Non-disassembly direct regeneration method for waste lithium iron phosphate battery cell

Through the non-disassembly direct regeneration method, overdischarge is used to repair the negative and positive electrodes of lithium-ion batteries, solving the problem of destructive structural disassembly and insufficient economic value in lithium-ion battery recycling, realizing the performance recovery and cycle stability of the battery cell Improvement, a closed-loop recycling system has been built, with commercial value.

CN119069855APending Publication Date: 2024-12-03SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310622547.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing lithium-ion battery recycling technology has structural destructive disassembly problems, especially the economic value of lithium iron phosphate batteries that do not contain precious metals, and the direct regeneration technology technology requirements are high, making it difficult to apply on a large scale, and overdischarge leads to battery performance. Attenuation and safety hazards.

Method used

Using non-disassembly direct regeneration method, lossless physical repair is carried out through external energy input, solid electrolyte interface layer on the negative electrode surface is decomposed, lithium ion transmission obstacles are reduced, and lithium ions released from overdischarge are used to supplement lithium with positive electrode to achieve overall performance recovery of the battery cell .

Benefits of technology

It realizes direct regeneration of the battery cell without disassembly, improves capacity and cycle stability, and builds a completely closed-loop recycling system, which has high safety, low equipment requirements, and has commercial value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119069855A_ABST
    Figure CN119069855A_ABST
Patent Text Reader

Abstract

A waste lithium iron phosphate cell non-disassembly direct regeneration method comprises the following steps: inputting external energy into a waste cell to carry out nondestructive physical repair regeneration, namely decomposing an inactive lithium-containing compound on a solid electrolyte interface layer on the surface of a negative electrode, reducing the thickness of a lithium ion transport barrier layer on the negative electrode side, and improving the lithium ion transport barrier layer; meanwhile, active lithium ions and electrons provided by decomposition are used for supplementing lithium for the positive electrode, so that the overall performance of the battery cell is recovered. According to the method, a completely closed-loop recovery system is constructed, the treatment process is simple to operate and high in safety, the disassembly problem of large-scale expansion is avoided, additional lithium source input is not needed, and the method is good in compatibility with an existing process technology, low in equipment requirement and very high in commercial value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technology in the field of waste lithium-ion battery recycling, in particular to a method for directly regenerating waste lithium iron phosphate batteries without disassembling them. Background Art

[0002] The economic and infrastructure challenges faced by retired battery processing technology at this stage have jointly restricted the development of the battery recycling industry. At present, lithium-ion battery recycling is mainly focused on disassembling and recovering valuable metals in the positive electrode, such as Li, Co, Ni, etc. This structurally destructive recycling process will destroy a large part of the value of the positive electrode material, especially for lithium iron phosphate (LFP) batteries that do not contain precious metals. The economic value of the elemental products they recover is not enough to compensate for the high cost required by pyrometallurgical and hydrometallurgical processes (ACS Sustainable Chem. Eng., 2018, 6, 1504). Direct regeneration technology has been proposed as an alternative to traditional recycling. Without destroying the original crystal structure, the positive electrode is replenished with lithium and structural defects are repaired, which can directly output high-value positive electrode materials (Energy Storage Mater., 2023, 54, 120), which is more environmentally and economically beneficial. However, this technology has extremely high requirements for the process and is difficult to apply on a large scale. The main difficulty lies in disassembly pretreatment. In the laboratory, high-purity waste positive and negative electrode powders are obtained by manual disassembly and separation, which is the basis for direct regeneration (Waste Manage. Res., 2016, 34, 474), and the practical application of manual disassembly technology still faces considerable challenges. If it is compatible with existing industrial technology and adopts mechanical separation methods for industrial-scale pretreatment, a mixed product consisting of positive and negative electrode materials, conductive agents, PVDF binders and other residual impurities (Al, Cu, etc.) will be obtained, which brings technical obstacles to the development of scalable direct regeneration processes. Therefore, it is very important to seek new, more environmentally friendly and convenient pretreatment methods or to fundamentally avoid complex disassembly pretreatment for the real market application of battery regeneration technology.

[0003] Overdischarge is a common phenomenon in battery packs. When there is an internal resistance mismatch in parallel batteries and the battery management system cannot balance the uneven current distribution caused by this, some cells may be overdischarged (J. Power Sources, 2014, 252, 8). Battery overdischarge will cause the dissolution of the negative copper current collector (Scientific Reports, 2016, 6, 1). After repeated cycles, it will block the electrode intercalation sites, destroy the electrode structure, destroy the SEI film, and promote the formation of copper plating and lithium dendrites, accelerate the decay of capacity, increase the internal resistance, and even cause the battery to short-circuit, which may cause serious safety hazards. Although overdischarge is generally considered a harmful phenomenon that needs to be avoided, studies have shown that a single overdischarge is a benign electrical abuse (J. Electrochem. Soc., 2020, 167, 090558), which provides a feasible basis for the effective use of overdischarge. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a method for direct regeneration of waste lithium iron phosphate batteries without disassembly, which can realize direct regeneration and reuse of batteries in only three steps, thereby building a completely closed-loop recycling system. The processing process is simple to operate and highly safe, avoiding the difficulty of manual disassembly requiring large-scale expansion, and does not require additional lithium source input. It has good compatibility with existing process technologies, has low equipment requirements, and has high commercial value.

[0005] The present invention is achieved through the following technical solutions:

[0006] The present invention relates to a non-disassembly direct regeneration method for waste lithium iron phosphate battery cells, which performs non-destructive physical repair and regeneration of waste battery cells by inputting external energy into the waste battery cells, i.e., decomposing inactive lithium-containing compounds in the solid electrolyte interface layer (SEI) on the surface of the negative electrode, reducing the thickness of the lithium ion transmission barrier layer (i.e., SEI) on the negative electrode side, and simultaneously utilizing the active lithium ions and electrons provided by the decomposition to replenish lithium at the positive electrode, thereby realizing recovery of the overall performance of the battery cells.

[0007] The state of charge (SOC) of the waste battery cell is 20-100%, preferably 40-80%.

[0008] The external energy input refers to: over-discharging the waste battery cell to oxidatively decompose the SEI on the negative electrode side, wherein: the over-discharge cut-off voltage is -0.5-1V, preferably -0.2-0.5V; the over-discharge mode includes constant current discharge, constant voltage discharge, high-frequency resonant current discharge, step current discharge, step voltage discharge or a combination thereof; the over-discharge path includes continuous discharge and intermittent discharge.

[0009] The non-destructive physical repair refers to: re-forming and aging the lithium-ion battery after filling and sealing the battery, so that the over-discharged battery can re-form a stable SEI film to obtain a regenerated battery.

[0010] The injection refers to: injecting an electrolyte solvent or a mixture of an electrolyte solvent and an electrolyte into the lithium iron phosphate battery cell, wherein the electrolyte solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl ether, tetrahydrofuran, methyl acetate, and methyl propionate; the electrolyte includes one or more of LiPF6, LiBF4, LiClO4, LiAsF6, LiN(C2F5SO2)2, LiC(CF3SO2)3, LiN(CF3SO2)2, and LiBOB.

[0011] The formation includes constant current charging, constant voltage charging, step charging, high temperature pressure formation and high voltage shallow cycle or a combination thereof; the formation current density is 0.05-0.5C, the charging cut-off voltage is 3.4-3.65V; the temperature is 5-45°C.

[0012] The aging temperature is 5-45°C and the aging time is 1-14 days. Technical Effects

[0013] The present invention makes rational use of harmful over-discharge behavior and transforms it into an effective battery regeneration method. Without disassembling the battery cell, the electrons released during the over-discharge process and the active lithium ions are used to directly regenerate the positive electrode, thereby achieving the regeneration of the entire battery cell. Different from the previous destructive battery disassembly and recycling technology that only focuses on the recovery of high-cost positive electrode materials, the present invention uses non-destructive physical repair, and the direct output product is a complete battery cell with restored performance, thus constructing a completely closed-loop recycling system. The capacity and cycle stability of the repaired and regenerated battery cell are significantly improved, and can be directly used to assemble battery modules. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is an over-discharge curve diagram of Embodiment 1 of the present invention;

[0015] Figure 2 is the XPS spectrum of the graphite negative electrode surface before and after overdischarge in Example 1 of the present invention;

[0016] Figure 3 This is the cycle performance curve of the regenerated battery cell of Example 1 of the present invention. DETAILED DESCRIPTION Example 1

[0017] This embodiment includes the following steps:

[0018] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=76.57%.

[0019] 2) After normal discharge, the used battery cells are over-discharged at a constant current of 0.1C to -0.1V.

[0020] 3) The over-discharged battery cell is transferred to a glove box, and after cutting a small opening, vacuum evacuates the air and reseals the glove box without injecting electrolyte.

[0021] 4) Use the step-charging formation method to re-form a stable SEI film. The resealed battery cell is formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.5C, and then charged to 3.65V at 0.33C. The formed battery cell is placed in a 45°C constant temperature box for aging for 1 day. Example 2

[0022] This embodiment includes the following steps:

[0023] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=74.19%.

[0024] 2) After normal discharge, the used battery cells are over-discharged at a constant current of 0.1C to -0.1V.

[0025] 3) Transfer the over-discharged cells to the glove box and inject a certain amount of 1.0 mol L -1 The LiPF6 solution is made of EC, DEC and DMC, and the volume of the injected liquid is 10mL. The lithium-ion battery cell after injection is then vacuum packaged.

[0026] 4) Use the step-charging formation method to re-form a stable SEI film. The resealed battery cell is formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.5C, and then charged to 3.65V at 0.33C. The formed battery cell is placed in a 45°C constant temperature box for aging for 1 day.

[0027] Example 3

[0028] This embodiment includes the following steps:

[0029] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=79.47%.

[0030] 2) After normal discharge, the used battery cells are over-discharged at a constant current of 0.1C to 0.5V.

[0031] 3) Transfer the over-discharged cells to the glove box and inject a certain amount of 1.0 mol L -1 The LiPF6 solution is made of EC, DEC and DMC, and the volume of the injected liquid is 10mL. The lithium-ion battery cell after injection is then vacuum packaged.

[0032] 4) The SEI film was reformed using a step-charge formation method. The resealed battery cell was formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.5C, and then charged to 3.65V at 0.33C. The formed battery cell was placed in a 45°C constant temperature box for aging for 1 day. Example 4

[0033] This embodiment includes the following steps:

[0034] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=77.40%.

[0035] 2) After normal discharge, the used battery cells are over-discharged at a constant current of 0.1C to -0.2V.

[0036] 3) Transfer the over-discharged cells to the glove box and inject a certain amount of 1.0 mol L -1 The LiPF6 solution is made of EC, DEC and DMC, and the volume of the injected liquid is 10mL. The lithium-ion battery cell after injection is then vacuum packaged.

[0037] 4) The SEI film was reformed using a step-charge formation method. The resealed battery cell was formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.5C, and then charged to 3.65V at 0.33C. The formed battery cell was placed in a 45°C constant temperature box for aging for 1 day. Example 5

[0038] This embodiment includes the following steps:

[0039] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=63.78%.

[0040] 2) After normal discharge, the used battery cells are over-discharged at a constant current of 0.1C to -0.2V.

[0041] 3) The over-discharged battery cell is transferred to a glove box, and 10 mL of a mixed solvent of EC, DEC and DMC is injected into the battery cell using a small needle syringe. The injected lithium-ion battery cell is then vacuum packaged.

[0042] 4) The SEI film was reformed using a step-charge formation method. The resealed cells were formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.1C, and then charged to 3.65V at 0.25C. The formed cells were placed in a 45°C thermostat for aging for 1 day. Example 6

[0043] This embodiment includes the following steps:

[0044] 1) The recycled waste battery cells were charged to 3.65V at 1C with constant current and constant voltage, and the cut-off current was 0.05C, and then discharged to 2.5V with constant current, SOC=75.33%.

[0045] 2) After normal discharge, the used battery cells are over-discharged to -0.2V at a constant current and constant voltage of 0.1C, and the cut-off current is 0.01C.

[0046] 3) Transfer the over-discharged cells to the glove box and inject a certain amount of 1.0 mol L -1 The LiPF6 solution is made of EC, DEC and DMC, and the volume of the injected liquid is 10mL. The lithium-ion battery cell after injection is then vacuum packaged.

[0047] 4) The SEI film was reformed using a step-charge formation method. The resealed cells were formed at 45°C, first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at a slightly faster current of 0.1C, and then charged to 3.65V at 0.25C. The formed cells were placed in a 45°C thermostat for aging for 1 day. Example 7

[0048] The difference between this embodiment and embodiment 6 is that a constant current intermittent discharge mode is adopted in step 2), and during the over-discharge process, the discharge is performed for 10 minutes and then left to stand for 1 minute. Example 8

[0049] The difference between this embodiment and embodiment 6 is that a constant voltage discharge mode is adopted in step 2) and the cut-off current is 0.01C. Example 9

[0050] The difference between this embodiment and embodiment 6 is that in step 4), a 45°C high voltage shallow cycle formation is used, the sealed battery cell is first charged to 3.4V at a constant current of 0.05C, and then charged and discharged for ten times at a voltage range of [3.4, 3.65]V at 0.5C. The formed battery cell is aged in a 5°C constant temperature box for 7 days. Example 10

[0051] The difference between this embodiment and embodiment 6 is that in step 4), a low temperature of 5°C is used for formation, and the battery is first charged to 3.4V at a low current of 0.05C, then charged to 3.6V at 0.1C, and then charged to 3.65V at 0.25C. The formed battery cell is placed in a 45°C constant temperature box for aging for 14 days. Comparative Example

[0052] The battery was charged to 3.65V at 1C with a cut-off current of 0.05C, and then discharged to 2.5V with a SOC of 73.24%. Without any regeneration and repair treatment, it can be used for comparison with the previous ten embodiments, effectively demonstrating the regeneration effect achieved by the unique over-discharge cell repair technology proposed by the present invention.

[0053] Electrochemical performance: In the above embodiment, the regenerated battery cell was subjected to 80 cycles of 1C charge and discharge in the voltage range of 2.5-3.65V. The capacity improvement effect of the first cycle and the cycle stability of the regenerated battery cell are shown in Table 1.

[0054] Table 1 Electrochemical performance test of regenerated battery cells

[0055] Compared with the prior art, this method adopts an over-discharge regeneration and repair process, which has certain effects on the recovery of battery cell capacity and the extension of cycle life. The present invention can achieve effective regeneration of waste lithium battery cells in different states, especially has a significant improvement effect on the cycle stability of waste batteries. The capacity of the battery cells after over-discharge repair can be restored to SOC=80%, and the improvement effect of the battery cells with serious capacity decay is more obvious. After 80 cycles, the capacity of the waste battery cells decays rapidly, and the capacity retention rate of the regenerated battery cells can be increased by more than 24% compared with it, and the cycle stability is comparable to that of fresh batteries. This shows that the non-disassembly direct regeneration method of the present invention can significantly extend the service life of the battery cells. After regeneration, the capacity of the battery cells is partially restored, and the consistency and cycle stability are improved, so they can be reused.

[0056] The above-mentioned specific implementation can be partially adjusted in different ways by those skilled in the art without departing from the principle and purpose of the present invention. The protection scope of the present invention shall be based on the claims and shall not be limited by the above-mentioned specific implementation. Each implementation scheme within its scope shall be subject to the constraints of the present invention.

Claims

1. A method for direct regeneration of waste lithium iron phosphate batteries without disassembly. It is characterized in that The waste battery cells are regenerated by non-destructive physical repair through external energy input, that is, the inactive lithium-containing compounds in the solid electrolyte interface layer on the negative electrode surface are decomposed to reduce the thickness of the lithium ion transmission barrier layer on the negative electrode side, and the active lithium ions and electrons provided by the decomposition are used to replenish lithium at the positive electrode, thereby realizing the recovery of the overall performance of the battery cells; The non-destructive physical repair means: over-discharging the waste battery cells, and then filling the discharged lithium iron phosphate battery cells with liquid, sealing them, and then re-forming and aging them, so that the over-discharged battery cells can re-form a stable SEI film to obtain regenerated battery cells.

2. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The state of charge SOC of the waste battery cell is 20-100%.

3. The non-disassembly direct regeneration method of waste lithium iron phosphate batteries according to claim 1, Its characteristics are: The external energy input refers to: over-discharging the waste battery cells to oxidatively decompose the SEI on the negative electrode side, wherein: the cut-off voltage of over-discharging is -0.5-1V.

4. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The over-discharge modes include constant current discharge, constant voltage discharge, high frequency resonant current discharge, step current discharge, step voltage discharge or a combination thereof; the over-discharge paths include continuous discharge and intermittent discharge.

5. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The injection means: injecting an electrolyte solvent or a mixture of an electrolyte solvent and an electrolyte into the lithium iron phosphate battery cell, wherein the electrolyte solvent includes ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dimethyl ether, tetrahydrofuran, methyl acetate, methyl propionate or a combination thereof; the electrolyte includes LiPF 6 , LiBF 4 、LiClO 4 、LiAsF 6 、LiN(C 2 F 5 SO 2 ) 2 、LiC(CF 3 SO 2 ) 3 、LiN(CF 3 SO 2 ) 2 , LiBOB or a combination thereof.

6. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The formation includes constant current charging, constant voltage charging, step charging, high temperature pressure formation and high voltage shallow cycle or a combination thereof.

7. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The formation current density is 0.05-0.5C, the charging cut-off voltage is 3.4-3.65V, and the temperature is 5-45°C.

8. The method for direct regeneration of waste lithium iron phosphate batteries without disassembly according to claim 1, Its characteristics are: The aging temperature is 5-45°C and the aging time is 1-14 days.