Multilayer piezoelectric actuator, preparation method and application

Through two-step solid-phase reaction method and low-temperature sintering technology, high-performance multi-layer piezoelectric drivers are prepared, which solves the problem of limited application of single crystal drivers in miniaturization and low-drive environments in the prior art, and achieves high output strain and Sensitivity and reduce production costs.

CN119072212APending Publication Date: 2024-12-03XI AN JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411202595.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The performance of existing piezoelectric drivers cannot meet the high precision and high sensitivity requirements in ultra-precision micro-nano processing technology, robotics technology, microsatellite/micro-aircraft, especially the application of single crystal drivers in miniaturized and low-drive environments. limit.

Method used

The xPYN-yPMN-(1-x-y)PT fine crystal ceramic powder was synthesized by a two-step solid-phase reaction method, and the orientation treatment was performed through the seed crystal template of sheet-like perovskite structure, and the multi-layer piezoelectric driver was prepared in combination with low-temperature sintering technology. , realize high-performance texture of ceramic materials and high output strain at low driving voltage.

Benefits of technology

It achieves output strain and sensitivity far higher than that of commercial PZT ceramic drivers, avoiding the problems of high driving voltage and uneven performance of single crystal drivers, and has good complex environment tolerance and low production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072212A_ABST
    Figure CN119072212A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps that xPYN-yPMN-(1-x-y) PT fine-grain ceramic powder is synthesized through a two-step solid-phase reaction method, x is larger than or equal to 0.1 and smaller than or equal to 0.4, and y is larger than or equal to 0.2 and smaller than or equal to 0.55; synthesizing a flaky perovskite structure seed crystal template with [001] orientation; the flaky perovskite structure seed crystal template is added into the xPYN-yPMN-(1-x-y) PT fine grain ceramic powder, slurry is prepared, and tape casting is carried out; printing an inner electrode, laminating and cutting a film belt of the printed inner electrode, discharging glue from a glue-containing blank obtained by cutting, and sintering the blank obtained by glue discharging at high temperature to obtain a multi-layer ceramic block; the multi-layer ceramic block obtained through high-temperature sintering is polished and stacked, a driver is prepared, and an outer electrode is prepared on the obtained driver; the driver with the outer electrode is polarized to obtain a multi-layer piezoelectric driver; according to the preparation method of the driver, low-temperature sintering can be carried out, the multilayer texture ceramic driver with low driving voltage and high sensitivity can be prepared, production equipment and the technological process are simple, and the preparation method is suitable for industrial large-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of piezoelectric devices and technologies, and in particular relates to a multilayer piezoelectric driver, a preparation method and an application thereof. Background Art

[0002] Piezoelectric material is a special functional material that can realize the conversion of electrical energy and mechanical deformation. The piezoelectric drive developed by using the inverse piezoelectric effect of piezoelectric materials with piezoelectric materials as the core part is an important piezoelectric device, which is widely used in various micro-nano displacement control systems and precision drive devices. Phase change Traditional electromagnetic drive, piezoelectric drive has the advantages of fast response speed, high displacement accuracy, large travel range, simple drive system, etc. At the same time, the multilayer piezoelectric drive developed by mechanical series connection and circuit parallel connection of piezoelectric materials has greatly reduced the driving voltage and improved the displacement sensitivity. At present, most of the commercial piezoelectric drives on the market use lead zirconate titanate (PZT)-based ceramic materials as piezoelectric functional layers, and their maximum output strain is about 1‰. Limited by the intrinsic piezoelectric properties of PZT ceramics, the performance of commercial piezoelectric drives has long been difficult to break through the bottleneck. The rapid development of ultra-precision micro-nano processing technology, robotics technology, micro-satellite / micro-aircraft precision operation and precision servo control technology has put forward higher requirements on the accuracy and sensitivity of existing drives. The performance of existing commercial PZT ceramic drives cannot meet the requirements of the above new technology fields for high-performance drive performance. Therefore, developing a new generation of high-performance piezoelectric actuators has become a difficult problem that needs to be solved urgently in the field of piezoelectric device research.

[0003] The key to improving the performance of piezoelectric actuators is to improve the piezoelectric properties of the piezoelectric materials used to make the functional layers. As we all know, relaxor ferroelectric single crystal materials, due to the anisotropy of the crystal, have much higher piezoelectric properties than PZT ceramics. Taking lead magnesium niobate-lead titanate (PMN-PT) single crystal as an example, its piezoelectric coefficient can reach more than 2000pm / V, which is 3-5 times that of PZT ceramics. Therefore, the output strain of single crystal piezoelectric multilayer actuators developed by replacing PZT ceramics with relaxor ferroelectric single crystals is greatly improved. There are related patents that have been studied in this regard. However, the current single crystal growth technology cannot achieve single crystal growth and co-firing of multilayer actuators. Multilayer actuators must be made by pre-thinning single crystals and then stacking them to form single crystal multilayer actuators. The poor mechanical properties of single crystals make it very easy for single crystals to crack during the thinning process, and the thickness of the wafer cannot be thinned to less than 200μm (the thickness of a single layer of ceramic actuators is about 50-100μm), which leads to the need for high operating voltages for single crystal actuators. At the same time, the single crystal will experience component segregation during its growth, causing uneven composition and performance of the wafer, resulting in poor performance consistency of the single crystal driver. These shortcomings of single crystal drivers limit their application in areas such as miniaturization, array applications, and low-drive environments. To this end, the development of high-performance piezoelectric drivers that can achieve low drive, high output sensitivity, and a large travel range can provide important basic technical support for promoting technological progress in many technical fields. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a multilayer piezoelectric driver and a preparation method thereof, which achieves a breakthrough in the performance of high-performance piezoelectric drivers and promotes the development of precision displacement and control technology.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: a method for preparing a multilayer piezoelectric actuator, comprising the following steps:

[0006] Synthesis of xPYN-yPMN-(1-xy)PT fine-grained ceramic powders by two-step solid phase reaction method, 0.1≤x≤0.4, 0.2≤y≤0.55;

[0007] Synthesizing a

[001] -oriented perovskite seed template;

[0008] Adding the sheet-like perovskite structure seed crystal template to the xPYN-yPMN-(1-xy)PT fine-grained ceramic powder, preparing a slurry and performing tape casting;

[0009] Printing inner electrodes, laminating and cutting the film strips of the printed inner electrodes, debinding the cut glue-containing embryonic body, and sintering the debinding embryonic body at high temperature to obtain a multilayer ceramic block;

[0010] The multilayer ceramic block obtained by high-temperature sintering is polished and stacked to prepare a driver, and an external electrode is prepared on the obtained driver;

[0011] The actuator with external electrodes is polarized to obtain a multilayer piezoelectric actuator.

[0012] Furthermore, when xPYN-yPMN-(1-xy)PT fine-grained ceramic powder is synthesized by a two-step solid phase reaction method, the calcination temperature is 700-800°C and the holding time is 1-4h.

[0013] Furthermore, in the two-step solid-phase reaction method for synthesizing xPYN-yPMN-(1-xy)PT fine-grained ceramic powder, the additives used during calcination are one or a combination of CuO, PbO, B2O3, ZnO, and Li2CO3, and the amount of additive added is 0.1%-2% of the mass fraction of the ceramic powder.

[0014] Furthermore, the flake perovskite structure seed crystal template is synthesized by topological chemistry or hydrothermal method, and its chemical composition is one of BaTiO3, (Ba, Sr) TiO3, (Ba, Ca) TiO3 or Ba(Ti, Zr) O3; the thickness is 0.5-1.0 μm, the radial size is 5-15 μm, the diameter-to-thickness ratio is greater than 8, and the template addition amount accounts for 0.5%-10% of the volume fraction of the fine-grained ceramic powder.

[0015] Furthermore, when printing the inner electrode, the inner electrode material used is a silver-palladium electrode, and the outer electrode material is one of silver or copper, wherein the palladium content in the silver-palladium electrode does not exceed 10wt.%.

[0016] Furthermore, the high temperature sintering temperature is 900-1000°C, and the holding time is 6-10h.

[0017] In a second aspect, the present invention provides a multilayer piezoelectric actuator, which is obtained by the preparation method of the multilayer piezoelectric actuator, wherein xPb(Yb 1 / 2 Nb 1 / 2 )O3-yPb(Mg 1 / 3 Nb 2 / 3 The grains of the )O3-(1-xy)PbTiO3 textured ceramic material are preferentially oriented along the

[001] direction, and the orientation degree of the grains of the textured ceramic material along the

[001] direction is greater than 95%.

[0018] Furthermore, the thickness of a single ceramic layer is 20 to 50 μm.

[0019] Furthermore, the driving voltage range is -20 to 100 V, the operating temperature is -50°C to 200°C, and the maximum output strain is 0.3%.

[0020] In a third aspect, the present invention provides an application of the above-mentioned multilayer piezoelectric actuator for use in a workbench stepper, a servo mechanism, a lens assembly or a micro-motion robot.

[0021] Compared with the prior art, the present invention has at least the following beneficial effects: the multilayer piezoelectric actuator described in the present invention constructs a multilayer textured ceramic piezoelectric actuator through grain orientation engineering technology, which has an output strain and sensitivity far higher than the current mainstream commercial PZT ceramic piezoelectric actuator, and avoids the shortcomings of single crystal stacked piezoelectric actuators such as high driving voltage and poor performance consistency, and can achieve high-sensitivity displacement output under low driving voltage conditions; the multilayer piezoelectric actuator described in the present invention has good tolerance to complex environments, and can maintain stable performance in a temperature range of -50°C to 200°C and a strong field environment of 0 to 10 kV / cm.

[0022] The manufacturing method of a multilayer piezoelectric actuator described in the present invention combines ceramic material design with low-temperature liquid phase sintering technology to achieve the preparation of high-performance textured ceramic actuators under low-temperature sintering conditions, thereby reducing production energy consumption, effectively inhibiting the volatilization of elements such as lead that are harmful to the human body and the environment during the sintering process, and avoiding the use of expensive metal internal electrode materials; at the same time, the low-temperature sintering process can effectively reduce the leakage of the internal electrode during the sintering process and improve the yield rate of the product; the production cost of the actuator is greatly reduced. The driver preparation method shown in the present invention is based on ceramic solid phase sintering technology, and the production equipment and process are simple, which is suitable for industrial-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a process flow chart for manufacturing a multilayer piezoelectric actuator provided in an embodiment of the patent of the present invention.

[0024] Figure 2 This is a cross-sectional microscopic morphology image of the piezoelectric actuator described in Example 1.

[0025] Figure 3 This is the X-ray diffraction spectrum of the piezoelectric layer of the piezoelectric actuator described in Example 2.

[0026] Figure 4 It is the dielectric temperature spectrum of the piezoelectric actuator described in Example 3.

[0027] Figure 5 This is the driving voltage-output strain relationship curve of the piezoelectric driver described in Example 4. DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments and accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0029] On the one hand, the technical solution provided by the present invention is a method for preparing a multilayer piezoelectric actuator, comprising the following steps:

[0030] Synthesis of xPYN-yPMN-(1-xy)PT fine-grained ceramic powders by two-step solid phase reaction method, 0.1≤x≤0.4, 0.2≤y≤0.55;

[0031] Synthesizing a

[001] -oriented perovskite seed template;

[0032] Adding the sheet-like perovskite structure seed crystal template to the xPYN-yPMN-(1-xy)PT fine-grained ceramic powder, preparing a slurry and performing tape casting;

[0033] Printing inner electrodes, laminating and cutting the film strips of the printed inner electrodes, debinding the cut glue-containing embryonic body, and sintering the debinding embryonic body at high temperature to obtain a multilayer ceramic block;

[0034] The multilayer ceramic block obtained by high-temperature sintering is polished and stacked to prepare a driver, and an external electrode is prepared on the obtained driver;

[0035] The actuator with external electrodes is polarized to obtain a multilayer piezoelectric actuator.

[0036] The calcination temperature of xPYN-yPMN-(1-xy)PT fine-grained ceramic powder synthesized by the two-step solid phase reaction method can be further optimized to 700-800°C and the holding time to 1-4h.

[0037] When xPYN-yPMN-(1-xy)PT fine-grained ceramic powder is synthesized by a two-step solid phase reaction method, the additives used during calcination are one or a combination of CuO, PbO, B2O3, ZnO, and Li2CO3, and the amount of additive added is 0.1%-2% of the mass fraction of the ceramic powder.

[0038] Preferably, the flake perovskite structure seed crystal template is synthesized by topological chemistry or hydrothermal method, and the chemical composition of the flake perovskite structure seed crystal template is one of BaTiO3, (Ba, Sr) TiO3, (Ba, Ca) TiO3 or Ba(Ti, Zr) O3; the average thickness is 0.5-1.0 μm, the average radial size is 5-15 μm, the diameter-to-thickness ratio is greater than 8, and the template addition amount accounts for 0.5%-10% of the volume fraction of the fine-grained ceramic powder.

[0039] When printing the inner electrode, the inner electrode material used is a silver-palladium electrode, and the outer electrode material is one of silver or copper, wherein the palladium content in the silver-palladium electrode does not exceed 10wt.%.

[0040] In the above scheme, the high temperature sintering temperature is 900-1000°C and the insulation time is 6-10h.

[0041] Based on the above scheme, the polarization voltage is 100-200V and the polarization time is 10-20min.

[0042] Comply with the above technical solution, the specific implementation is as follows:

[0043] Example 1

[0044] The multilayer piezoelectric actuator described in this embodiment 1 is manufactured according to the following steps, and its process flow is as follows: Figure 1 As shown:

[0045] S1, select high-purity nano-grade PbO, TiO2, Yb2O3, MgO, Nb2O5 as reaction raw materials, mix them according to the stoichiometric ratio of 0.2PYN-0.48PMN-0.32PT, ball-mill and mix them, and then calcine at 800℃ for 1h to synthesize PYN-PMN-PT fine-crystalline powder.

[0046] S2, using a topological chemical method to synthesize BaTiO3 thin-plate micron crystals with a

[001] orientation as a seed crystal template, the seed crystal template has a thickness of 1.0 μm and an average radial size of 10.0 μm. The average radial size described in the present invention expresses the diameter of the seed crystal template.

[0047] S3, first mix the PYN-PMN-PT fine-crystalline powder synthesized by S1 with 0.5% by mass of nano-ZnO additive, and add solvent and dispersant, and ball mill for 10 hours; secondly, add adhesive and plasticizer, and ball mill again for 10 hours; then, add flaky seed crystals synthesized by S2 at a volume fraction of 5% of the fine-crystalline powder, and ball mill for 20 minutes; finally, vacuum defoam the mixed slurry, adjust the height of the casting scraper to 300μm, cast, and obtain the cast film tape containing the seed crystal template after drying.

[0048] S4, cutting the dried cast film strip, and printing the inner electrode by screen printing technology, wherein the inner electrode slurry adopts silver-palladium electronic slurry.

[0049] S5, the cast film strip with printed inner electrode is laminated at 70°C by a laminating machine to form a block containing glue, and then isostatically pressed in warm water at 80°C and 20Mpa for 30 minutes. Finally, it is cut according to the designed shape to obtain a glue-containing embryo.

[0050] S6, heating the colloid-containing embryo obtained by cutting in S5 to 600°C at a heating rate of 0.4°C / min, keeping the temperature for 6 hours, and then cooling it to room temperature at a cooling rate of 2.0°C / min to obtain a colloid-free embryo.

[0051] S7, the debinding green body is subjected to cold isostatic pressing at a pressure of 200 MPa and a holding time of 3 min; then, it is placed in a high temperature furnace and sintered at 1000° C. for 6 h to obtain a PYN-PMN-PT multilayer textured ceramic sample.

[0052] The multilayer ceramic blocks obtained by sintering S8 and S7 were ground and polished, and then stacked longitudinally using epoxy resin to make driver samples with different thicknesses.

[0053] S9, grinding and polishing the side of the sample stacked in S8, exposing the inner electrode of the interdigitated part, screen-printing the outer electrode slurry, and sintering at high temperature to form the outer electrode.

[0054] The stacked samples obtained in S10 and S9 are polarized in silicone oil at room temperature with a polarization voltage of 200 V and a polarization time of 10 min, and finally the multilayer piezoelectric actuator described in the present invention is obtained.

[0055] Figure 2 This is a microscopic morphology of the planed surface of a low-drive, high-sensitivity textured ceramic multilayer actuator described in this embodiment. The ceramic layer thickness is uniform, and the thickness of a single ceramic layer is about 50μm. The ceramic layer and the electrode layer are precisely combined without delamination or cracking.

[0056] Embodiment 2:

[0057] The multilayer piezoelectric actuator described in this embodiment 2 is completed according to the following steps:

[0058] S1, select high-purity nano-grade PbO, TiO2, Yb2O3, MgO, Nb2O5 as reaction raw materials, mix them according to the stoichiometric ratio of 0.3PYN-0.4PMN-0.3PT, ball-mill and mix them, and calcine them at 750℃ for 3h to synthesize PYN-PMN-PT fine-crystalline powder.

[0059] S2, Ba(Ti,Zr)O3 thin-plate micron crystals with (001) orientation were synthesized by hydrothermal method as seed crystal templates, the average thickness of the seed crystal template was 1.0 μm, and the average radial size was 15.0 μm.

[0060] S3, firstly, the PYN-PMN-PT fine-crystalline powder synthesized by S1 was mixed with 0.1% by mass of nano-LiCO3 additive, and solvent and dispersant were added, and ball-milled for 20 hours; secondly, adhesive and plasticizer were added, and ball-milled again for 20 minutes; then, flaky seed crystals synthesized by S2 were added at a volume fraction of 10% of the fine-crystalline powder, and ball-milled for 30 minutes; finally, the mixed slurry was vacuum-defoamed, the height of the casting scraper was adjusted to 200 μm, and the casting was carried out, and after drying, a casting film tape containing a seed crystal template was obtained.

[0061] S4, cutting the dried cast film strip, and printing the inner electrode by screen printing technology, wherein the inner electrode slurry adopts silver-palladium electronic slurry.

[0062] S5, the cast film strip with printed inner electrode is laminated at 70°C by a laminating machine to form a block containing glue, and then isostatically pressed in warm water at 70°C and 40Mpa for 20 minutes. Finally, it is cut according to the designed shape to obtain a glue-containing embryo.

[0063] S6, heating the colloid-containing embryo obtained by cutting in S5 to 600°C at a heating rate of 0.3°C / min, keeping the temperature for 2h, and then cooling it to room temperature at a cooling rate of 2.0°C / min to obtain a colloid-free embryo.

[0064] S7, the debinding green body is subjected to cold isostatic pressing at a pressure of 200 MPa and a holding time of 3 min; and then placed in a high temperature furnace and sintered at 950° C. for 9 h to obtain a PYN-PMN-PT multilayer textured ceramic sample.

[0065] The multilayer ceramic blocks obtained by sintering S8 and S7 were ground and polished, and then stacked longitudinally using epoxy resin to make driver samples with different thicknesses.

[0066] S9, grinding and polishing the side of the sample stacked in S8, exposing the inner electrode of the interdigitated part, screen-printing the outer electrode slurry, and sintering at high temperature to form the outer electrode.

[0067] The stacked samples obtained in S10 and S9 are polarized in silicone oil at room temperature with a polarization voltage of 100 V and a polarization time of 10 min, and finally the multilayer piezoelectric actuator described in the present invention is obtained, wherein the thickness of a single ceramic layer is about 35 μm.

[0068] Figure 3 The surface X-ray diffraction spectrum of the PYN-PMN-PT multilayer textured ceramic sample obtained by sintering in step S7 of this embodiment is given. It can be seen from the figure that it exhibits a high degree of (001) crystal plane preferential orientation, and its

[001] orientation degree is calculated to be greater than 98%.

[0069] Example 3

[0070] The multilayer piezoelectric actuator described in this embodiment is manufactured according to the following steps, and its process flow is as follows: Figure 1 As shown:

[0071] S1, select high-purity nano-grade PbO, TiO2, Yb2O3, MgO, Nb2O5 as reaction raw materials, mix them according to the stoichiometric ratio of 0.4PYN-0.2PMN-0.4PT, ball-mill and mix them, and then calcine at 700℃ for 4h to synthesize PYN-PMN-PT fine-crystalline powder.

[0072] S2, using topological chemistry to synthesize (BaSr)TiO3 thin-plate micron crystals with

[001] orientation as seed templates, the seed templates have an average thickness of 0.5 μm and an average radial size of 5.0 μm;

[0073] S3, firstly, the PYN-PMN-PT fine-crystalline powder synthesized by S1 is mixed with 0.2% by mass of nano-CuO additive, and a solvent and a dispersant are added, and the mixture is ball-milled for 30 hours; secondly, a binder and a plasticizer are added, and the mixture is ball-milled for 15 hours; then, 0.5% by volume of the fine-crystalline powder is added with the flaky seed crystals synthesized by S2, and the mixture is ball-milled for 30 minutes; finally, the mixed slurry is vacuum-defoamed, the height of the casting scraper is adjusted to 150 μm, and the casting is performed, and after drying, a casting film tape containing a seed crystal template is obtained.

[0074] S4, cutting the dried cast film strip, and printing the inner electrode by screen printing technology, wherein the inner electrode slurry adopts silver-palladium electronic slurry.

[0075] S5, the cast film strip with printed inner electrode is laminated at 70°C by a laminating machine to form a block containing glue, and then isostatically pressed in warm water at 80°C and 25Mpa for 20 minutes. Finally, it is cut according to the designed shape to obtain a glue-containing embryo.

[0076] S6, heating the colloid-containing embryo obtained by cutting in S5 to 600°C at a heating rate of 0.3°C / min, keeping the temperature for 6 hours, and then cooling it to room temperature at a cooling rate of 1.0°C / min to obtain a colloid-free embryo.

[0077] S7, the debinding green body is subjected to cold isostatic pressing at a pressure of 200 MPa and a holding time of 3 min; then, it is placed in a high-temperature furnace and sintered at 900° C. for 10 h to obtain a PYN-PMN-PT multilayer textured ceramic sample.

[0078] The multilayer ceramic blocks obtained by sintering S8 and S7 were ground and polished, and then stacked longitudinally using insulating glass slurry to produce driver samples with different thicknesses.

[0079] S9, grinding and polishing the side of the sample stacked in S8, exposing the inner electrode of the interdigitated part, screen-printing the outer electrode slurry, and sintering at high temperature to form the outer electrode.

[0080] The stacked samples obtained in S10 and S9 are polarized in silicone oil at room temperature with a polarization voltage of 100 V and a polarization time of 20 min, and finally the multilayer piezoelectric actuator described in the present invention is obtained, wherein the single-layer piezoelectric ceramic layer is 20 μm thick.

[0081] Figure 4This is the dielectric temperature spectrum of the multilayer piezoelectric ceramic described in Example 3. It can be seen from the figure that the Curie temperature of the piezoelectric driver is about 245°C, and the dielectric constant remains stable below 200°C. Furthermore, when the temperature of the material is reduced to -50°C, its dielectric constant does not change significantly compared with room temperature. The dielectric constant is linearly related to the piezoelectric properties of the material. This conclusion shows that the driver can output stably within the range of -50-200°C.

[0082] Example 4

[0083] The multilayer piezoelectric actuator described in this embodiment 1 is manufactured according to the following steps, and its process flow is as follows: Figure 1 As shown:

[0084] S1, select high-purity nano-grade PbO, TiO2, Yb2O3, MgO, and Nb2O5 as reaction raw materials, mix them according to the stoichiometric ratio of 0.15PYN-0.53PMN-0.32PT, ball-mill and mix them, and then calcine at 780°C for 2h to synthesize PYN-PMN-PT fine-crystalline powder.

[0085] S2, using topological chemistry to synthesize (BaCa)TiO3 thin-plate micron crystals with

[001] orientation as seed templates, the seed templates have an average thickness of 0.8 μm and an average radial size of 12.0 μm;

[0086] S3, first mix the PYN-PMN-PT fine-crystalline powder synthesized by S1 with 2% by mass of nano-PbO-B2O3 composite additive, add solvent and dispersant, and ball-mill for 20 hours; secondly, add adhesive and plasticizer, and ball-mill for 10 hours; then, add flaky seed crystals synthesized by S2 at a volume fraction of 3% of the fine-crystalline powder, and ball-mill for 20 minutes; finally, vacuum defoam the mixed slurry, adjust the height of the casting scraper to 250μm, cast, and obtain a cast film tape containing the seed crystal template after drying.

[0087] S4, cutting the dried cast film strip, and printing the inner electrode by screen printing technology, wherein the inner electrode slurry adopts silver-palladium electronic slurry.

[0088] S5, the cast film strip with printed inner electrode is laminated at 70°C by a laminating machine to form a block containing glue, and then isostatically pressed in warm water at 80°C and 20Mpa for 30 minutes. Finally, it is cut according to the designed shape to obtain a glue-containing embryo.

[0089] S6, heating the colloid-containing embryo obtained by cutting in S5 to 600°C at a heating rate of 0.15°C / min, keeping the temperature for 3 hours, and then cooling it to room temperature at a cooling rate of 0.5°C / min to obtain a colloid-free embryo.

[0090] S7, the debinding green body is subjected to cold isostatic pressing at a pressure of 150 MPa and a holding time of 3 min; and then placed in a high temperature furnace and sintered at 980° C. for 9 h to obtain a PYN-PMN-PT multilayer textured ceramic sample.

[0091] The multilayer ceramic blocks obtained by sintering S8 and S7 were ground and polished, and then stacked longitudinally using inorganic glass slurry to make driver samples of different thicknesses.

[0092] S9, grinding and polishing the side of the sample stacked in S8, exposing the inner electrode of the interdigitated part, screen-printing the outer electrode slurry, and sintering at high temperature to form the outer electrode.

[0093] The stacked samples obtained in S10 and S9 are polarized in silicone oil at room temperature with a polarization voltage of 150 V and a polarization time of 15 min, and finally the multilayer piezoelectric actuator described in the present invention is obtained, wherein the thickness of a single-layer piezoelectric ceramic layer is 40 μm.

[0094] Figure 5 The relationship curve between the driving voltage and the output strain of the multilayer piezoelectric driver described in this embodiment 4. Under a driving voltage of 100V, the maximum strain of the driver can reach 0.3% and maintain good linearity. Its performance is much higher than the 0.1% performance of the current commercial piezoelectric driver, achieving a leap in the performance of the piezoelectric multilayer piezoelectric ceramic driver.

[0095] On the other hand, the present invention provides a multilayer piezoelectric actuator, which is obtained by the preparation method of the multilayer piezoelectric actuator, wherein xPb(Yb 1 / 2 Nb 1 / 2 )O3-yPb(Mg 1 / 3 Nb 2 / 3 )O3-(1-xy)PbTiO3 textured ceramic material grains are preferentially oriented along the

[001] direction, the orientation degree of the textured ceramic material grains along the

[001] direction is greater than 95%, and the thickness of the single ceramic layer is 20 to 50 μm; the driving voltage range is -20 to 100 V, the operating temperature is -50°C to 200°C, and the maximum output strain is 0.3%.

[0096] At the same time, according to the actual scenario, the multilayer piezoelectric driver can be applied to workbench steppers, servo mechanisms, lens assemblies or micro-motion robots.

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a multilayer piezoelectric actuator, It is characterized in that The following steps are involved: Synthesis of xPYN-yPMN-(1-xy)PT fine-grained ceramic powders by two-step solid phase reaction method, 0.1≤x≤0.4, 0.2≤y≤0.55; Synthesizing a [001]-oriented perovskite seed template; Adding the sheet-like perovskite structure seed crystal template to the xPYN-yPMN-(1-xy)PT fine-grained ceramic powder, preparing a slurry and performing tape casting; Printing inner electrodes, laminating and cutting the film strips of the printed inner electrodes, debinding the cut glue-containing embryonic body, and sintering the debinding embryonic body at high temperature to obtain a multilayer ceramic block; The multilayer ceramic block obtained by high-temperature sintering is polished and stacked to prepare a driver, and an external electrode is prepared on the obtained driver; The actuator with external electrodes is polarized to obtain a multilayer piezoelectric actuator.

2. The method for preparing the multilayer piezoelectric actuator according to claim 1, It is characterized in that The calcination temperature of xPYN-yPMN-(1-xy)PT fine-grained ceramic powder synthesized by the two-step solid phase reaction method is 700-800°C and the holding time is 1-4h.

3. The method for preparing the multilayer piezoelectric actuator according to claim 1, It is characterized in that In the two-step solid phase reaction method for synthesizing xPYN-yPMN-(1-xy)PT fine-grained ceramic powder, the additives used during calcination are CuO, PbO, B 2 O 3 、ZnO、Li 2 CO 3 One or a combination of the above, the additive addition amount is 0.1%-2% of the mass fraction of the ceramic powder.

4. The method for preparing the multilayer piezoelectric actuator according to claim 1, It is characterized in that The sheet-like perovskite structure seed crystal template is synthesized by topological chemistry or hydrothermal method, and its chemical composition is BaTiO 3 、(Ba,Sr)TiO 3 、(Ba,Ca)TiO 3 Or Ba(Ti,Zr)O 3 One of the above; the average thickness is 0.5-1.0 μm, the average radial size is 5-15 μm, the diameter-to-thickness ratio is greater than 8, and the template addition amount accounts for 0.5%-10% of the volume fraction of the fine-grained ceramic powder.

5. The method for preparing the multilayer piezoelectric actuator according to claim 1, It is characterized in that When printing the inner electrode, the inner electrode material used is a silver-palladium electrode, and the outer electrode material is one of silver or copper, wherein the palladium content in the silver-palladium electrode does not exceed 10wt.%.

6. The method for preparing the multilayer piezoelectric actuator according to claim 1, It is characterized in that The high temperature sintering temperature is 900-1000℃ and the holding time is 6-10h.

7. A multilayer piezoelectric actuator, It is characterized in that The method for preparing the multilayer piezoelectric actuator according to any one of claims 1 to 6 is used, wherein xPb(Yb 1 / 2 Nb 1 / 2 ) 3 -yPb(Mg 1 / 3 Nb 2 / 3 ) 3 -(1-xy)PbTiO 3 The grains of the textured ceramic material are preferentially oriented along the [001] direction, and the orientation degree of the grains of the textured ceramic material along the [001] direction is greater than 95%.

8. The multilayer piezoelectric actuator according to claim 7, It is characterized in that The thickness of a single ceramic layer is 20 to 50 μm.

9. The multilayer piezoelectric actuator according to claim 7, It is characterized in that The driving voltage range is -20 to 100 V, the operating temperature is -50°C to 200°C, and the maximum output strain is 0.3%.

10. Application of a multilayer piezoelectric actuator, It is characterized in that For use with stage steppers, servos, lens assemblies or micro-motion robots.