Semiconductor device and MRAM

By using alloy layers composed of multiple metals in MRAM to form the second pinned layer, the problem of performance degradation after high-temperature annealing is solved, and the thermal stability and reliability of the device are improved.

CN119072214APending Publication Date: 2024-12-03ZHEJIANG HIKSTOR TECHOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310642392.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

After high-temperature annealing of existing MRAM, the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength performance will seriously degrade, resulting in poor device reliability.

Method used

A semiconductor device is designed, which includes a seed layer, a first pinning layer and a second pinning layer, the second pinning layer consisting of an alloy layer and an isolation layer composed of a variety of metals, and the metal layer includes a transition metal and an alkaline earth metal. Ensure good thermal stability is maintained after high temperature annealing.

Benefits of technology

The vertical magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device after high temperature annealing are improved, performance degradation caused by the single metal is avoided, and data retention capabilities and reliability are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072214A_ABST
    Figure CN119072214A_ABST
Patent Text Reader

Abstract

The invention provides a semiconductor device and an MRAM. The semiconductor device comprises a seed layer, a first pinning layer and a second pinning layer, and the first pinning layer is located on the surface of the seed layer; the second pinning layer is located on the side, away from the seed layer, of the first pinning layer, the second pinning layer comprises a metal layer and an isolation layer which are stacked, the metal layer is located on the surface, close to the first pinning layer, of the isolation layer, and the metal layer comprises alloy composed of multiple kinds of metal. The second pinning layer comprises the metal layer, and the metal layer is an alloy composed of a plurality of metals, so that the metal layer has high thermal stability, the vertical magnetic anisotropy and the synchronous antiferromagnetic coupling strength of the device are good after the metal layer is annealed at a high temperature, and the performance of the device is improved. The problem that in the prior art, due to the fact that metal in the second pinning layer is single, the performance becomes poor after high-temperature annealing is solved, the problem that in the prior art, the performance becomes poor after high-temperature annealing is solved, and it is guaranteed that the performance of a semiconductor device is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductor memory, and in particular, to a semiconductor device and an MRAM. Background Art

[0002] At present, after high-temperature annealing, the MTJ (Magnetic Tunnel Junction) structure, the main structure of MRAM (Magnetoresistive Random Access Memory), will seriously degrade the performance of perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength, resulting in poor reliability of MRAM devices. Summary of the invention

[0003] The main purpose of the present application is to provide a semiconductor device and an MRAM to solve the problem in the prior art that the performance of the MRAM deteriorates after high-temperature annealing.

[0004] In order to achieve the above-mentioned purpose, according to one aspect of the present application, a semiconductor device is provided, which includes a seed layer, a first pinning layer and a second pinning layer, wherein the first pinning layer is located on the surface of the seed layer; the second pinning layer is located on the side of the first pinning layer away from the seed layer, the second pinning layer includes a stacked metal layer and an isolation layer, the metal layer is located on the surface of the isolation layer close to the first pinning layer, and the metal layer includes an alloy composed of multiple metals.

[0005] Optionally, the material of the metal layer includes a first metal and a second metal, wherein the first metal includes a transition metal; and the second metal includes a transition metal and / or an alkaline earth metal.

[0006] Optionally, the first metal includes one of Co, Fe, CoFe and CoFeB, and the second metal includes at least one of Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg.

[0007] Optionally, the second metal accounts for 5%-50% of the metal layer.

[0008] Optionally, the semiconductor device further includes a coupling layer, wherein the coupling layer is located between the first pinning layer and the second pinning layer, and the coupling layer is in contact with the first pinning layer and the metal layer respectively.

[0009] Optionally, the material of the coupling layer includes Ir.

[0010] Optionally, the semiconductor device further includes a reference layer, a first tunneling layer, a free layer, a second tunneling layer and a covering layer, wherein the reference layer is located on a surface of the second pinning layer away from the first pinning layer, and the reference layer is in contact with the isolation layer; the first tunneling layer is located on a surface of the reference layer away from the second pinning layer; the free layer is located on a surface of the first tunneling layer away from the reference layer; the second tunneling layer is located on a surface of the free layer away from the first tunneling layer; and the covering layer is located on a surface of the second tunneling layer away from the free layer.

[0011] Optionally, the material of the isolation layer includes at least one of Ta, W and Mo.

[0012] Optionally, the thickness of the metal layer is in the range of 3 angstroms to 15 angstroms.

[0013] According to another aspect of the present application, an MRAM is provided, and the MRAM includes any one of the semiconductor devices described above.

[0014] According to the technical solution of the present application, the semiconductor device includes a seed layer, a first pinning layer and a second pinning layer, wherein the first pinning layer is located on the surface of the seed layer; the second pinning layer is located on the side of the first pinning layer away from the seed layer, and the second pinning layer includes a stacked metal layer and an isolation layer, wherein the metal layer is located on the surface of the isolation layer close to the first pinning layer, and the metal layer includes an alloy composed of multiple metals. Compared with the problem of poor performance of MRAM after high-temperature annealing in the prior art, the semiconductor device of the present application, since the second pinning layer includes the metal layer, and since the metal layer is an alloy composed of multiple metals, the metal layer has a high thermal stability, which ensures that the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are good after high-temperature annealing of the metal layer, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, and ensuring good performance of the semiconductor device. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The drawings constituting part of the present application are used to provide a further understanding of the present application. The exemplary embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0016] Figure 1 A schematic structural diagram of a semiconductor device according to an embodiment of the present application is shown;

[0017] Figure 2A schematic diagram showing a performance test of an MRAM device in the prior art after high temperature annealing is shown;

[0018] Figure 3 A schematic diagram of a performance test of a semiconductor device after high temperature annealing according to an embodiment of the present application is shown.

[0019] The above drawings include the following reference numerals:

[0020] 10. Seed layer; 20. First pinned layer; 30. Second pinned layer; 40. Coupling layer; 50. Reference layer; 60. First tunneling layer; 70. Free layer; 80. Second tunneling layer; 90. Covering layer; 301. Metal layer; 302. Isolation layer. DETAILED DESCRIPTION

[0021] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0022] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0023] It should be understood that when an element (such as a layer, film, region, or substrate) is described as being "on" another element, the element may be directly on the other element, or there may be intermediate elements. Moreover, in the specification and claims, when an element is described as being "connected" to another element, the element may be "directly connected" to the other element, or "connected" to the other element through a third element.

[0024] As introduced in the background technology, the MRAM in the prior art has the problem of poor performance after high-temperature annealing. To solve the above problem, the embodiments of the present application provide a semiconductor device and an MRAM.

[0025] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0026] According to an embodiment of the present application, a semiconductor device is provided, such as Figure 1As shown, the semiconductor device includes a seed layer 10, a first pinning layer 20 and a second pinning layer 30, wherein the first pinning layer 20 is located on the surface of the seed layer 10; the second pinning layer 30 is located on the side of the first pinning layer 20 away from the seed layer 10, and the second pinning layer 30 includes a stacked metal layer 301 and an isolation layer 302, the metal layer 301 is located on the surface of the isolation layer 302 close to the first pinning layer 20, and the metal layer 301 includes an alloy composed of multiple metals.

[0027] The semiconductor device comprises a seed layer, a first pinning layer and a second pinning layer, wherein the first pinning layer is located on the surface of the seed layer; the second pinning layer is located on the side of the first pinning layer away from the seed layer, the second pinning layer comprises a stacked metal layer and an isolation layer, the metal layer is located on the surface of the isolation layer close to the first pinning layer, and the metal layer comprises an alloy composed of multiple metals. Compared with the problem of poor performance of MRAM after high-temperature annealing in the prior art, the semiconductor device of the present application, since the second pinning layer comprises the metal layer, and since the metal layer is an alloy composed of multiple metals, the metal layer has high thermal stability, ensuring that the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are good after high-temperature annealing, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, and ensuring good performance of the semiconductor device.

[0028] In addition, the semiconductor device of the present application has better data retention capability after high-temperature annealing because the metal layer of the second pinning layer includes an alloy composed of multiple metals, thereby ensuring better reliability of the semiconductor device.

[0029] In the prior art, the material of the metal layer is generally Co. Figure 2 as well as Figure 3 As shown, Figure 2 The synchronous antiferromagnetic coupling strength performance test diagram of the semiconductor device in the prior art after high temperature annealing is shown. Figure 3 The synchronous antiferromagnetic coupling strength performance test diagram of the semiconductor device of the present application after high temperature annealing is shown, wherein the high temperature annealing is annealed at 400°C for 1H, and the synchronous antiferromagnetic coupling strength is represented by AP1 (the first pinned layer) and AP2 (the second pinned layer). Figure 2 as well as Figure 3 It can be seen that Figure 2 The high temperature data retention capability is weak, which makes the reliability of the semiconductor device in the prior art poor. Figure 3The data in is step-up, that is, Figure 3 The high-temperature data retention capability is strong, and it has BEOL (Back End Of Line) compatibility after 400°C, which enhances the data retention capability at high temperatures and ensures that the above-mentioned semiconductor device of the present application has good reliability.

[0030] Among them, perpendicular magnetic anisotropy is a magnetic anisotropy with a preferred orientation along a certain direction due to factors such as interface and lattice distortion. This magnetic anisotropy is very important for the function of the memory. The synchronous antiferromagnetic coupling strength refers to the exchange interaction strength between two adjacent antiferromagnetic layers. When two adjacent antiferromagnetic layers are in a synchronous state, their spin directions are complementary, that is, one spin is up and the other is down. At this time, an exchange interaction called synchronous antiferromagnetic coupling will occur. Therefore, properties such as perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength are more important for judging the function of the memory.

[0031] In order to further ensure the good performance of the semiconductor device, the material of the metal layer includes a first metal and a second metal, wherein the first metal includes a transition metal; and the second metal includes a transition metal and / or an alkaline earth metal. Since the material of the metal layer includes the first metal and the second metal, and since the first metal includes the transition metal, and the second metal includes the transition metal and / or the alkaline earth metal, the metal layer is a structural layer composed of multiple metals, which further ensures that the metal layer has high thermal stability, so that after high-temperature annealing, the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are good, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, and further ensuring the good performance of the semiconductor device.

[0032] In the above implementation process, transition metals have advantages such as good electronic conductivity, high stability and controllable oxidation state. Alkaline earth metals have advantages such as long-term data storage and low power consumption. Specifically, the above alkaline earth metals can provide lower resistivity and better retention time, while also reducing power consumption and increasing lifespan.

[0033] Specifically, the first metal in the metal layer includes a transition metal, and the second metal includes a transition metal and / or an alkaline earth metal. In order to obtain the semiconductor device with superior performance, the specific material selection of the first metal and the second metal can be determined according to experiments, that is, after determining the parameters such as the material and thickness of other structural layers in the semiconductor device, the first metal and the second metal of different materials can be prepared to obtain the semiconductor devices of different materials. The semiconductors corresponding to the metal layers of different materials are respectively subjected to performance tests, mainly including perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength, and the material of the metal layer with the best performance is determined as the preferred material. Therefore, the materials of the first metal and the second metal can be determined according to actual conditions.

[0034] In order to further ensure that the semiconductor device has good performance, the first metal includes one of Co, Fe, CoFe and CoFeB, and the second metal includes at least one of Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg. Since the second metal includes at least one of Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg, the second metal has high thermal stability, ensuring that the second metal has a high-temperature diffusion isolation function, so that after the metal layer is annealed at high temperature, the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling of the semiconductor device will not be degraded, that is, the semiconductor device is guaranteed to have better high-temperature data retention capability, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, further ensuring the reliability of the semiconductor device, and further ensuring the performance of the semiconductor device.

[0035] Specifically, Mg is an alkaline earth metal, and Hf, Zr, Ta, Mo, W, Cr, Ti, Rh and Nb are transition metals. Among them, the materials Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg in the second metal all have extremely high thermal stability, which ensures that the second metal has a high-temperature diffusion isolation function, and ensures that the vertical magnetic anisotropy and synchronous antiferromagnetic coupling strength of the semiconductor device will not degrade after high-temperature annealing, further ensuring that the performance of the semiconductor device is good.

[0036] In addition, the alkaline earth metal in the above-mentioned second metal is not limited to Mg, and semiconductor devices corresponding to alkaline earth metals of different materials can be prepared according to actual conditions, and performance tests can be performed on multiple of the above-mentioned semiconductor devices to obtain the material of the above-mentioned second metal with the best performance.

[0037] In the above implementation process, the metal layer includes one of CoZr, CoFeCr, CoFeBHf and FeW. Wherein, when the material of the metal layer is CoZr, the material of the first metal is Co, and the material of the second metal is Zr; when the material of the metal layer is CoFeCr, the material of the first metal is CoFe, and the material of the second metal is Cr; when the material of the metal layer is CoFeBHf, the material of the first metal is CoFeB, and the material of the second metal is Hf; when the material of the metal layer is FeW, the material of the first metal is Fe, and the material of the second metal is W.

[0038] Of course, the specific materials of the first metal and the second metal in the metal layer are not limited to the above four types. According to actual experimental tests, when the first metal includes one of Co, Fe, CoFe and CoFeB, and the second metal includes at least one of Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg, the metal layers of various materials can be freely combined, and performance tests can be performed on the semiconductor devices with different material combinations, and the material with the best performance can be selected as the optimal material ratio of the semiconductor device.

[0039] In a specific implementation process, the proportion of the second metal in the metal layer is in a range of 5%-50%. Specifically, the proportion of the second metal in the metal layer can be determined according to actual detection results.

[0040] Of course, the proportion of the second metal in the metal layer is not limited to 5%-50%. According to the thickness and material of other layers of the semiconductor device, the metal layers with various proportions can be provided, and then the vertical magnetic anisotropy and synchronous antiferromagnetic coupling and other properties of the metal layers with various proportions can be tested. Finally, the proportion of the second metal with better performance can be determined as the final proportion, that is, the proportion range of the second metal in the metal layer can be determined according to actual conditions.

[0041] In a specific embodiment, Figure 1 As shown, the semiconductor device further includes a coupling layer 40, and the coupling layer 40 is located between the first pinned layer 20 and the second pinned layer 30, and the coupling layer 40 is respectively in contact with the first pinned layer 20 and the metal layer 301. Since the semiconductor device further includes the coupling layer, the first pinned layer and the second pinned layer can be antiferromagnetically coupled according to the coupling layer, which further ensures that the performance of the semiconductor device is good.

[0042] In the above implementation process, the above coupling layer can be formed by PVD (Physical Vapor Deposition). Of course, other manufacturing methods can also be selected. In addition, the above isolation layer and other layer structures can also be obtained by PVD and other methods. In the above PVD operation process, an inert gas or a rare gas such as argon (Ar), helium (He), krypton (Kr) or xenon (Xe) is ionized into a plasma in a sputtering chamber, and the chamber is maintained in a vacuum state. In addition, the PVD processing chamber also contains at least one sputtering target, the material of the target is determined according to the material of the structure to be prepared, and the substrate is arranged to face the substantially flat surface of the sputtering target. The sputtering target is connected to a power supply so that the sputtering target is electrically driven or self-established as a cathode state in a circuit of the power supply, through plasma to ground, such as a grounding part of the sputtering chamber. The substrate is arranged on a base or other structure in the sputtering chamber, and the base or other structure can be at a floating potential, connected to ground, or can be biased to form an anode in the cathode target, with plasma to anode or grounding circuit. The positively ionized portion of the inert gas atoms in the sputtering chamber is electrically attracted to the negatively biased target, causing the plasma ions to bombard the target, thereby causing the atoms in the target to be ejected and deposited on the substrate to form a thin film of the material corresponding to the target on the substrate.

[0043] Specifically, the seed layer is mainly used to ensure that the quality of the first pinned layer is good. The material of the seed layer includes platinum (Pt) or ruthenium (Ru). By reducing or eliminating the lattice mismatch between the subsequent structures such as the first pinned layer and the substrate, the seed layer can be used to improve the adhesion and seeding effect of the subsequently deposited layer. Subsequently, the first pinned layer is formed on the surface of the seed layer by sputtering. Here, the first pinned layer includes a cobalt (Co) layer, and then sputtering is performed to form the coupling layer on the surface of the first pinned layer away from the seed layer. The coupling layer can be formed by iridium (Ir) sputtered from its target. Then, the second pinned layer is formed on the surface of the coupling layer away from the first pinned layer by sputtering. Since the coupling layer is located between the first pinned layer and the second pinned layer, when the semiconductor device is exposed to a magnetic field, the surface atoms of the first pinned layer and the second pinned layer are aligned with the surface atoms of the coupling layer, thereby pinning the orientation of the first pinned layer and the second pinned layer. The first pinned layer and the second pinned layer each exhibit similar magnetic moments, and the coupling layer maintains antiparallel alignment of the magnetic moments of the first pinned layer and the second pinned layer.

[0044] In a specific implementation process, the material of the coupling layer includes Ir. The material of the coupling layer is Ir, because Ir has good magnetic and electrical properties, and because Ir is located between the first pinned layer and the second pinned layer, Ir can realize spin transmission between the first pinned layer and the second pinned layer, further ensuring that the performance of the semiconductor device is good.

[0045] In the above implementation process, in MRAM, the material of the coupling layer is selected as Ir, mainly because Ir has good magnetic and electrical properties, Ir can form a strong exchange coupling with ferromagnets, and has high resistivity and low magnetic leakage characteristics, which is very important for achieving high-density storage. By placing Ir between the first pinned layer and the second pinned layer, spin transfer between the two can be achieved, and an effective exchange bias field can be generated. In addition, the use of Ir in MRAM also has the advantages of increasing reading speed, reducing power consumption and increasing stability. In short, Ir plays a vital role as a coupling layer in MRAM. It not only affects basic parameters such as memory capacity and stability, but also directly determines whether the entire system can meet application requirements such as high speed and low power consumption.

[0046] Of course, the material of the coupling layer is not limited to Ir, and other materials with the same performance may also be selected, which is determined according to actual conditions.

[0047] In a specific embodiment, Figure 1 As shown, the semiconductor device further includes a reference layer 50, a first tunneling layer 60, a free layer 70, a second tunneling layer 80 and a cover layer 90, wherein the reference layer 50 is located on a surface of the second pinned layer 30 away from the first pinned layer 20, and the reference layer 50 is in contact with the isolation layer 302; the first tunneling layer 60 is located on a surface of the reference layer 50 away from the second pinned layer 30; the free layer 70 is located on a surface of the first tunneling layer 60 away from the reference layer 50; the second tunneling layer 80 is located on a surface of the free layer 70 away from the first tunneling layer 60; and the cover layer 90 is located on a surface of the second tunneling layer 80 away from the free layer 70. Since the semiconductor device further includes the reference layer, the first tunneling layer, the free layer, the second tunneling layer and the cover layer, the semiconductor device can realize the storage and reading functions of the magnetic tunnel junction.

[0048] In the above implementation process, the reference layer is a magnetic material with a stable polarity of constant magnetization. The reference layer can generate a magnetoresistance effect by interacting with the free layer, and determine the rotation direction of the electrons in the free layer. The free layer is a thin and movable magnetic material, which can change its magnetization state when an external field strength is applied. When the current passes through the magnetic tunnel junction, it will cause a positive or reverse rotation movement in the free region, thereby realizing data storage and reading. The first tunnel layer and the second tunnel layer are mainly metal oxides, forming an insulating medium. By adjusting the thickness and material properties of the first tunnel layer and the second tunnel layer, the energy required for electrons to cross the insulating interface between the two ferromagnets can be controlled. By greatly increasing the difference in device impedance ratio, the reading sensitivity of the semiconductor device can be improved. In short, the reference layer, the free layer, the first tunnel layer and the second tunnel layer work together to realize the functions of data storage, reading and transmission of the memory.

[0049] In addition, the above-mentioned covering layer is mainly used to include the above-mentioned second tunneling layer and other layers, so as to prevent other layers in the above-mentioned semiconductor device from being damaged, and further ensure that the performance of the above-mentioned semiconductor device is good.

[0050] In a specific implementation process, the material of the isolation layer includes at least one of Ta, W and Mo. The isolation layer can be one of Ta, W or Mo, and the isolation layer is used to isolate the metal layer and the free layer, further ensuring that the performance of the semiconductor device is good.

[0051] In the above implementation process, the thickness of the above isolation layer ranges from 2 angstroms to 4 angstroms.

[0052] In a specific embodiment, the thickness of the metal layer is in the range of 3 angstroms to 15 angstroms.

[0053] In addition, the thickness range of the metal layer is not limited to 3 angstroms to 15 angstroms, and can be 2.5 angstroms, 15.5 angstroms, 16 angstroms, etc., which is determined based on test results.

[0054] The following are several main implementations of the semiconductor device, but the implementations of the present application are not limited thereto.

[0055] In Embodiment 1, the semiconductor device comprises the stacked seed layer, the first pinned layer, the coupling layer, the second pinned layer (including the metal layer and the isolation layer), the reference layer, the first tunneling layer, the free layer, the second tunneling layer and the capping layer. The metal layer is made of the first metal and the second metal, the first metal includes Co, the second metal includes Zr, the coupling layer includes Ir, and the isolation layer includes at least one of Ta, W and Mo.

[0056] Embodiment 2: Embodiment 2 differs from Embodiment 1 in that the first metal in Embodiment 2 includes CoFe, and the second metal in Embodiment 2 includes Cr;

[0057] Embodiment 3: The difference between Embodiment 3 and Embodiment 1 is that the first metal in Embodiment 3 includes CoFeB, and the second metal in Embodiment 3 includes Hf;

[0058] Example 4: The difference between Example 4 and Example 1 is that the first metal in Example 4 includes Fe, and the second metal in Example 4 includes W.

[0059] An embodiment of the present application further provides an MRAM, and the MRAM includes any one of the above-mentioned semiconductor devices.

[0060] The above-mentioned MRAM includes any of the above-mentioned semiconductor devices. Compared with the problem of poor performance of MRAM in the prior art after high-temperature annealing, the above-mentioned MRAM of the present application, because the above-mentioned second pinning layer in the above-mentioned semiconductor device includes the above-mentioned metal layer, and because the above-mentioned metal layer is an alloy composed of multiple metals, the above-mentioned metal layer has high thermal stability, which ensures that the above-mentioned metal layer has good perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device after high-temperature annealing, avoids the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solves the problem of poor performance of MRAM in the prior art after high-temperature annealing, and ensures good performance of the above-mentioned semiconductor device.

[0061] In the above implementation process, the above semiconductor device is mainly an MTJ stacking structure in MRAM, and at least one of the above second metals Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg is arranged in the above metal layer of the above MTJ stacking structure, and because Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg have good thermal stability, the above metal layer has a high-temperature diffusion isolation function. Therefore, in the process of high-temperature annealing of the above MTJ stacking structure, since the above metal layer has a high-temperature diffusion isolation function, the vertical magnetic anisotropy and synchronous antiferromagnetic coupling strength of the above MTJ stacking structure will not be degraded, thereby avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, and further ensuring the good performance of the above MRAM.

[0062] In addition, the first metal in the metal layer in the MRAM includes one of Co, Fe, CoFe and CoFeB, so that the metal layer is a metal alloy composed of the first metal and the second metal, and because the metal alloy has high thermal stability, it is ensured that after high-temperature annealing of the metal layer, the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are good, further ensuring the good performance of the MRAM.

[0063] In the above embodiments of the present invention, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0064] From the above description, it can be seen that the above embodiments of the present application achieve the following technical effects:

[0065] 1) The semiconductor device of the present application includes a seed layer, a first pinning layer and a second pinning layer, wherein the first pinning layer is located on the surface of the seed layer; the second pinning layer is located on the side of the first pinning layer away from the seed layer, and the second pinning layer includes a stacked metal layer and an isolation layer, the metal layer is located on the surface of the isolation layer close to the first pinning layer, and the metal layer includes an alloy composed of multiple metals. Compared with the problem of poor performance of MRAM after high-temperature annealing in the prior art, the semiconductor device of the present application, because the second pinning layer includes the metal layer, and because the metal layer is an alloy composed of multiple metals, the metal layer has a higher thermal stability, which ensures that the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are better after high-temperature annealing, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinning layer in the prior art, solving the problem of poor performance of MRAM after high-temperature annealing in the prior art, and ensuring the good performance of the semiconductor device.

[0066] 2) The MRAM mentioned above in the present application includes any of the above-mentioned semiconductor devices. Compared with the problem of poor performance of MRAM in the prior art after high-temperature annealing, the MRAM mentioned above in the present application, because the second pinned layer in the semiconductor device includes the metal layer, and because the metal layer is an alloy composed of multiple metals, the metal layer has high thermal stability, which ensures that the perpendicular magnetic anisotropy and synchronous antiferromagnetic coupling strength of the device are good after high-temperature annealing, avoiding the problem of poor performance after high-temperature annealing due to the relatively single metal in the second pinned layer in the prior art, solving the problem of poor performance of MRAM in the prior art after high-temperature annealing, and ensuring good performance of the semiconductor device.

[0067] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A semiconductor device, characterized in that: The semiconductor device comprises: Seed layer; A first pinning layer, located on a surface of the seed layer; The second pinning layer is located on a side of the first pinning layer away from the seed layer. The second pinning layer includes a stacked metal layer and an isolation layer. The metal layer is located on a surface of the isolation layer close to the first pinning layer. The metal layer includes an alloy composed of multiple metals.

2. The semiconductor device according to claim 1, wherein: The material of the metal layer includes: a first metal, the first metal comprising a transition metal; The second metal comprises a transition metal and / or an alkaline earth metal.

3. The semiconductor device according to claim 2, characterized in that The first metal includes one of Co, Fe, CoFe and CoFeB, and the second metal includes at least one of Hf, Zr, Ta, Mo, W, Cr, Ti, Rh, Nb and Mg.

4. The semiconductor device according to claim 2, characterized in that The second metal accounts for 5%-50% of the metal layer.

5. The semiconductor device according to claim 1, wherein: The semiconductor device further comprises: The coupling layer is located between the first pinning layer and the second pinning layer, and the coupling layer is in contact with the first pinning layer and the metal layer respectively.

6. The semiconductor device according to claim 5, characterized in that The material of the coupling layer includes Ir.

7. The semiconductor device according to claim 1, wherein: The semiconductor device further comprises: A reference layer, located on a surface of the second pinned layer away from the first pinned layer, the reference layer being in contact with the isolation layer; a first tunneling layer, located on a surface of the reference layer away from the second pinning layer; A free layer, located on a surface of the first tunneling layer away from the reference layer; A second tunneling layer, located on a surface of the free layer away from the first tunneling layer; The capping layer is located on a surface of the second tunneling layer away from the free layer.

8. The semiconductor device according to any one of claims 1 to 7, characterized in that The material of the isolation layer includes at least one of Ta, W and Mo.

9. The semiconductor device according to any one of claims 1 to 7, characterized in that: The thickness of the metal layer is in the range of 3 angstroms to 15 angstroms.

10. An MRAM, characterized in that: A semiconductor device comprising any one of claims 1 to 9.