Silver microparticle composition
By adjusting the particle size distribution and adding amines and diols in the silver microparticle composition, the problem of reducing the sintering volume and low bonding strength of silver microparticles during low-temperature sintering is solved, and the effect of forming a dense sintered layer and high bonding strength at low temperature is achieved. .
Patent Information
- Application Number
- CN202380029460.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-20
- Publication Date
- 2024-12-03
AI Technical Summary
When silver particles are sintered at low temperatures, silver particles with small particle sizes lead to a reduction in sintering volume, forming problems such as many voids and low bonding strength. Silver particles with large particle sizes are difficult to sinter at low temperatures, limiting the bondable components and thermal energy requirements.
The silver microparticle composition is adopted, wherein the average particle size of the silver microparticles is 40 nm or more and 100 nm or less, the volume ratio of silver microparticles with a particle size exceeding 100 nm or less is 5% or less and 25% or less, and the volume ratio of silver microparticles with a particle size exceeding 500 nm is 10%. The above and 60% or less, and amine and diol are added as dispersant and dispersion medium to the composition to form a dense sintered layer.
A dense sintered silver layer is formed at low temperatures to ensure firm bonding of large areas of bonding surfaces, suppress shrinkage of sintered volume and improve bonding strength.
Smart Images

Figure CN119072374A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a silver microparticle composition.
[0002] This application claims priority based on Japanese Patent Application No. 2022-054774 filed on March 30, 2022, and cites all the contents described in the Japanese Patent Application. Background Art
[0003] Bonding compositions or conductive inks that utilize the low-temperature sintering properties of silver microparticles have attracted attention. The bonded silver microparticles have physical properties roughly equivalent to those of general silver bulk, and therefore have very high heat resistance, and are also reliable and have good heat dissipation properties.
[0004] Taking advantage of this property, it has been proposed to use a composition containing silver particles in a bonding material for bonding a light-emitting element such as a light-emitting diode (LED) to a substrate, a bonding material for bonding a semiconductor chip to a substrate, a bonding material for further bonding these substrates to a heat dissipation component, and the like.
[0005] Patent document 1 proposes a bonding material for inorganic raw materials as a bonding material for inorganic raw materials such as metals, wherein the bonding material for inorganic raw materials comprises a paste containing metal colloid particles and a solvent, wherein the metal colloid particles comprise metal nanoparticles (A) and a dispersant (B), and the metal nanoparticles (A) contain metal nanoparticles having a number average particle size of less than 50 nm and a particle size of 100 nm to 200 nm.
[0006] Patent document 2 proposes a silver particle composition as a bonding composition for low-temperature bonding of electronic parts, the silver particle composition comprising silver particles, a dispersant containing an alkoxyamine, and a dispersion medium, wherein the content of the dispersant is 0.1 mass % to 7.0 mass % relative to the content of the silver particles, and the weight loss when heated from room temperature to 200° C. is more than 70 mass % of all organic components contained.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2011-94223
[0010] Patent Document 2: International Publication No. 2016 / 166948 Summary of the invention
[0011] Problems to be solved by the invention
[0012] When silver particles are melted at a low temperature (low temperature sintering), the smaller the particle size of the silver particles is, the lower the sintering temperature can be.
[0013] On the other hand, when silver particles with a small particle size are sintered, the volume of the obtained silver sintered body is greatly reduced compared to the volume of the applied silver particle composition. Therefore, the formed sintered layer has many voids, making it difficult to obtain a dense sintered layer.
[0014] In addition, when a silver particle composition as a bonding composition is sandwiched between the members to be bonded, if the silver particle composition used is a silver particle composition whose volume is greatly reduced after sintering, it is difficult to bond a large area (for example, 25 mm 2 The joining surfaces of the above) are firmly joined to each other.
[0015] Therefore, in order to suppress the volume reduction after sintering, the particle size of the silver particles needs to be increased. However, if the number of silver particles with large particle size increases, it will be difficult to sinter at a low temperature, the joinable components will be limited, or the heat energy required for joining will increase.
[0016] The present invention has been made in view of such actual conditions, and an object of the present invention is to provide a silver microparticle composition capable of forming a sintered layer having few voids and excellent bonding strength while maintaining low-temperature sinterability.
[0017] Technical means of solving problems
[0018] (1) Silver microparticle composition of the present invention
[0019] The invention comprises silver microparticles, amines and diols, wherein the silver microparticle composition comprises:
[0020] The average particle size of the silver microparticles is greater than or equal to 40 nm and less than or equal to 100 nm.
[0021] The volume ratio of the silver particles with a particle size of 100 nm or less to the total volume of the silver particles is 5% or more and 25% or less,
[0022] The volume ratio of the silver microparticles having a particle diameter exceeding 500 nm to the entire silver microparticles is 10% to 60%.
[0023] (2) In the silver microparticle composition of (1), the volume ratio of the silver microparticles having a particle size exceeding 300 nm to the entire silver microparticles is preferably 40% to 90%.
[0024] (3) In the silver microparticle compositions of (1) and (2), preferably, the amine is one or more amines selected from the group consisting of 3-methoxypropylamine, 3-ethoxypropylamine, 3-propoxypropylamine, 3-butoxypropylamine, 2-ethoxypropylamine, 3-isopropoxypropylamine, 2-methoxy-2-methylpropylamine, hexylamine, heptylamine, octylamine and 2-(2-aminoethoxy)ethanol.
[0025] (4) In the silver microparticle composition of (1) to (3), the diol is preferably one or more diols selected from the group consisting of 1,2-octanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, and 3-methyl-1,3-butanediol.
[0026] (5) The silver microparticle composition of (1) to (4) above preferably contains the silver microparticles in an amount of 85% by weight or more and 97% by weight or less.
[0027] (6) The silver microparticle composition of (1) to (5) is preferably prepared at a shear rate of 5 s -1 The measured shear viscosity was 100 Pa·s or more.
[0028] Effects of the Invention
[0029] The silver microparticle composition can be calcined at a low temperature and a dense sintered silver layer can be formed. Therefore, even when components with a large bonding area are bonded to each other, they can be firmly bonded. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] [ Figure 1 ] Figure 1 This is a microscope photograph of the silver microparticle composition of Example 1.
[0031] [ Figure 2 ] Figure 2 This is a graph showing the particle size distribution of the silver fine particle composition of Example 1.
[0032] [ Figure 3 ] Figure 3 This is a microscope photograph of the silver microparticle composition of Example 2.
[0033] [ Figure 4 ] Figure 4 This is a graph showing the particle size distribution of the silver fine particle composition of Example 2.
[0034] [ Figure 5 ] Figure 5 This is a microscope photograph of the silver microparticle composition of Example 3.
[0035] [ Figure 6 ] Figure 6 This is a graph showing the particle size distribution of the silver fine particle composition of Example 3.
[0036] [ Figure 7 ] Figure 7 This is a microscope photograph of the silver microparticle composition of Example 4.
[0037] [ Figure 8 ] Figure 8 This is a graph showing the particle size distribution of the silver fine particle composition of Example 4.
[0038] [ Fig. 9 ] Fig. 9 This is a microscope photograph of the silver microparticle composition of Example 6.
[0039] [ Fig.10 ] Fig.10 This is a graph showing the particle size distribution of the silver microparticle composition of Example 6.
[0040] [ Fig.11 ] Fig.11 This is a microscope photograph of the silver microparticle composition of Example 7.
[0041] [ Fig.12 ] Fig.12 This is a graph showing the particle size distribution of the silver microparticle composition of Example 7.
[0042] [ Fig.13 ] Fig.13 This is a microscope photograph of the silver fine particle composition of Comparative Example 1.
[0043] [ Fig.14 ] Fig.14 This is a graph showing the particle size distribution of the silver fine particle composition of Comparative Example 1.
[0044] [ Fig.15 ] Fig.15 This is a microscope photograph of the silver fine particle composition of Comparative Example 2.
[0045] [ Fig.16 ] Fig.16 This is a graph showing the particle size distribution of the silver microparticle composition of Comparative Example 2.
[0046] [ Fig.17 ] Fig.17 This is a microscope photograph of the silver fine particle composition of Comparative Example 3.
[0047] [ Fig.18 ] Fig.18 This is a graph showing the particle size distribution of the silver fine particle composition of Comparative Example 3.
[0048] [ Fig.19 ] Fig.19This is a microscope photograph of the silver fine particle composition of Comparative Example 4.
[0049] [ Fig. 20 ] Fig. 20 This is a graph showing the particle size distribution of the silver microparticle composition of Comparative Example 4.
[0050] [ Fig.21 ] Fig.21 This is a microscope photograph of the silver fine particle composition of Comparative Example 5.
[0051] [ Fig. 22 ] Fig. 22 This is a graph showing the particle size distribution of the silver microparticle composition of Comparative Example 5.
[0052] [ Fig.23 ] Fig.23 This is a microscope photograph of the silver fine particle composition of Comparative Example 6.
[0053] [ Fig.24 ] Fig.24 This is a graph showing the particle size distribution of the silver microparticle composition of Comparative Example 6.
[0054] [ Fig.25 ] Fig.25 This is a microscopic photograph of a sintered silver layer formed using the silver fine particle composition of Example 1.
[0055] [ Fig.26 ] Fig.26 This is a microscope photograph of a sintered silver layer formed using the silver fine particle composition of Comparative Example 2.
[0056] [ Fig. 27 ] Fig. 27 This is a microscopic photograph of a sintered silver layer formed using the silver fine particle composition of Comparative Example 4. DETAILED DESCRIPTION
[0057] Hereinafter, embodiments of the present invention will be described.
[0058] The silver fine particle composition according to the embodiment of the present invention contains silver fine particles having a specific particle diameter, amine, and diol.
[0059] <Silver particles>
[0060] In the embodiment of the present invention, it is extremely important that the silver microparticles have a specific particle size.
[0061] Specifically, the average particle size of the silver particles is greater than 40 nm and less than 100 nm, the volume ratio of silver particles with a particle size of less than 100 nm to the total silver particles is greater than 5% and less than 25%, and the volume ratio of silver particles with a particle size exceeding 500 nm to the total silver particles is greater than 10% and less than 60%.
[0062] In the silver microparticle composition, the average particle size of the silver microparticles is suppressed to less than 100 nm, and more than 10% of large particles with a particle size exceeding 500 nm are contained on a volume basis. That is, the silver microparticle composition contains small-diameter silver microparticles and large-diameter silver microparticles in a balanced manner.
[0063] Therefore, the silver microparticle composition can be calcined at a low temperature and a dense sintered silver layer can be formed.
[0064] From the viewpoint of reducing volume shrinkage caused by sintering of the silver fine particles, the average particle diameter of the silver fine particles is 40 nm or more and 100 nm or less.
[0065] When the average particle size is less than 40 nm, the amount of amine required for stably dispersing the silver particles increases, so the volume shrinkage accompanying sintering increases, which may result in an increase in the porosity of the silver sintered layer after calcination or a decrease in the bonding strength. On the other hand, if the average particle size exceeds 100 nm, it is difficult to sinter the silver particles at a relatively low temperature. In the present invention, the so-called relatively low temperature refers to a temperature below 200°C.
[0066] The average particle size is preferably 50 nm or more and 80 nm or less.
[0067] In the present invention, the average particle size is the primary average particle size of the silver particles and is the number average particle size.
[0068] The average particle size is obtained by observing and photographing the silver microparticles at a magnification of 50,000 times using a scanning electron beam microscope (S-4800 model manufactured by Hitachi), measuring the particle size of 300 points of the microparticles contained in the image obtained by the photograph using image analysis software (WinROOF manufactured by MITANI CORPORATION), and calculating the numerical average value.
[0069] Among the silver particles, the volume ratio of silver particles having a particle diameter of 100 nm or less to the entire silver particles is 5% or more and 25% or less.
[0070] When the volume ratio of silver particles with a particle size of less than 100 nm is less than 5%, it is difficult to achieve a balance with the average particle size, and low-temperature sintering properties are impaired. On the other hand, if the volume ratio of silver particles with a particle size of less than 100 nm exceeds 25%, the particles with a small average particle size become excessive, so the volume shrinkage accompanying calcination becomes large. Therefore, it is difficult to use for joining components with a large area of the joined surface.
[0071] The volume ratio of the silver microparticles having a particle size of 100 nm or less to the entire silver microparticles is preferably 10% or more and 25% or less.
[0072] The volume ratio was calculated using the image analysis software.
[0073] Furthermore, among the silver particles, the volume ratio of the silver particles having a particle diameter exceeding 500 nm to the entire silver particles is 10% to 60%.
[0074] Thus, in the silver fine-particle composition containing silver fine-particles having a large particle size, volume shrinkage during firing can be suppressed.
[0075] When the volume ratio of the silver particles with a particle size of more than 500 nm is less than 10%, it is difficult to suppress the volume shrinkage during calcination. On the other hand, if the volume ratio of the silver particles with a particle size of more than 500 nm exceeds 60%, it is difficult to achieve a balance with the average particle size, and the low temperature sintering property is impaired.
[0076] Among the silver microparticles, the volume ratio of microparticles having a particle diameter exceeding 300 nm to the entire silver microparticles is preferably 50% to 90%.
[0077] By setting the volume ratio of the fine particles having a particle size exceeding 300 nm to 50% or more, volume shrinkage is less likely to occur during calcination.
[0078] When the volume ratio of the microparticles with a particle size of more than 300 nm is less than 50%, the volume shrinkage after calcination tends to become large, making it difficult to use for joining components with a large area of the joined surface. On the other hand, if the volume ratio of the microparticles with a particle size of more than 300 nm exceeds 90%, it is difficult to achieve a balance with the average particle size.
[0079] The volume ratio of the fine particles having a particle diameter exceeding 300 nm to the entire silver fine particles is more preferably 50% or more and 80% or less.
[0080] <Amine>
[0081] The amine is a component that prevents the aggregation of silver microparticles and improves the dispersion stability of the silver microparticles. The amine has a function as a dispersant.
[0082] It is considered that in the silver microparticle composition, at least a part of the amine is coordinated to and present in the silver microparticles, thereby protecting the silver microparticles from aggregation. Therefore, as the amine, an amine having a polar group can be used.
[0083] As the amine having such a function, an amine having 4 to 8 carbon atoms is preferred.
[0084] The amine is preferably a primary amine having a boiling point of 180° C. or less from the viewpoint of ensuring low-temperature sintering properties of the silver fine particle composition.
[0085] When the silver microparticle composition is welded, if the amine remains, it will hinder the welding of the silver microparticles. Therefore, it is expected that the amine evaporates or decomposes as early as possible during calcination and detaches from the surface of the silver microparticles. In this regard, the boiling point of the amine is preferably below 180°C, more preferably below 150°C.
[0086] In the present invention, the boiling point refers to the boiling point at 1 atmosphere pressure.
[0087] In addition, when a primary amine is selected as the amine, compared with a secondary amine or a tertiary amine, steric hindrance is less and thus it is easy to adsorb to silver microparticles, thereby improving the effect of stabilizing the dispersion of silver microparticles, which is advantageous in the above aspect.
[0088] The amine may be linear or branched.
[0089] The amine may be a compound including a functional group other than amine, such as a hydroxyl group, a carboxyl group, an alkoxy group, a carbonyl group, an ester group, or a mercapto group.
[0090] Preferred specific examples of the amine include 3-methoxypropylamine, 3-ethoxypropylamine, 3-propoxypropylamine, 3-butoxypropylamine, 2-ethoxypropylamine, 3-isopropoxypropylamine, 2-methoxy-2-methylpropylamine, hexylamine, heptylamine, octylamine, 2-(2-aminoethoxy)ethanol, etc. These amines may be used alone or in combination of two or more.
[0091] The content of the amine in the silver microparticle composition is preferably 0.1% by weight or more and 5% by weight or less.
[0092] If the content of the amine in the silver microparticle composition is 0.1% by weight or more, the effect as a dispersant is exerted, and there is a tendency that the dispersion stability of the silver microparticle composition is preferred. In addition, if the content of the amine is 5% by weight or less, the amine that hinders the fusion of the silver microparticles during calcination disappears or tends to become a trace amount.
[0093] A more preferred lower limit of the amine content is 0.2% by weight, a more preferred upper limit is 4% by weight, a further preferred lower limit is 0.3% by weight, and a further preferred upper limit is 3% by weight.
[0094] <Diol>
[0095] The diol functions as a dispersion medium in the silver fine particle composition.
[0096] When glycol is used as a dispersion medium, the viscosity of the silver microparticle composition can be easily adjusted. In addition, when glycol is used as a dispersion medium, the life of the silver microparticle composition when used as a coating paste can be easily ensured.
[0097] The diol is preferably a diol having a boiling point of 200° C. or higher from the viewpoint of ease of handling when applied as a joining material to members to be joined.
[0098] The diol that functions as a dispersion medium is preferably a diol having 5 to 9 carbon atoms.
[0099] Preferred specific examples of the diol include 1,2-octanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, and 3-methyl-1,3-butanediol.
[0100] These diols may be used alone or in combination of two or more.
[0101] The silver fine particle composition may further contain an alcohol (an alcohol having one or three or more hydroxyl groups) other than diol as a component functioning as a dispersion medium.
[0102] In addition, the silver microparticle composition may also contain compounds such as isotridecanol and 2,2,4-trimethylpentane-1,3-diol monoisobutyrate (also known as texanol) as components that function as a dispersion medium. If these components are contained, the viscosity of the silver microparticle composition becomes easier to adjust.
[0103] The concentration of the diol based on the entire silver microparticle composition is preferably 2% by weight or more and 15% by weight or less.
[0104] When the concentration of the diol is within the above range, separation of the silver microparticles and the diol can be effectively prevented, and coating stability of the silver microparticle composition is improved.
[0105] On the other hand, if the concentration of the diol is less than 2% by weight, the shear viscosity of the silver microparticle composition is too high, so the operability is poor and it is difficult to apply it to the joined component. In addition, if the concentration of the diol exceeds 15% by weight, the proportion of the fluid contained in the silver microparticle composition increases, and the sedimentation rate of the silver microparticles increases, so the separation of the diol and the silver microparticles in the silver microparticle composition cannot be effectively prevented, and the stability of the silver microparticle composition may be reduced. Furthermore, since the content of the silver microparticles in the silver microparticle composition decreases, the density of the silver sintered body obtained by calcination becomes low, and sometimes sufficient strength cannot be obtained.
[0106] A more preferred concentration of the diol is 3% by weight or more and 12% by weight or less.
[0107] In the silver microparticle composition, the total amount of components other than the silver microparticles is preferably as small as possible within a range that does not impair the performance of the silver microparticle composition.
[0108] The content of the silver fine particles relative to the entire silver fine particle composition is preferably 85% by weight or more and 97% by weight or less.
[0109] When the content of the silver particles is less than 85% by weight, the volume may be greatly reduced during the calcination process. In addition, the amount of gas generated during calcination increases, and the silver sintered body is prone to voids. On the other hand, if the content of the silver particles exceeds 97% by weight, the silver particle composition cannot maintain the shape of a paste, and sometimes the silver particles aggregate and cause the viscosity of the silver particle composition to change. In the above case, the silver particle composition cannot be stably applied.
[0110] The silver microparticle composition may contain a polymer dispersant. The polymer dispersant can further improve the dispersibility of the silver microparticles or function as a dispersion medium for the silver microparticles.
[0111] As the polymer dispersant, a commercially available polymer dispersant can be used.
[0112] Examples of the commercially available products include SOLSPERSE 11200, SOLSPERSE 13940, SOLSPERSE 16000, SOLSPERSE 17000, SOLSPERSE 18000, SOLSPERSE 20000, SOLSPERSE 21000, SOLSPERSE 24000, SOLSPERSE 26000, SOLSPERSE 27000, SOLSPERSE 28000 (Japan Lubrizol Lubrizol (manufactured by Japan Chemicals Co., Ltd.); DISPERBYK 118, DISPERBYK 142, DISPERBYK 160, DISPERBYK 161, DISPERBYK 162, DISPERBYK 163, DISPERBYK 166, DISPERBYK 170, DISPERBYK 180, DISPERBYK 182, DISPERBYK 184, DISPERBYK 190, DISPERBYK 2155 (manufactured by Japan Chemicals Co., Ltd.); EFKA-46, EFKA-47, EFKA-48, EFKA-49 (manufactured by EFKA Chemical Co., Ltd.); polymer (polymer) r) 100, polymer 120, polymer 150, polymer 400, polymer 401, polymer 402, polymer 403, polymer 450, polymer 451, polymer 452, polymer 453 (manufactured by EFKA Chemical Co., Ltd.); Ajisper PB711, Ajisper PA111, Ajisper PB811, Ajisper PW911 (manufactured by Ajinomoto Co., Ltd.); Flowlen DOPA-15B, Flowlen DOPA-22, Flowlen DOPA-17, Flowlen TG-730W, Flowlen G-700, Flowlen TG-720W (manufactured by Kyoeisha Chemical Industry Co., Ltd.), etc.
[0113] When the silver microparticle composition contains the polymer dispersant, the content of the polymer dispersant is preferably 1 wt % or less. If the content of the polymer dispersant exceeds 1 wt %, the fusion of the silver microparticles is easily hindered during calcination.
[0114] In addition to the above-mentioned components, the silver microparticle composition of the present embodiment may also add any components such as oligomer components, resin components, organic solvents (which can dissolve or disperse a part of the solid components), surfactants, thickeners or surface tension adjusters that play a role as a binder within the scope that does not impair the effect of the present invention to impart appropriate viscosity corresponding to the purpose of use, or impart functions such as adhesion, drying or printability. The above-mentioned arbitrary components are not particularly limited.
[0115] Examples of the resin component include polyester resins, polyurethane resins, polyacrylate resins, polyacrylamide resins, polyether resins, melamine resins, and terpene resins. These resin components may be used alone or in combination of two or more.
[0116] Examples of the organic solvent include methyl alcohol, ethyl alcohol, n-propyl alcohol, 2-propyl alcohol, 1,2,6-hexanetriol, 1-ethoxy-2-propanol, 2-butoxyethanol, ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol having a weight average molecular weight of 200 to 1,000, propylene glycol, dipropylene glycol, tripropylene glycol, polypropylene glycol having a weight average molecular weight of 300 to 1,000, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, N,N-dimethylacetamide, glycerin, acetone, and the like. These may be used alone or in combination of two or more.
[0117] When the organic solvent is contained, the organic solvent may also function as a dispersion medium for the silver fine particles.
[0118] Examples of the thickener include polyester emulsion resins, acrylic emulsion resins, polyurethane emulsion resins, or emulsions such as blocked isocyanates; cellulose derivatives such as methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, and hydroxypropyl methyl cellulose; and polysaccharides such as xanthan gum and guar gum. These may be used alone or in combination of two or more.
[0119] The surfactant is not particularly limited, and any of anionic surfactants, cationic surfactants, and nonionic surfactants can be used, and examples thereof include alkylbenzene sulfonates, quaternary ammonium salts, etc. Fluorine-based surfactants are preferred because they can achieve the desired effect with a small amount of addition.
[0120] The silver microparticle composition is preferably prepared by shearing at a rate of 5 s -1 The measured shear viscosity was 100 Pa·s or more.
[0121] When the shear viscosity is 100 Pa·s or more, the silver microparticle composition does not drip when applied to the member to be joined, so that the coating thickness of the silver microparticle composition can be set to a desired thickness.
[0122] Furthermore, the members to be joined by the silver microparticle composition can be made members that can withstand tests with large strains such as temperature cycle tests.
[0123] On the other hand, when the shear viscosity is less than 100 Pa·s, it is difficult to apply the silver fine particle composition thickly, and it is difficult to form a bonding layer that can withstand a large strain.
[0124] If the shear viscosity of the silver microparticle composition is too high, the coating method may be limited or the fusion property with the member to be joined may be deteriorated, resulting in inconvenience in handling.
[0125] From these viewpoints, the shear viscosity is preferably 100 Pa·s or more and 500 Pa·s or less. The shear viscosity is more preferably 100 Pa·s or more and 400 Pa·s or less.
[0126] The shear viscosity was measured using a cone-plate viscometer (rheometer Physica MCR301 manufactured by Anton Paar).
[0127] Here, at 25°C, a cone plate (φ25 mm, angle 2°, gap 0.105 mm) was used to first -1 After pre-shearing, the shearing speed was set at 0.1s. -1 ~100s -1 The viscosity behavior when changing between 27 points was measured and read for 5 seconds. -1 The value at time.
[0128] The shear viscosity can be adjusted by adjusting the particle size of silver microparticles, adjusting the content of amines, adjusting the amount of diol or other components added, adjusting the blending ratio of each component, adding a thickener, etc.
[0129] (Method for producing silver microparticle composition)
[0130] Examples of a method for producing the silver fine particles include a method of preparing silver fine particles having an amine attached to the surface, kneading the obtained silver fine particles with diol, and dispersing the silver fine particles in the diol.
[0131] The method for preparing silver microparticles having amine attached to the surface is not particularly limited, and examples thereof include a method of preparing a dispersion containing silver microparticles and then washing the dispersion.
[0132] As a process for preparing a dispersion containing silver microparticles, for example, the silver salt (or silver ions) dissolved in the solvent can be reduced as described below, and the reduction sequence can be a sequence based on a chemical reduction method. In addition, a metal amine complex decomposition method can also be used.
[0133] Specifically, for example, the silver salt constituting the silver microparticles, the amine having 4 to 8 carbon atoms, the polymer dispersant prepared as required, and the dispersion solvent (organic solvent) can be prepared by reducing the raw material solution. In addition, a part of the components of the raw material solution can also be dispersed without being dissolved. In addition, the raw material solution can also contain water.
[0134] By the reduction, silver microparticles having amine attached to a part of the surface can be obtained.
[0135] As the initiating material for obtaining silver microparticles with amine attached to a part of the surface, various known silver salts or their hydrates can be used. As the initiating material, for example, silver salts such as silver nitrate, silver sulfate, silver chloride, silver oxide, silver acetate, silver oxalate, silver formate, silver nitrite, silver chlorate, and silver sulfide can be cited, and there is no particular limitation as long as they are compounds that can be dissolved in an appropriate dispersion medium and can be reduced. In addition, these can be used alone or in combination of multiple types.
[0136] The method for reducing these silver salts in the raw material solution is not particularly limited, and for example, a method using a reducing agent, a method of irradiating light such as ultraviolet light, an electron beam, ultrasonic waves or thermal energy, etc. Among these, the method using a reducing agent is preferred from the viewpoint of easy operation.
[0137] As the reducing agent, there can be listed: amine compounds such as dimethylamine ethanol, methyldiethanolamine, triethanolamine, phenidone, hydrazine, etc.; hydrogen compounds such as sodium borohydride, hydrogen iodide, hydrogen, etc.; oxides such as carbon monoxide and sulfurous acid, such as ferrous sulfate, iron oxide, iron fumarate, iron lactate, iron oxalate, iron sulfide, tin acetate, tin chloride, tin diphosphate, tin oxalate, tin oxide, tin sulfate, etc.; sugars such as ethylene glycol, glycerol, formaldehyde, hydroquinone, pyrogallol, tannin, tannic acid, salicylic acid, D-glucose, etc., but if it is a reducing agent that can be dissolved in a dispersion medium and reduce the silver salt, it is not particularly limited. When using the reducing agent, light and / or heat can also be added to promote the reduction reaction.
[0138] As a specific method for preparing silver microparticles having amine attached to the surface using the silver salt, the amine, the dispersing solvent and the reducing agent, for example, there can be cited a method of dissolving the silver salt in an organic solvent (such as toluene, etc.) to prepare a silver salt solution, adding the amine to the silver salt solution, and then slowly dropping a solution in which the reducing agent is dissolved therein.
[0139] In the dispersion liquid containing silver microparticles with amine attached to the surface obtained as described above, in addition to the silver microparticles, there are also counter ions of silver salt, residues of reducing agent or amine not attached to the silver microparticles, and there is a tendency that the electrolyte concentration or organic matter concentration of the entire liquid is high. The liquid in this state is easy to coagulate and precipitate the silver microparticles due to its high conductivity. Therefore, it is preferred to wash the solution containing the silver microparticles to remove the excess residue.
[0140] As the cleaning method, for example, there can be listed a method of allowing a dispersion containing silver microparticles with amines attached to the surface to stand for a certain period of time, removing the resulting supernatant, then adding alcohol (methanol, etc.) and stirring again, further allowing to stand for a certain period of time and removing the resulting supernatant, and repeating the above steps several times; a method of performing centrifugal separation instead of the above standing; a method of performing desalination by an ultrafiltration device or an ion exchange device, etc. By removing excess residues and organic solvents through such cleaning, silver microparticles with amines attached to the surface suitable for the above silver microparticle composition can be obtained.
[0141] Silver microparticles having amines attached to the surface can also be produced by using a metal amine complex decomposition method.
[0142] When the metal amine complex decomposition method is used, silver microparticles can be produced by, for example, the following steps: a first step of mixing an amine having a polar group with a silver compound containing silver atoms to generate a complex compound containing the silver compound and the amine; and a second step of heating the complex compound to decompose it to generate silver microparticles.
[0143] For example, a complex compound formed by a metal compound such as silver oxalate containing silver and an amine is heated in the presence of an amine, so that the atomic silver generated by the decomposition of the metal compound such as the oxalate ion contained in the complex compound is condensed, thereby producing silver microparticles with amine attached to the surface.
[0144] When silver microparticles are produced by the metal amine complex decomposition method, relatively weak coordination bonds of multiple amine molecules are generated on the surface of the produced silver microparticles, which form a dense protective coating on the surface of the silver microparticles, thereby producing silver microparticles with a clean surface and excellent storage stability.
[0145] Furthermore, since the amine molecules forming the coating can be easily released by heating or the like, the obtained silver microparticles can be sintered at a very low temperature.
[0146] The silver fine particle composition can be obtained by kneading the silver fine particles having amine attached to the surface obtained by the above method and diol.
[0147] The kneading method of the silver fine particles with amine attached thereto and the diol is not particularly limited, and the kneading can be carried out by a conventionally known method using a stirrer or a blender, etc. The mixture can also be stirred by a tool such as a spatula, or by using an ultrasonic homogenizer with a suitable output power.
[0148] The silver fine particle composition according to the embodiment of the present invention has a predetermined particle size distribution.
[0149] The particle size distribution of the silver microparticles can be adjusted by, for example, changing the mixing ratio of the raw materials.
[0150] In addition, when the silver particles are produced by the metal amine complex decomposition method, the particle size distribution of the silver particles can be adjusted by, for example, the heating conditions in the second step. In order to achieve a predetermined particle size distribution of the silver particles, for example, a method of adjusting the heating rate in the second step within a range of 3°C / min to 20°C / min can be adopted.
[0151] When the heating rate is faster than 20° C. / min, the particle size distribution of the silver microparticles tends to be narrower, while when the heating rate is slower than 3° C. / min, the average particle size of the silver microparticles tends to be larger.
[0152] At this time, the heating means is not particularly limited, and thermostatic bath, oil bath, various heaters, microwave, hot plate, etc. can be cited. In addition, in order to reproduce the complex particle size distribution of the silver microparticles, it is preferred to control the heating conditions while actually measuring the temperature of the reaction solution. Furthermore, in order to stably produce the silver microparticles, it is preferred to have a heating means that can set a temperature program.
[0153] Alternatively, silver particles having a predetermined particle size distribution may be produced by changing the mixing ratio of the raw materials or the heating conditions in the second step of the metal amine complex decomposition method to prepare silver particles prepared under different conditions and mixing these silver particles.
[0154] (How to use the silver microparticle composition)
[0155] The silver microparticle composition can be used as a bonding composition.
[0156] For example, when two joined members (a first joined member and a second joined member) are joined, the first joined member and the second joined member can be joined by the following steps:
[0157] (1) a coating step of coating the bonding composition (silver particle composition) between the first bonded member and the second bonded member; and
[0158] (2) A firing step of firing the joining composition applied between the first member to be joined and the second member to be joined at a desired temperature (for example, 200° C. or less, preferably about 150° C.).
[0159] During the calcining process, the first joined member and the second joined member can be pressurized in the direction facing each other. Even if no special pressurization is performed, sufficient bonding strength can be obtained, which is also one of the advantages of the silver microparticle composition of the embodiment of the present invention. In addition, when calcining, the temperature can also be increased or decreased in stages. In addition, a surfactant or a surfactant can also be applied to the surface of the joined member in advance.
[0160] The term "coating" in the coating step includes coating the bonding composition in a planar form and coating (drawing) the bonding composition in a linear form. The shape of the coating film including the bonding composition before being coated and heated and fired can be set to a desired shape.
[0161] Therefore, the bonding layer formed through the calcination step includes a planar bonding layer or a linear bonding layer.
[0162] The first member to be joined and the second member to be joined that can be joined using the joining composition are not particularly limited as long as they can be coated with the joining composition and joined by heating and calcining. However, members having heat resistance to a degree that will not be damaged by the temperature during joining are preferred.
[0163] Examples of materials constituting such joined components include: polyesters such as polyamide (PA), polyimide (PI), polyamide-imide (PAI), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), polycarbonate (PC), polyether sulfone (PES), vinyl resin, fluororesin, liquid crystal polymer, ceramics, glass, or metal.
[0164] The shape of the member to be joined is not particularly limited, and various shapes such as plate-like and belt-like can be cited. In addition, the member to be joined can be rigid or flexible. Furthermore, the size of the member to be joined can also be appropriately selected.
[0165] In order to improve the adhesion or close contact with the bonding composition, the member to be bonded may be formed with a surface layer such as a primer, or may be subjected to a surface treatment such as a corona treatment, a plasma treatment, an ultraviolet (UV) treatment, or an electron beam treatment.
[0166] As the first and second joined members, resin substrates, metal plates, light-emitting elements such as LEDs, semiconductor chips, ceramic substrates formed with electronic circuits, etc. can be cited. The bonding layer (sintered layer) formed using the bonding composition has high bonding strength, so it can also be preferably used for bonding light-emitting elements such as LEDs, semiconductor chips, etc. with metal substrates, ceramic substrates, etc.
[0167] In the process of applying the bonding composition to the first bonded member and / or the second bonded member, various methods can be used, for example, dipping, screen printing, spraying, rod coating, spin coating, inkjet, dispenser, pin transfer, stamping, coating with a brush, cast, flexographic, gravure, flat plate, transfer, hydrophilic-hydrophobic patterning, syringe, pin transfer, stencil printing, etc. Among them, the bonding composition can be preferably used for dispenser, pin transfer, and stencil printing due to its high solid content concentration.
[0168] The method for performing the calcination is not particularly limited, and for example, a conventionally known oven or the like can be used to heat the bonding composition applied or drawn on the bonded member to a temperature of, for example, 200° C. or less. The lower limit of the heating temperature is not necessarily limited, and is preferably a temperature within a range where the bonded members can be bonded to each other and the effects of the present invention are not impaired.
[0169] In order to obtain the highest possible bonding strength, the amount of organic matter derived from amines, diols, etc. remaining in the sintered layer formed through the calcination step is preferably as small as possible, but a part of the organic matter may remain.
[0170] The bonding composition can form a sintered layer (bonding layer) having sufficient strength even when calcined at a low temperature of 200° C. or less, so that relatively heat-sensitive bonding members can be bonded to each other. In addition, the calcination time is not particularly limited as long as it is a calcination time that allows bonding members to be bonded to each other.
[0171] Example
[0172] Hereinafter, the embodiments of the present invention will be described in more detail with reference to examples, but the embodiments of the present invention are not limited to the following examples.
[0173] (Example 1)
[0174] <Manufacturing of silver microparticles (A)>
[0175] To a mixed solution of 35.0 g of 3-methoxypropylamine (manufactured by Tokyo Chemical Industry), 40.0 g of 3-ethoxypropylamine (manufactured by Tokyo Chemical Industry), and 33.0 g of decanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 30.0 g of silver oxalate (manufactured by Toyo Chemical Industry) was added while stirring to obtain a viscous substance.
[0176] Next, the obtained viscous substance was heated to 100° C. over 12 minutes and allowed to react.
[0177] Then, 150 ml of methanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (A) having amine adsorbed on the surface.
[0178] 0.3 g of 2-ethyl-1,3-hexanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added to 5.0 g of the silver fine particles (A), and the mixture was thoroughly kneaded to obtain a silver fine particle composition.
[0179] (Example 2)
[0180] <Manufacturing of silver microparticles (B)>
[0181] Silver fine particles (B) were obtained in the same manner as in the production of the silver fine particles (A) in Example 1, except that the viscous material was heated to 100° C. over 8 minutes.
[0182] 0.3 g of 2-ethyl-1,3-hexanediol was added to 5.0 g of the silver fine particles (B), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0183] (Example 3)
[0184] <Manufacturing of silver microparticles (C)>
[0185] Silver fine particles (C) were obtained in the same manner as in the production of the silver fine particles (A) in Example 1, except that the amount of decanol was changed to 30.0 g and the viscous material was heated to 100° C. over 10 minutes.
[0186] 0.3 g of 2-ethyl-1,3-hexanediol was added to 5.0 g of the silver fine particles (C), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0187] (Example 4)
[0188] <Manufacturing of silver microparticles (D)>
[0189] Silver fine particles (D) were obtained in the same manner as in the production of the silver fine particles (A) in Example 1, except that the amount of decanol was changed to 35.0 g and the viscous material was heated to 100° C. over 9 minutes.
[0190] 0.3 g of 2-ethyl-1,3-hexanediol was added to 5.0 g of the silver fine particles (D), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0191] (Example 5)
[0192] A silver fine particle composition was obtained in the same manner as in Example 1 except that 0.35 g of 2,4-diethyl-1,5-pentanediol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) was added instead of 2-ethyl-1,3-hexanediol.
[0193] (Example 6)
[0194] <Manufacturing of silver microparticles (E)>
[0195] 10.0 g of silver oxalate was added to a mixed solution of 10.0 g of 3-ethoxypropylamine and 20.0 g of 2-(2-aminoethoxy)ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) with stirring to obtain a viscous substance.
[0196] Next, the obtained viscous substance was heated to 100° C. over 4 minutes and allowed to react.
[0197] Then, 30 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (E) with amine adsorbed on the surface.
[0198] <Manufacturing of silver microparticles (F)>
[0199] 3.0 g of silver oxalate was added to 2.0 g of 3-methoxypropylamine while stirring, thereby obtaining a viscous substance.
[0200] Next, the obtained viscous substance was heated to 100° C. over 1.5 minutes and allowed to react.
[0201] Then, 10 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (F) having amine adsorbed on the surface.
[0202] 0.4 g of 2,4-diethyl-1,5-pentanediol, 0.13 g of 1,2-octanediol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), and 0.02 g of Sonupas 21000 (manufactured by Lubrizol) were added to 3.0 g of silver particles (E) and 2.0 g of silver particles (F), and the mixture was thoroughly kneaded to obtain a silver particle composition.
[0203] (Example 7)
[0204] <Manufacturing of silver microparticles (G)>
[0205] Silver fine particles (G) were obtained in the same manner as in the production of the silver fine particles (D) in Example 4 except that the amount of decanol was changed to 40.0 g.
[0206] 0.2 g of 2-ethyl-1,3-hexanediol and 0.1 g of 1,2-octanediol were added to 5.0 g of the silver fine particles (G), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0207] (Comparative Example 1)
[0208] 0.2 g of 2-ethyl-1,3-hexanediol was added to 2.5 g of the silver fine particles (A) of Example 1 and 2.5 g of the silver fine particles (E) of Example 6, and the mixture was fully kneaded to obtain a silver fine particle composition.
[0209] (Comparative Example 2)
[0210] <Manufacturing of silver microparticles (H)>
[0211] To a mixed solution of 9.0 g of 3-methoxypropylamine and 90.0 g of diethylene glycol monobutyl ether acetate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 30.0 g of silver oxalate was added while stirring to obtain a viscous substance.
[0212] Next, the obtained viscous substance was heated to 140° C. over 10 minutes and reacted.
[0213] Then, 9.0 g of 3-methoxypropylamine was added, the reaction liquid was cooled, and 8.0 g of 3-ethoxypropylamine was added.
[0214] Furthermore, 100 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (H) having amine adsorbed on the surface.
[0215] 0.56 g of 2-ethyl-1,3-hexanediol was added to 5.0 g of the silver fine particles (H), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0216] (Comparative Example 3)
[0217] <Production of silver microparticles (I)>
[0218] 30.0 g of silver oxalate was added to a mixed solution of 4.5 g of 3-methoxypropylamine and 90.0 g of diethylene glycol monobutyl ether acetate while stirring, thereby obtaining a viscous substance.
[0219] Next, the obtained viscous substance was heated to 140° C. over 10 minutes and reacted.
[0220] Then, 9.0 g of 3-methoxypropylamine was added and the reaction liquid was cooled.
[0221] Furthermore, 100 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (I) having amine adsorbed on the surface.
[0222] 0.56 g of 2-ethyl-1,3-hexanediol was added to 5.0 g of the silver fine particles (I), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0223] (Comparative Example 4)
[0224] <Manufacturing of silver microparticles (J)>
[0225] To a mixed solution of 7.0 g of 3-methoxypropylamine and 0.5 g of dodecylamine (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.), 6.0 g of silver oxalate was added while stirring to obtain a viscous substance.
[0226] Next, the obtained viscous substance was heated to 100° C. over 3 minutes and allowed to react.
[0227] Then, 20 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (J) having amine adsorbed on the surface.
[0228] 1.2 g of isotridecanol and 0.03 g of Sonupas 21000 (manufactured by Lubrizol) were added to 6.0 g of silver fine particles (J), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0229] (Comparative Example 5)
[0230] <Manufacturing of silver microparticles (K)>
[0231] 10.0 g of silver oxalate was added to a mixed solution of 5.0 g of 3-ethoxypropylamine and 11.0 g of 3-methoxypropylamine while stirring, thereby obtaining a viscous substance.
[0232] Next, the obtained viscous material was reacted in a constant temperature bath at 120°C.
[0233] Then, 30 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (K) having amine adsorbed on the surface.
[0234] 0.32 g of 1-decanol and 0.06 g of Sonupas 16000 (manufactured by Lubrizol) were added to 4 g of the silver fine particles (K) and 4 g of the silver fine particles (E) of Example 6, and the mixture was fully kneaded to obtain a silver fine particle composition.
[0235] (Comparative Example 6)
[0236] <Manufacturing of silver microparticles (L)>
[0237] 3.0 g of silver oxalate was added to 3.0 g of 3-methoxypropylamine while stirring, thereby obtaining a viscous substance.
[0238] Next, the obtained viscous substance was heated to 100° C. over 1.5 minutes and allowed to react.
[0239] Then, 10 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (L) having amine adsorbed on the surface.
[0240] <Manufacturing of silver microparticles (M)>
[0241] 3.0 g of silver oxalate was added to 6.0 g of 2-(2-aminoethoxy)ethanol while stirring to obtain a viscous substance.
[0242] Next, the obtained viscous substance was heated to 100° C. over 15 minutes and allowed to react.
[0243] Then, 10 ml of methanol was added to the reaction solution and stirred, and then the silver microparticles were precipitated and separated by centrifugation, and the supernatant was removed. The above operation was repeated again to obtain silver microparticles (M) having amine adsorbed on the surface.
[0244] 0.15 g of 2,4-diethyl-1,5-pentanediol, 0.06 g of 1,2-octanediol and 0.01 g of Sonupas 21000 (manufactured by Lubrizol) were added to 0.5 g of silver fine particles (L) and 1.5 g of silver fine particles (M), and the mixture was fully kneaded to obtain a silver fine particle composition.
[0245] [Evaluation test]
[0246] (1) Particle size measurement
[0247] The silver microparticle composition obtained in the above manner was observed and photographed at a magnification of 50,000 times using a scanning electron beam microscope (S-4800 model manufactured by Hitachi). For the microparticles contained in the image obtained by the photograph, 300 particles were randomly extracted, and the particle size was measured using image analysis software (WinROOF manufactured by MITANI CORPORATION), and the number average particle size was calculated.
[0248] Figure 1 , 3 , 5, 7, 9, 11, 13, 15, 17, 19, 21 and 23 are parts of the captured images.
[0249] The volume of the silver microparticles was calculated based on the particle diameter of each particle calculated from the microscope photograph, assuming that each particle was a sphere. Based on the result, the volume ratio was determined.
[0250] The results are shown in Figure 2 , 4 , 6, 8, 10, 12, 14, 16, 18, 20, 22 and 24.
[0251] In addition, in each figure showing the results, the vertical axis represents the frequency (%) of the volume ratio, and the horizontal axis represents the particle size (nm). In addition, regarding the meaning of the particle size in each bar graph of the horizontal axis, for example, when the bar graph is 100nm, "100nm" represents the particle size range greater than 100nm and less than 200nm, and the height of the bar graph represents the total volume ratio of the particles within the range. Among them, "500nm" represents the total volume ratio of all particles greater than 500nm.
[0252] (2) Thermal analysis
[0253] The content of organic components (components other than silver particles) contained in the silver particle composition obtained in the above manner was measured by thermogravimetric analysis. Specifically, the silver particle composition was heated at a heating rate of 10°C / min in an atmospheric environment using a thermogravimetric measuring device (TG-DTA8122 manufactured by Rigaku), and the content (weight %) of the organic component was determined as the weight reduction rate at 30°C to 500°C. The value obtained by subtracting the content (weight %) of the organic component from 100 (weight %) is shown in Tables 1 and 2 as the content (weight %) of the silver particles.
[0254] (3) Determination of void ratio and bonding strength
[0255] The silver microparticle composition obtained in the above manner was applied in small amounts to a copper plate (20 mm × 25 mm × t1 mm) with silver plated on the surface by manual printing using a metal mask, and a virtual silicon carbide chip (bottom area 3 mm × 3 mm × t0.2 mm, surface film structure Au 200 nm / Ni 200 nm / Ti 200 nm) was stacked thereon. At this time, in order to make the components close together, an external force of about 30 gf was applied, but no more than necessary pressure was applied.
[0256] Then, the laminate was placed in an air-sending constant temperature dryer (FV-630 manufactured by Advantec), and calcined at 70° C. for 40 minutes in an atmospheric environment, and then calcined at 200° C. for 60 minutes. After the air-sending constant temperature dryer was left to be below 150° C., the laminate was taken out, and the porosity (%) was measured using an ultrasonic flaw detector (manufactured by KJTD).
[0257] Then, a bonding strength test was performed using an adhesive strength tester (manufactured by RHESCA). A 100 kgf load cell was used for the bonding strength test. The value obtained by dividing the bonding strength when the dummy chip was peeled off by the bottom area of the chip was used. In addition, the unit of bonding strength is MPa.
[0258] The results are shown in Tables 1 and 2.
[0259] Furthermore, the bonded samples prepared by the above method were cut along the diagonal line of the chip in Example 1, Comparative Example 2, and Comparative Example 4, and the cross sections were observed using a scanning electron beam microscope.
[0260] The results are shown in Figures 25-27 middle.
[0261] like Figures 25-27 As shown in the figure, in Comparative Example 4 ( Fig. 27 ) has many relatively small pores and many particles larger than 100 nm and less than 200 nm. Fig.26 ) produced a large number of relatively large pores.
[0262] On the other hand, in Example 1 ( Fig.25 ) was observed to be sintered silver structure becomes dense, and a sintered silver structure that firmly joins the components was obtained in Example 1. This is also clear from the fact that the porosity of the joined sample confirmed by the ultrasonic flaw detector is suppressed to a low level and the joined sample shows high joining strength.
[0263] In addition, Fig. 27 In the figure, the area A is the sintered silver layer, the upper side of the sintered silver layer is the chip, and the lower side is the copper plate.
[0264]
[0265]
[0266] Industrial Applicability
[0267] The silver microparticle composition according to the embodiment of the present invention can be preferably used as a bonding composition for bonding electronic materials and the like, for example.
Claims
1. A silver microparticle composition comprising silver microparticles, amines and diols, wherein the silver microparticle composition: The average particle size of the silver microparticles is greater than or equal to 40 nm and less than or equal to 100 nm. The volume ratio of the silver particles with a particle size of 100 nm or less to the total volume of the silver particles is 5% or more and 25% or less, The volume ratio of the silver microparticles having a particle diameter exceeding 500 nm to the entire silver microparticles is 10% to 60%.
2. The silver microparticle composition according to claim 1, wherein The volume ratio of the silver microparticles having a particle diameter exceeding 300 nm to the entire silver microparticles is 40% to 90%.
3. The silver microparticle composition according to claim 1 or 2, wherein The amine is one or more amines selected from the group consisting of 3-methoxypropylamine, 3-ethoxypropylamine, 3-propoxypropylamine, 3-butoxypropylamine, 2-ethoxypropylamine, 3-isopropoxypropylamine, 2-methoxy-2-methylpropylamine, hexylamine, heptylamine, octylamine and 2-(2-aminoethoxy)ethanol.
4. The silver microparticle composition according to any one of claims 1 to 3, wherein The diol is one or more diols selected from the group consisting of 1,2-octanediol, 2-methyl-2,4-pentanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, and 3-methyl-1,3-butanediol.
5. The silver microparticle composition according to any one of claims 1 to 4, wherein The content of the silver microparticles is 85 wt % or more and 97 wt % or less.
6. The silver microparticle composition according to any one of claims 1 to 5, wherein At shear speed 5s -1 The measured shear viscosity was 100 Pa·s or more.
Citation Information
Patent Citations
Joining agent for inorganic stock, and joined body of inorganic stock
JP2011094223A
Method and device for detecting connection position of existing pipe