expansion of the silicon-based negative electrode, the problem of large volume expansion of the silicon-based negative electrode during the charging and discharging process can be improved. At the same time, it can also further improve the infiltration of the electrolyte into the pole piece and the ability of the pole piece to retain the electrolyte during the long cycle process, thereby improving the power and cycle performance of the battery cell.
[0054] In order to alleviate the problem of arc lithium deposition in the battery and improve the battery cycle performance, the present invention is achieved by adjusting the particle size of the ternary material and the width of the first groove. The particle size of the ternary material is within the scope of this application, the consumption of electrolyte is small, the arc interface problem will be weakened, and accordingly, the width of the first groove can be appropriately reduced, which will not cause excessive loss of active material, thereby avoiding lithium deposition caused by excessive loss and low CB value.
[0055] In a possible implementation manner, the depth h2 of the first groove is approximately equal to the particle size Dv50 of the carbon material. (1) Satisfy the formula: 4.347≤0.005*h2*Dv50 (1) ≤18.75, the unit of h2 is μm.
[0056] The depth h2 of the first groove and the particle size Dv50 of the carbon material (1) Satisfying the above formula can improve the problem of large expansion of the negative electrode while avoiding large loss of negative electrode activity that affects the uniformity of the electrode sheet. Increasing the particle size of the carbon material can slow down the consumption rate of the electrolyte on the negative electrode side, so that the depth h2 of the first groove does not need to be too deep, and will not cause excessive loss of active materials. The synergy between battery cell performance and cost can be achieved by adjusting the particle size of the carbon material and the depth of the first groove.
[0057] In one possible embodiment, holes are provided on the positive electrode active material layer, and lithium replenishers are provided in the holes. The formation of the negative electrode SEI film during the battery formation stage will consume a large amount of active lithium (especially in a high-capacity silicon-based negative electrode material system), which will affect the battery's first-week coulomb efficiency and battery capacity. Positive electrode lithium replenishment is an effective way to solve this problem. Positive electrode lithium replenishment technology is to add lithium replenishment materials to the positive electrode. During the battery charging process, the lithium replenishment materials on the surface of the positive electrode plate will decompose and release active lithium to make up for the irreversible active lithium loss caused by the growth of the negative electrode SEI. The positive electrode plate containing a lithium replenisher of the present invention has the advantages of relatively stable chemical properties, easy processing, low price and high lithium replenishment capacity.
[0058] The traditional mechanical mixing and coating method has a relatively bumpy lithium supplementation process, and it takes a long time to build an ion path. Unlike the traditional slurry mixing lithium supplementation method, the present invention can significantly increase the effective contact area between the later lithium film and the negative electrode by making holes on the positive electrode surface and filling the lithium supplementation agent, and can form more abundant electron pathway sites on the contact interface. These electron pathway sites can reduce the local current density gathered at the electron pathway, maintain the structural characteristics of the electron pathway during the pre-lithiation process, and thus improve the lithium source utilization rate; for battery performance, the lithium supplementation method of the present invention can improve the battery capacity retention rate and extend the life.
[0059] In a possible implementation, the holes on the positive electrode active material layer are arranged on the side away from the current collector, the transmission impedance will be lower and the kinetics on the positive electrode side will be better.
[0060] The holes on the positive electrode active material layer can be made by mechanical punching, embossing, etc. After the holes are made, the lithium replenisher is coated into the holes. The positive electrode point coating lithium replenisher technology improves the stability of the positive electrode side.
[0061] In a possible implementation, the positive electrode plate is pore-formed by mechanical punching, wherein the pores have a depth of 1 μm to 20 μm, a pore diameter of 20 to 100 μm, and a pore spacing of 10 to 400 μm; the pore spacing refers to the distance between the centers of two holes.
[0062] In a possible implementation, the positive electrode sheet is pore-formed by positive electrode embossing, wherein the depth of the pores is 50 μm to 200 μm, the pore diameter is 1 to 10 μm, and the pore spacing is 2 to 400 μm;
[0063] Preferably, the lithium supplement is at least one of a binary lithium-containing compound and a ternary lithium-containing compound, preferably Li6CoO4 or Li5FeO4;
[0064] Preferably, based on the mass of the positive electrode active material, the content y1wt% of the lithium supplement agent satisfies: 0.1wt%≤y1wt%≤2.0wt%, preferably 0.1wt%≤y1wt%≤1.0wt%.
[0065] In a possible implementation, the thickness H1 of the positive electrode active material layer, the content y1wt% of the lithium supplement and the particle size Dv50 of the ternary material satisfy the formula Dv50*H1 / 4000≤y1≤Dv50*H1 / 2000+1; H1≤300μm.
[0066] The increase in the particle size Dv50 of the ternary material and the thickness H1 of the positive electrode active material layer will lead to a longer lithium ion diffusion path, resulting in a higher concentration polarization when the lithium ions diffuse internally, which in turn affects the kinetics on the positive electrode side, reducing the battery's first-week coulomb efficiency and battery capacity (more lithium supplements are needed at this time). If the content of the lithium supplement is too high, the risk of gas production in the battery will increase. During the design process, the present invention comprehensively considers the synergistic relationship between the particle size of the ternary material, the thickness of the positive electrode active material layer and the content of the lithium supplement y1wt%, thereby reducing the risk of gas production while improving the battery's first-week coulomb efficiency and battery capacity.
[0067] In a possible implementation, a second groove area is provided in the arc region of the positive electrode plate.
[0068] The arc area refers to the arc-shaped area where the edge of the wound battery cell is not pressed after pressing.
[0069] Ternary materials have large BET and small particle size, which consume electrolyte quickly. In addition, in order to pursue higher battery capacity and energy density, the compaction density and coating surface density of the pole piece will inevitably increase, which makes it easier for black spots and lithium precipitation to appear at the arc of the battery cell due to electrolyte bridge breakage. Therefore, it is particularly important to increase the amount of liquid retained at the arc of the battery cell and improve the interface problem on the anode side.
[0070] The present invention provides a second groove area at the arc of the positive electrode sheet, which can improve the pore structure of the positive electrode sheet, increase the CB value, improve the electrolyte infiltration of the positive electrode sheet and the electrolyte retention capacity of the positive electrode sheet during a long cycle, and improve the problem of lithium precipitation in the negative electrode arc; in addition, the mechanical strength of the second groove area of the positive electrode sheet is reduced, and it has higher elasticity, which can effectively alleviate the volume expansion at the arc. The present invention can alleviate the problem of lithium precipitation and abnormal thickness expansion of this part, thereby improving the power and cycle performance of the battery cell.
[0071] CB value = negative electrode active material gram capacity × negative electrode coating surface density × negative electrode active material content ratio ÷ (positive electrode active material gram capacity × positive electrode coating surface density × positive electrode active material content ratio).
[0072] Coating surface density = coating mass / coating area.
[0073] The smaller the CB value, the greater the risk of lithium plating.
[0074] The positive electrode plate provided by the present invention can increase the electrolyte infiltration effect and speed at the positive arc, increase the liquid storage space, and improve the liquid storage amount, effectively solving the problems of poor electrolyte infiltration and insufficient electrolyte in the late cycle of the ternary-silicon material system battery, thereby improving the battery cycle life and capacity retention rate. In a possible implementation, the second groove area is made by laser surface scanning, wire punching, drilling or thinning.
[0075] Preferably, the width of the second groove area is 5 mm to 20 mm;
[0076] Preferably, the depth h1 of the second groove region is 1 μm to 45 μm;
[0077] Preferably, the CB value of the arc region after the second groove region is prepared in the arc region is 1.05-1.25; the CB value of the arc region after the second groove region is prepared is increased by 0.05-0.1 compared with the CB value when the second groove region is not prepared.
[0078] In a possible implementation, a matrix channel region is prepared by local pore creation to increase the CB and liquid retention volume at the arc: the second groove region is composed of at least one matrix channel region;
[0079] Preferably, the second groove area is composed of more than two matrix channel areas, and the distance between two adjacent matrix channel areas is 0mm-5mm;
[0080] Preferably, the matrix channel region includes more than two holes, with a hole depth of 1 μm to 20 μm and a hole diameter of 20 to 200 μm;
[0081] In a possible embodiment, a matrix line area is prepared by local line making to increase the CB and liquid retention amount at the arc: the second groove area is composed of at least one matrix line area; the interval between two adjacent lines in the matrix line area is 0.1mm~2mm, the width of each line in the matrix line area is 1μm~500μm, and the depth of the line is 1μm~20μm.
[0082] In one possible implementation, the depth h1 of the second groove area and the particle size Dv50 of the ternary material satisfy the formula: 20 / Dv50≤h1≤10+350 / Dv50. If the depth of the second groove area is too shallow, the improvement of the arc problem is not obvious. If the depth of the second groove area is too deep, the positive electrode activity loss is large and the electrode uniformity is affected. In addition, increasing the particle size of the ternary material can slow down the consumption rate of the electrolyte on the positive electrode side (reduce the arc problem), so that the depth h of the second groove area does not need to be too deep, and will not cause excessive loss of active materials on the positive electrode side. Therefore, the synergy between battery cell performance and cost can be achieved by adjusting the particle size of the ternary material and the depth of the second groove area.
[0083] In a possible implementation, the proportion y2 of the silicon-based material in the negative electrode active material satisfies 5wt%≤y2≤20wt%; the proportion y3 of the carbon material in the negative electrode active material satisfies 80%≤y3≤95%. In the silicon-carbon material, the ratio of the Si element content to the C element content satisfies 0.2≤Si / C≤1.8; in the silicon-oxygen material, the ratio of the Si element content to the O element content satisfies 0.1≤Si / O≤1.2; in the negative electrode active material, the ratio of the Si element content to the O element content satisfies 0.4≤Si / O≤2.5. The present invention improves the energy density of the battery by adding an appropriate amount of silicon-based material to the carbon material, and regulates the ratio of Si, O, and C in the silicon-carbon material and the silicon-oxygen material, which can improve the energy density of the battery while alleviating the problem of large expansion of the silicon-doped negative electrode. In addition, the silicon-based material provided by the present invention can provide a large energy density margin for the battery system due to its large theoretical specific capacity (4200mAh / g). Based on this, the coating surface density can be appropriately reduced during battery cell design to further improve the dynamics on the positive and negative electrode sides.
[0084] In a possible implementation, the silicon-based material includes a silicon-carbon material and a silicon-oxygen material;
[0085] Preferably, the proportion of silicon-carbon material in silicon-based material y2(1) and the proportion of silicon-oxygen material in silicon-based material y2(2) satisfy: 0.4≤y2(1) / y2(2)≤2. Silicon-carbon material has lower cost and higher initial efficiency, but larger battery expansion; silicon-oxygen material has smaller particles, more uniform dispersion and more compact and stable material structure, which makes the volume expansion rate of the material lower, but the silicon-oxygen cycle performance is relatively poor. The present invention coordinates the ratio of the two materials to take into account both battery stability and cost.
[0086] Preferably, the silicon in the silicon-carbon material is located in a carbon skeleton structure.
[0087] Preferably, the silicon-oxygen material includes amorphous silicon.
[0088] Preferably, the carbon material includes at least one of natural graphite, artificial graphite, hard carbon and soft carbon.
[0089] In a possible embodiment, the particle size of the carbon material is 8 μm ≤ Dv50 (1) ≤23μm, particle size of silicon carbon material 4μm≤Dv50 (2) ≤16μm, particle size of silicon oxide material 3μm≤Dv50 (3) ≤10μm;
[0090] The carbon material Dv50 (1) , Dv50 of silicon carbon material (2) And Dv50 of silicon oxide material (3) Meets: Dv50 (1) ≤Dv50 (2) +Dv50 (3) ≤2*Dv50 (1) .
[0091] The particle size of the silicon-based material is limited within the scope of this application, which can avoid the problem of increased ion transmission distance and increased impedance due to excessively large particle size; at the same time, it can avoid the problem of easy agglomeration due to too small particle size, which is not conducive to the process and increases the consumption of electrolyte on the negative electrode side.
[0092] The particle sizes of silicon-based materials and carbon materials satisfy the above relationship, which can avoid the influence of poor particle size uniformity on the liquid phase transfer of electrodes and the increase of interfacial charge transfer impedance, which is more conducive to Li + Solid phase diffusion; at the same time, it can avoid affecting the electrode processing, compaction, and dynamic performance of the battery.
[0093] In a possible implementation, the first groove is made by laser surface scanning, line punching, drilling or thinning. The technical effect is to increase the CB value and liquid retention volume of the arc area to provide sufficient buffer margin for the expansion of the silicon negative electrode, so as to improve the problem of large volume expansion of the silicon-doped negative electrode during the charging and discharging process, and at the same time alleviate the lithium deposition on the entire surface of the negative electrode.
[0094] In a possible implementation manner, the thickness H2 of the negative electrode active material layer is about the same as the thickness Dv50 of the carbon material. (1) Satisfy: 0.1*H2≤9*Dv50 (1) +10≤H2; the thickness of the negative electrode active material layer H2≤300μm; the thickness of the negative electrode active material layer is too thin to significantly improve the battery energy density; the thickness of the negative electrode active material layer is too thick and the increase of the negative electrode material particle size will lead to a longer lithium ion diffusion path, resulting in higher concentration polarization, affecting the negative electrode side kinetics. Satisfying the above formula of the present invention can improve the battery energy density while ensuring the battery kinetic performance.
[0095] Preferably, the interval between two adjacent first grooves is 0.5 mm to 2 mm;
[0096] Preferably, the depth h2 of the first groove is 0.3 μm to 45 μm.
[0097] In one possible implementation, the tensile strength of the current collector on the negative electrode side is ≥130 MPa; the negative electrode coating surface density m≤15 mg / cm 2 .
[0098] In a possible embodiment, the first groove is prepared by making lines on the entire surface of the negative electrode. One line serves as a first groove to provide sufficient buffer margin for the expansion of the silicon negative electrode, increase the CB and liquid retention at the arc, and the interval between two adjacent lines is 0.5mm to 2mm. The width of the line is 1μm to 500μm, and the depth of the line ranges from 1μm to 30μm.
[0099] In one possible implementation, the first groove is prepared by local thinning of the negative electrode, sufficient buffer margin is established for the expansion of the silicon negative electrode, CB and liquid retention at the arc are increased, the thinning interval is 0.5mm~2mm, the thinning width is 1μm~500μm, and the thinning thickness is 1μm~20μm.
[0100] In a possible implementation, the electrolyte includes additive A, and the additive A is a nitrile and / or ether nitrile additive.
[0101] The positive electrode material battery exhibits strong oxidizing properties during discharge, and it is easy to react with the electrolyte to cause consumption of the positive electrode material and dissolution of excessive metal ions. Ternary materials have poor stability, so the ternary system battery needs to optimize the positive electrode protective agent in the electrolyte to maintain the stability of the positive electrode side. With respect to the protection of the positive electrode side, the present invention achieves this by adding nitrile / ether nitrile additives to the electrolyte. During the discharge process, the CO bond of the ether nitrile additive undergoes an oxidation reaction, forming a protective layer on the positive electrode side. In addition, the cyanide group can continue to react with the cobalt ion to form a more solid protection.
[0102] The grooves of the positive and negative pole pieces are achieved by destroying the surface of the pole pieces, which increases the surface burrs. Nitrile and / or ether nitrile additives in the electrolyte can be oxidized to form a film at the positive electrode. Since the surface of the groove area is uneven and the current distribution is uneven, the nitrile and / or ether nitrile additives are preferentially formed on the uneven points to reduce the safety risks caused by the uneven current brought by these protrusions (burrs). At the same time, the preferential film formation of nitrile and / or ether nitrile additives makes the surface of the positive electrode material relatively smooth, reduces the specific surface area, and reduces the impedance of the interface.
[0103] Preferably, the content w1 of the additive A in the electrolyte satisfies: 2%≤w1≤13%. Adding the additive A in the above range can provide good protection for the positive electrode side while avoiding the risk of lithium deposition and water drop in the battery cell cycle caused by excessive electrolyte impedance.
[0104] Preferably, the additive A is selected from one or more of ethylene glycol di(2-cyanoethyl) ether, ethylene glycol di(4-cyanobutyl) ether, 1,2,3-tri(cyanoethoxy)propane, diethylene glycol di(2-cyanoethyl) ether, tetraethylene glycol di(2-cyanoethyl) ether and ethylene glycol (bis)propionitrile ether.
[0105] In a possible embodiment, the electrolyte includes additive B, which is a negative electrode film-forming additive. The volume expansion of the silicon-doped negative electrode during the charge and discharge process is much greater than that of the traditional graphite system, so the electrolyte of silicon-based LIBs puts forward further requirements for film-forming additives. In order to protect the silicon-doped negative electrode side, the present invention adds negative electrode film-forming additives such as fluoroethylene carbonate (FEC), vinylene carbonate (VC) and organosilane compounds to the electrolyte. The additive B of the present invention is more suitable for silicon-based LIBs, forming a more stable protection to the negative electrode side, and further alleviating the safety problems caused by the large expansion of silicon.
[0106] Preferably, the content w2 of the additive B in the electrolyte satisfies: 0.1%≤w2≤5%.
[0107] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.
[0108] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0109] The electrolyte used in the lithium ion secondary battery of the present application may include any technology disclosed in the prior art.
[0110] The present application is further described in detail below in conjunction with specific examples, which should not be construed as limiting the scope of protection claimed in the present application. In all examples and comparative examples of the present application, the unit wt% represents the mass percentage content.
[0111] Example 1
[0112] This embodiment provides a method for preparing a wound lithium-ion battery, comprising:
[0113] (1) Preparation of positive electrode sheet: The ternary material NCM613 is used as the positive electrode active material, and the particle size of the positive electrode active material is Dv50 = 10 μm. The positive electrode active material, the conductive agent carbon black and the binder polyvinylidene fluoride are added to a stirring tank in a mass ratio of 96.5:2.0:1.5, and NMP solvent is added. After sufficient stirring, the mixture is passed through a 200-mesh sieve to prepare a positive electrode slurry. The positive electrode slurry is coated on an aluminum foil using a coating machine to prepare a positive electrode active material layer. The thickness of the positive electrode active material layer is H1 = 100 μm. Then, the positive electrode slurry is coated on an aluminum foil using a coating machine. The positive electrode active material layer is coated on an aluminum foil with a thickness of H1 = 100 μm. Figure 1 As shown, the positive electrode active material layer is subjected to lithium replenishment operation (wherein, mechanical punching is used to form pores in the positive electrode active material layer, with a pore depth of 3 μm, a pore diameter range of 50 μm, and a pore spacing range of 100 μm; the content of lithium replenisher 1 y1wt%=1wt%, and the lithium replenisher 1 is Li6CoO4). Then, it is subjected to rolling and slitting processing.
[0114] The cut product is Figure 2 As shown, laser scanning is performed on the positive electrode active material layer to prepare the second groove area 3, wherein the surface scanning depth is 7 μm (i.e., the second groove area 3 depth h1) and the width is 10 mm (i.e., the second groove area width). After laser scanning, the positive electrode sheet is obtained after cleaning and sheeting.
[0115] (2) Preparation of negative electrode sheet: 90wt% artificial graphite + 10wt% silicon-based material is used as the negative electrode active material. The silicon-based material includes silicon-carbon material and silicon-oxygen material. The silicon-carbon material accounts for y2(1) = 50wt% of the silicon-based material, and the silicon-oxygen material accounts for y2(2) = 50wt% of the silicon-based material. The silicon-carbon material is silicon carbide (SiC), and the silicon-oxygen material is SiO. The particle size of artificial graphite is Dv50 (1) =10μm, particle size of silicon carbon material Dv50 (2) =12μm, particle size of silicon oxide material Dv50 (3) =4μm.
[0116] The negative electrode active material, the conductive agent carbon nanotubes and the binder polyethylene oxide were added to a stirring tank in a mass ratio of 98.2:0.6:1.2, and deionized water solvent was added, fully stirred, and passed through a 150-mesh screen to prepare a negative electrode slurry. The negative electrode slurry was coated on a copper foil using a coating machine to prepare a negative electrode active material layer with a thickness of H2 = 110 μm, and then rolled and slit.
[0117] The cut products are based on Figure 3 The negative electrode active material layer is wired on the entire surface to prepare a plurality of first grooves 2, each line being a first groove, wherein the interval between two adjacent lines is 1 mm, the line width is 50 μm (i.e., the first groove width L1), and the line depth range is 10 μm (i.e., the first groove depth h2); subsequently, the negative electrode sheet is obtained after cleaning and sheeting.
[0118] (3) Electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed at a volume ratio of 1:1, and then fully dried lithium salt LiPF6 is dissolved in the above mixed organic solvent at a ratio of 1 mol / L, and additives A and additive B are added to prepare an electrolyte.
[0119] Additive A is ethylene glycol di(2-cyanoethyl) ether, with a content w1=5wt%. Additive B is fluoroethylene carbonate, with a content w2=3wt%.
[0120] (4) Assembling the core: The positive electrode sheet, negative electrode sheet and separator are wound together to form a battery cell. Then it is packaged with aluminum plastic film, baked to remove moisture, and then injected with electrolyte. After subsequent treatments such as formation and secondary sealing, a lithium-ion battery is obtained.
[0121] Example 2
[0122] This embodiment is carried out with reference to the embodiment 1, except that the width L1 of the first groove is 409 μm.
[0123] Example 3
[0124] This embodiment is carried out with reference to the embodiment 1, except that the width L1 of the first groove is 3 μm.
[0125] Example 4
[0126] This embodiment is carried out with reference to the embodiment 1, except that Dv50=5 μm.
[0127] Example 5
[0128] This embodiment is carried out with reference to the embodiment 1, except that Dv50=15 μm.
[0129] Example 6
[0130] This example is carried out with reference to Example 1, except that the particle size Dv50 of the carbon material is (1) =8μm.
[0131] Example 7
[0132] This example is carried out with reference to Example 1, except that the particle size Dv50 of the carbon material is (1) =13μm.
[0133] Example 8
[0134] This embodiment is carried out with reference to the embodiment 1, except that the depth h2 of the first groove is 8.6 μm.
[0135] Example 9
[0136] This embodiment is carried out with reference to the embodiment 1, except that the depth h2 of the first groove is 37 μm.
[0137] Example 10
[0138] This embodiment is carried out with reference to the embodiment 1, except that the depth h2 of the first groove is 0.4 μm.
[0139] Embodiment 11
[0140] This example is carried out with reference to Example 1, except that the lithium supplement is Li5FeO4.
[0141] Example 12
[0142] This example is carried out with reference to Example 1, except that the content of the lithium supplement y1wt%=0.1wt%.
[0143] Embodiment 13
[0144] This example is carried out with reference to Example 1, except that the content of the lithium supplement agent y1wt%=2wt%.
[0145] Embodiment 14
[0146] This example is carried out with reference to Example 1, except that the content of the lithium supplement y1wt%=0.5wt%.
[0147] Embodiment 15
[0148] This example is carried out with reference to Example 1, except that the thickness of the positive electrode active material layer H1 = 150 μm.
[0149] Example 16
[0150] This example is carried out with reference to Example 1, except that the thickness of the positive electrode active material layer H1 = 80 μm.
[0151] Embodiment 17
[0152] This example is carried out with reference to Example 1, except that the content y1wt% of the lithium supplement is 5wt%.
[0153] Embodiment 18
[0154] This embodiment is carried out with reference to the embodiment 1, except that the depth h1 of the second groove region is 5 μm.
[0155] Embodiment 19
[0156] This embodiment is carried out with reference to the embodiment 1, except that the depth h1 of the second groove region is 45 μm.
[0157] Embodiment 20
[0158] This embodiment is carried out with reference to the embodiment 1, except that the depth h1 of the second groove region of the positive electrode sheet is 1 μm.
[0159] Embodiment 21
[0160] This embodiment is carried out with reference to the embodiment 1, except that 80 wt % artificial graphite + 20 wt % silicon-based material are used as the negative electrode active material.
[0161] Embodiment 22
[0162] This embodiment is carried out with reference to the embodiment 1, except that 95 wt % artificial graphite + 5 wt % silicon-based material are used as the negative electrode active material.
[0163] Embodiment 23
[0164] This embodiment is carried out with reference to the embodiment 1, except that the proportion of silicon-carbon material in the silicon-based material is y2(1)=65wt%, and the proportion of silicon-oxygen material in the silicon-based material is y2(2)=35wt%.
[0165] Embodiment 24
[0166] This embodiment is carried out with reference to the embodiment 1, except that the proportion of silicon-carbon material in the silicon-based material is y2(1)=30wt%, and the proportion of silicon-oxygen material in the silicon-based material is y2(2)=70wt%.
[0167] Embodiment 25
[0168] This embodiment is carried out with reference to the embodiment 1, except that the proportion of silicon-carbon material in the silicon-based material is y2(1)=80wt%, and the proportion of silicon-oxygen material in the silicon-based material is y2(2)=20wt%.
[0169] Embodiment 26
[0170] This embodiment is carried out with reference to the embodiment 1, except that the Dv50 of the silicon carbon material (2) =6μm.
[0171] Embodiment 27
[0172] This embodiment is carried out with reference to the embodiment 1, except that the Dv50 of the silicon carbon material (2) =16μm.
[0173] Embodiment 28
[0174] This embodiment is carried out with reference to the embodiment 1, except that the Dv50 of the silicon carbon material (3) =3μm.
[0175] Embodiment 29
[0176] This embodiment is carried out with reference to the embodiment 1, except that the Dv50 of the silicon carbon material (3) =8μm.
[0177] Embodiment 30
[0178] This example is carried out with reference to Example 1, except that the particle size of the artificial graphite is Dv50 (1) =10μm, particle size of silicon carbon material Dv50 (2) =16μm, particle size of silicon oxide material Dv50 (3) =10μm.
[0179] Embodiment 31
[0180] This example is carried out with reference to Example 1, except that the thickness of the negative electrode active material layer H2 = 300 μm.
[0181] Embodiment 32
[0182] This example is carried out with reference to Example 1, except that the thickness of the negative electrode active material layer H2 = 100 μm.
[0183] Embodiment 33
[0184] This example is carried out with reference to Example 1, except that the content of additive A in the electrolyte is w1=13wt%.
[0185] Embodiment 34
[0186] This example is carried out with reference to Example 1, except that the content of additive A in the electrolyte is w1=2wt%.
[0187] Embodiment 35
[0188] This example is carried out with reference to Example 1, except that the content of additive B in the electrolyte is w2 = 5 wt%.
[0189] Embodiment 36
[0190] This example is carried out with reference to Example 1, except that the content of additive B in the electrolyte, w2, is 0.1 wt%.
[0191] Embodiment 37
[0192] This example is carried out with reference to Example 1, except that the content of additive A in the electrolyte is w1=13wt%, and the content of additive B in the electrolyte is w2=5wt%.
[0193] Embodiment 38
[0194] This example is carried out with reference to Example 1, except that the content of additive A in the electrolyte is w1=2wt%, and the content of additive B in the electrolyte is w2=0.1wt%.
[0195] Embodiment 39
[0196] This embodiment is carried out with reference to the embodiment 1, except that the type of the positive electrode active material is NCM111.
[0197] Embodiment 40
[0198] This embodiment is carried out with reference to the embodiment 1, except that the type of positive electrode active material is NCM523.
[0199] Comparative Example 1
[0200] This comparative example is carried out with reference to Example 1, except that the negative electrode is not provided with the first groove.
[0201] Comparative Example 2
[0202] This comparative example is carried out with reference to Example 1, except that the first groove width L1 is 1000 μm.
[0203] Comparative Example 3
[0204] This comparative example is carried out with reference to Example 1, except that the first groove width L1 is 500 μm.
[0205] Table 1
[0206]
[0207]
[0208] Table 2
[0209]
[0210]
[0211] Test Case
[0212] Corresponding invention point parameter test method:
[0213] Calculation of liquid retention coefficient: Liquid retention coefficient = liquid retention amount / battery capacity. According to the production process, a certain amount of electrolyte is injected, and then the battery undergoes formation and sorting, and part of the electrolyte will be consumed. During the second sealing process, the excess electrolyte will be extracted and packaged. Therefore, liquid retention amount = battery cell mass + electrolyte injection amount - battery cell mass after second sealing.
[0214] Performance parameter test methods:
[0215] Furnace temperature test:
[0216] 1. Place the fully charged battery in the test chamber. The temperature of the test chamber is raised at a rate of (5±2)℃ / min. When the temperature in the chamber reaches 140℃±2℃, the constant temperature is maintained for 60 minutes.
[0217] 2. After the test is completed, go down to test the voltage and internal resistance, and take pictures after the test.
[0218] Cycle test:
[0219] 1. At 25°C, discharge at 0.2C to a cut-off voltage of 3.0V and let stand for 10 minutes;
[0220] 2.1C-50% SOC, 0.7C-100% SOC, charge to the upper limit voltage, cut-off current 0.05C, and stand for 10 minutes;
[0221] Measure the voltage, internal resistance, thickness, and DC internal resistance (1C 3s) at the first full charge;
[0222] 3.1C-50% SOC, 0.7C-100% SOC charged to the upper limit voltage, cut-off current 0.05C, cycle 600 times;
[0223] 4. After the cycle is completed, place the sample at room temperature and let it rest for about 2 hours. After the sample temperature cools to room temperature, measure the data under the fully charged state.
[0224] Table 3
[0225]
[0226]
[0227] Expansion rate at arc = (thickness at arc after cycle - thickness at arc before cycle) / thickness at arc before cycle
[0228] Main body expansion = (main body thickness after cycle - main body thickness before cycle) / main body thickness before cycle
[0229] Note: The thickness of the main body surface after the cycle refers to the overall thickness excluding the arc abnormality, which can be measured with a micrometer;
[0230] The furnace temperature passes the standard that the battery does not catch fire or explode.
[0231] If the arc and main surface expansion after 600T cycle is within 10%, the battery cell is considered to have good cycle performance and meet the standards.
[0232] From the comparison between the embodiment and the comparative example in Table 4, it can be seen that after 600 cycles, no black spots are generated on the arc and the main body surface of the battery of the present invention, and the cycle effect is significantly improved compared with the comparative example.
[0233] By comparing Example 1 with Example 7, it can be seen that 0.1*H2≤9*Dv50 is satisfied. (1) +10≤H2, can avoid the appearance of black spots at the arc and the main body surface during the battery cycle, while further improving the battery's liquid retention and reducing the expansion rate at the arc and the main body surface.
[0234] By comparing Example 1 with Example 10, it can be seen that 4≤0.05*h2*Dv50 is satisfied. (1) ≤18.75, which can avoid the appearance of black spots on the arc and the main surface during battery cycling, while further improving the battery's liquid retention and reducing the expansion rate of the arc and the main surface.
[0235] By comparing Example 1 with Example 12, it can be seen that satisfying Dv50*H1 / 4000≤y1≤Dv50*H1 / 2000+1 can compensate for the irreversible active lithium loss caused by the growth of SEI at the negative electrode, further improve the long cycle performance of the battery, and reduce the expansion rate of the arc and the main surface in the late cycle (after 500T).
[0236] By comparing Example 1 with Example 17, it can be seen that satisfying the lithium supplement content y1wt% satisfies 0.1wt%≤y1wt%≤2.0wt%, which can further increase the battery's liquid retention capacity and reduce the expansion rate of the arc and the main surface while avoiding the appearance of black spots at the arc and the main surface during the battery cycle.
[0237] By comparing Example 13 with Examples 1, 12, and 14, it can be seen that within the range of 0.1wt%≤y1wt%≤1.0wt%, the expansion rate of the arc and the main surface of the battery can be further improved.
[0238] By comparing Example 1 with Example 20, it can be seen that satisfying the formula: 20 / Dv50≤h1≤10+350 / Dv50 can avoid the appearance of black spots at the arc and the main surface during the battery cycle, while further reducing the expansion rate of the arc and the main surface.
[0239] By comparing Example 1 with Example 25, it can be seen that satisfying 0.4≤y2(1) / y2(2)≤2 can further improve the battery's liquid retention capacity and reduce the expansion rate of the arc and the main surface while avoiding the appearance of black spots at the arc and the main surface during the battery cycle.
[0240] It can be seen from the comparison between Example 1 and Example 30 that Dv50 is satisfied. (1) ≤Dv50 (2) +Dv50 (3) ≤2*Dv50 (1), which can further improve the battery's liquid retention capacity and reduce the expansion rate of the arc and the main surface while avoiding the appearance of black spots at the arc and the main surface during the battery cycle.
[0241] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A wound lithium-ion battery, characterized in that: It includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator between the positive electrode sheet and the negative electrode sheet; The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer located on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer comprises a positive electrode active material, and the positive electrode active material comprises a ternary material; The negative electrode sheet comprises a negative electrode current collector and a negative electrode active material layer located on at least one surface of the negative electrode current collector, wherein the negative electrode active material layer comprises a negative electrode active material, and the negative electrode active material comprises a carbon material and a silicon-based material; The negative electrode active material layer is evenly provided with a plurality of first grooves on the entire surface, and the width L1 of the first groove and the particle size Dv50 of the ternary material satisfy the formula: 1+0.25 / Dv50≤L1≤9+4000 / Dv50; L1 is 1~500μm, and Dv50 is 5μm~15μm.
2. The wound lithium-ion battery according to claim 1, characterized in that: The depth h2 of the first groove is related to the particle size Dv50 of the carbon material. (1) Satisfy the formula: 4≤0.05*h2*Dv50 (1) ≤18.75, Dv50 (1) The units of and h2 are both μm.
3. The wound lithium-ion battery according to claim 1, characterized in that: The positive electrode active material layer is provided with holes, and the lithium supplement agent is arranged in the holes; Preferably, the depth of the pores is 1 μm to 20 μm, the pore diameter is 20 to 100 μm, and the pore spacing is 10 to 400 μm; Preferably, the depth of the pores is 50 μm to 200 μm, the pore diameter is 1 to 10 μm, and the pore spacing is 2 to 400 μm; Preferably, the lithium supplement comprises at least one of a binary lithium-containing compound and a ternary lithium-containing compound, preferably Li6CoO4 and Li5FeO4; Preferably, based on the mass of the positive electrode active material, the content y1wt% of the lithium supplement agent satisfies 0.1wt%≤y1wt%≤2.0wt%, preferably 0.1wt%≤y1wt%≤1.0wt%.
4. The wound lithium-ion battery according to claim 3, characterized in that: The thickness H1 of the positive electrode active material layer, the content y1wt% of the lithium supplement and the particle size Dv50 of the ternary material satisfy the formula Dv50*H1 / 4000≤y1≤Dv50*H1 / 2000+1; H1≤300μm.
5. The wound lithium-ion battery according to any one of claims 1 to 4, characterized in that: The arc region of the positive electrode sheet is provided with a second groove region; Preferably, the width of the second groove area is 5 mm to 20 mm; Preferably, the depth h1 of the second groove region is 1 μm to 45 μm.
6. The wound lithium-ion battery according to claim 5, characterized in that: The depth h1 of the second groove area and the particle size Dv50 of the ternary material satisfy the formula: 20 / Dv50≤h1≤10+350 / Dv50.
7. The wound lithium-ion battery according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: (1) The proportion y2 of the silicon-based material in the negative electrode active material satisfies 5wt%≤y2≤20wt%; the proportion y3 of the carbon material in the negative electrode active material satisfies 80%≤y3≤95%; (2) The silicon-based material includes silicon-carbon material and silicon-oxygen material; Preferably, the proportion y2(1) of the silicon-carbon material in the silicon-based material and the proportion y2(2) of the silicon-oxygen material in the silicon-based material satisfy: 0.4≤y2(1) / y2(2)≤2.
8. The wound lithium-ion battery according to claim 7, characterized in that: The particle size of the carbon material is 8 μm≤Dv50 (1) ≤23μm, particle size of silicon carbon material 4μm≤Dv50 (2) ≤16μm, particle size of silicon oxide material 3μm≤Dv50 (3) ≤10μm; The carbon material Dv50 (1) , Dv50 of silicon carbon material (2) And Dv50 of silicon oxide materials (3) Meets: Dv50 (1) ≤Dv50 (2) +Dv50 (3) ≤2*Dv50 (1) .
9. The wound lithium-ion battery according to any one of claims 1 to 4, characterized in that: At least one of the following conditions is met: (1) The thickness H2 of the negative electrode active material layer and the carbon material Dv50 (1) Satisfy: 0.1*H2≤9*Dv50 (1) +10≤H2; thickness of negative electrode active material layer H2≤300μm; (2) The interval between two adjacent first grooves is 0.5 mm to 2 mm; (3) The depth h2 of the first groove is 0.3 μm to 45 μm.
10. The wound lithium-ion battery according to any one of claims 1 to 4, characterized in that: The electrolyte satisfies at least one of the following conditions: (1) The electrolyte includes additive A, and the additive A includes nitrile and / or ether nitrile additives; Preferably, the content w1 of the additive A in the electrolyte satisfies: 2%≤w1≤13%; Preferably, the additive A is selected from one or more of ethylene glycol di(2-cyanoethyl) ether, ethylene glycol di(4-cyanobutyl) ether, 1,2,3-tri(cyanoethoxy)propane, diethylene glycol di(2-cyanoethyl) ether, tetraethylene glycol di(2-cyanoethyl) ether and ethylene glycol (bis) propionitrile ether; (2) The electrolyte includes additive B, and additive B includes a negative electrode film-forming additive; Preferably, the additive B is selected from one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC) and organosilane compounds; Preferably, the content w2 of the additive B in the electrolyte satisfies: 0.1%≤w2≤5%.
Citation Information
Patent Citations
Positive pole piece, electrochemical device comprising positive pole piece and electronic device
CN114144919A
Battery and electronic equipment
CN115101737A
Positive plate and battery
CN117219726A
Double-layer positive electrode with local lithium supplement function, preparation method of double-layer positive electrode and lithium ion battery