Method for producing carbon fiber bundle composite material, and carbon fiber bundle composite material
By mixing short carbon fibers with epoxy resin molten resin and solidifying, combining epoxy curing agent to form carbon fiber bundle composite materials, the problem of insufficient production efficiency and strength of carbon fiber chopped materials in the prior art is solved, and excellent manufacturing strength is achieved CFRP products.
Patent Information
- Application Number
- CN202380019536.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-11-11
- Filing Date
- 2023-02-24
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to efficiently manufacture prepreg materials for reinforcement materials by shorter cut carbon fibers, and there are insufficient production efficiency and material strength.
By mixing short carbon fibers with molten resin containing epoxy resin components, and mixing epoxy curing agents in the molten resin after solidification, forming a carbon fiber bundle composite material with a plurality of short carbon fibers and an uncured solid epoxy resin composition, using the bundle The surface tension of the chemical liquid forms a carbon fiber bundle, and CFRP products are manufactured by compression molding.
It realizes efficient manufacturing of short carbon fiber bundle composite materials, improves the strength and production efficiency of CFRP products, and is suitable for use as an intermediate material for the molding of CFRP products.
Smart Images

Figure CN119072520A_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to a method for manufacturing a carbon fiber bundle composite material (Carbon-fiber Bundle Composite) and the carbon fiber bundle composite material. Background Art
[0002] Fiber reinforced plastic (CFRP) using carbon fibers as a reinforcing material is a lightweight material with excellent mechanical properties suitable for parts of transportation equipment such as automobiles, ships, railway vehicles, manned aircraft, and unmanned aircraft, and its importance has been increasing in recent years.
[0003] One of the intermediate molding materials used in the manufacture of CFRP products is carbon fiber sheet molding compound (CF-SMC). CF-SMC is formed by cutting a continuous carbon fiber bundle into a chopped carbon fiber bundle, spreading the chopped carbon fiber bundle on a carrier film to form a carbon fiber mat, and impregnating the carbon fiber mat with a thermosetting resin matrix to form a carbon fiber mat (for example, Patent Document 1).
[0004] In general, CFRP molded by CF-SMC using chopped carbon fiber bundles with smaller bundle size shows higher strength. On the other hand, the larger the bundle size of the continuous carbon fiber bundle, the higher the production efficiency. Based on this situation, a technology has been developed to divide a continuous carbon fiber bundle with a large bundle size such as 48K, which is called a large tow, into a bundle (fiber bundle) with a smaller bundle size (Patent Document 2).
[0005] It is proposed to produce carbon fiber reinforced thermoplastics by adding carbon fiber pellets to thermoplastic resins. The carbon fiber pellets are produced by mixing short carbon fibers cut by wet method with a solution or suspension of a sizing agent to form carbon fiber aggregates, pelletizing the aggregates with a disc pelletizer, and drying the aggregates (Patent Document 3).
[0006] It is known that after dispersing short carbon fibers in water, a small amount of chloroform is further added and the mixture is shaken violently, thereby obtaining a needle-shaped self-assembled carbon fiber bundle; in addition, by dissolving polyetherimide in the chloroform in advance, polyetherimide can be supported on the needle-shaped self-assembled carbon fiber bundle (Non-Patent Document 1).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 1-163218
[0010] Patent Document 2: U.S. Patent No. 6385828
[0011] Patent Document 3: Japanese Patent Publication No. 10-503812
[0012] Non-patent literature
[0013] Non-patent literature 1: JRBaxter, GRPalmese, NJAlvarez, Applied Materials Today 20(2020)100786 Summary of the invention
[0014] Problems to be solved by the invention
[0015] One of the objects of the present invention is to provide a novel prepreg material which can be easily manufactured from carbon fibers cut into relatively short lengths, wherein the carbon fibers may be virgin carbon fibers or recycled carbon fibers.
[0016] Another object of the present invention is to provide a novel method for manufacturing a prepreg material using carbon fibers cut shorter for reinforcement.
[0017] In this specification, problems that can be solved by each embodiment of the present invention may be explicitly or implicitly shown.
[0018] Means for solving problems
[0019] According to one embodiment of the present invention, there is provided a method for manufacturing a carbon fiber bundle composite material, comprising: mixing carbon fiber cotton composed of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing an epoxy curing agent into the molten resin.
[0020] According to another aspect of the present invention, there is provided a carbon fiber bundle composite material, which is composed of a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition. In the carbon fiber bundle composite material, the positions of the front ends of the plurality of short carbon fibers are not consistent at each end of the bundle, and the uncured solid epoxy resin composition contains an epoxy curing agent.
[0021] According to another aspect of the present invention, there is provided a carbon fiber bundle composite sheet obtained by mutually fusing a plurality of the carbon fiber bundle composite materials, and a method for producing the same.
[0022] Effects of the Invention
[0023] According to a preferred embodiment of the present invention, there is provided a prepreg material that can be suitably used as an intermediate material when manufacturing a CFRP product by various methods including a compression molding method. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] [ Figure 1 ] Figure 1 This is a conceptual diagram showing an apparatus for producing a carbon fiber bundle composite sheet.
[0025] [ Figure 2 ] Figure 2 This is a photograph showing a carbon fiber composite material having a shape close to a spindle shape.
[0026] [ Figure 3 ] Figure 3 This is a photograph showing a linear carbon fiber bundle composite material.
[0027] [ Figure 4 ] Figure 4 This is a photograph showing a needle-shaped carbon fiber bundle composite material.
[0028] [ Figure 5 ] Figure 5 This is a photograph showing a carbon fiber composite sheet. DETAILED DESCRIPTION
[0029] Embodiments of the present invention will be described in detail below.
[0030] 1. Method for manufacturing carbon fiber bundle composite material
[0031] One embodiment of the present invention relates to a method for producing a carbon fiber bundle composite material (hereinafter sometimes referred to as "CBC").
[0032] The manufacturing method includes: mixing carbon fiber cotton composed of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing an epoxy curing agent into the molten resin.
[0033] Hereinafter, the method for producing CBC according to the embodiment will be described separately into a method using virgin carbon fiber as a starting material and a method using regenerated carbon fiber as a starting material.
[0034] 1.1. Method using virgin carbon fiber as starting material
[0035] The method using virgin carbon fiber as a starting material typically includes the following steps (i) to (iv).
[0036] (i) Short Cutting Process
[0037] (ii) Defibrination process
[0038] (iii) Bundling process
[0039] (iv) Cooling process
[0040] Each step will be described in detail below.
[0041] (i) Short Cutting Process
[0042] In the chopped carbon fiber bundle, a continuous carbon fiber bundle consisting of virgin carbon fibers is cut at predetermined intervals in the fiber direction using, for example, a rotary cutter, thereby forming a chopped carbon fiber bundle.
[0043] The bundle size of the continuous carbon fiber bundle (the number of carbon fiber filaments constituting the bundle) is, for example, 10K or more, and may be 12K or more, 15K or more, 24K or more, 36K or more, 48K or more, or 50K or more. The upper limit of the bundle size is not particularly limited, and is, for example, 100K or less.
[0044] Here, "K" is a symbol representing 1000. For example, 1K means 1000, and 10K means 10000.
[0045] The larger the bundle size of the continuous carbon fiber bundle, the more carbon fiber filaments are contained in one piece of the chopped carbon fiber bundle, and thus the higher the production efficiency of the CBC. In addition, the production cost of the continuous carbon fiber bundle also decreases with the increase of the bundle size. Therefore, the bundle size of the continuous carbon fiber bundle is preferably 24K or more, more preferably 36K or more, and further preferably 48K or more.
[0046] In the case of PAN-based carbon fibers made from polyacrylonitrile fibers, the diameter of the carbon fiber filaments is generally in the range of 5 μm to 15 μm.
[0047] The fiber length of the chopped fiber bundle can be set to the required length of the carbon fibers constituting the CBC to be produced. This is because there is no step of intentionally cutting the carbon fibers after the chopped step.
[0048] The fiber length of the chopped fiber bundle is not limited, for example, it is 3 mm or more, and it can also be 5 mm or more or 10 mm or more. The fiber length of the chopped fiber bundle is not limited, for example, it is 60 mm or less, and it can be 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
[0049] The bundle length of the CBC formed of a plurality of short carbon fibers having the same fiber length, in other words, the dimension in the fiber direction is equal to or greater than the fiber length of the short carbon fibers.
[0050] (ii) Defibrination process
[0051] In the defibration step, the chopped carbon fiber bundle obtained in the chopped step is untied and formed into a cotton-like shape, thereby obtaining carbon fiber cotton.
[0052] The defibration is preferably performed in such a way that all the carbon fibers contained in the chopped carbon fiber bundle are in the form of monofilaments, but this is not essential. That is, the carbon fiber wool obtained in the defibration step may include a thin carbon fiber bundle composed of a small number of filaments, such as less than 100.
[0053] In the defibration step, a general defibrator can be used, and the defibrator used is not limited.
[0054] In one example, only chopped carbon fiber bundles are put into a stirring mixer such as a Henschel mixer and stirred in a dry state, thereby defibration can be performed. This method has the advantage that the cotton-like carbon fibers can be fed into the next bundling step without having to be taken out of the stirring mixer.
[0055] In one example, the chopped carbon fiber bundles may be defibrated by immersing them in an organic solvent such as acetone that can dissolve the sizing agent contained in the chopped carbon fiber bundles and irradiating them with ultrasonic waves. After washing away the sizing agent, cotton-like carbon fibers remain.
[0056] In a preferred example, the carbon fiber wool does not contain carbon fibers having a fiber length of less than 3 mm, or even if it contains carbon fibers, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
[0057] In a more preferred example, the carbon fiber wool does not contain carbon fibers having a fiber length of less than 5 mm, or even if it contains carbon fibers, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
[0058] In a more preferred example, the carbon fiber wool does not contain carbon fibers having a fiber length of less than 10 mm, or even if it contains carbon fibers, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
[0059] (iii) Bundling process
[0060] In the bundling step, the carbon fiber wool obtained in the defibration step is mixed with a bundling liquid. The carbon fiber filaments or thin carbon fiber bundles constituting the carbon fiber wool are aggregated by capillary force based on the surface tension of the bundling liquid to form a carbon fiber bundle containing the bundling liquid.
[0061] As the bundling liquid, a molten resin containing an epoxy resin component is used. The molten resin is equivalent to the melt of the solid resin, but it does not need to be prepared through a process of melting the solid resin. That is, the molten resin in a molten state during preparation can be directly used as the bundling liquid.
[0062] In the present specification, a solid resin refers to a resin that is solid at least at a temperature in the range of 15 to 25° C. (so-called room temperature).
[0063] In this specification, for convenience, a non-crystalline resin or resin composition is considered to be "solid" when it has a viscosity of 100,000 Pa·s or more. In addition, when the temperature of the molten resin is lowered without crystallization and the viscosity increases to 100,000 Pa·s, it is considered to be "solidified".
[0064] The viscosity is a value measured using a rotational viscometer (eg, HAAKE MARS 40 manufactured by Thermo Fisher Scientific) under the following conditions: constant stress mode, stress value 300 Pa, frequency 1.59 Hz, plate diameter 25 mm, plate type parallel plates, and plate gap 0.5 mm.
[0065] The molten resin contains an epoxy resin component, in other words, it means that the epoxy resin is blended into the molten resin.
[0066] When a compound having one or more epoxy groups per molecule is referred to as an epoxy compound, an epoxy resin is generally a mixture containing a plurality of epoxy compounds and has an average of more than one epoxy group per molecule.
[0067] One or more epoxy resins may be blended into the molten resin.
[0068] Examples of the epoxy resin that can be blended with the molten resin include glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type epoxy resins, but are not limited thereto.
[0069] Glycidyl ether epoxy resin is an epoxy resin obtained by the reaction of a compound having a hydroxyl group with epichlorohydrin. Examples of glycidyl ether epoxy resins include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, resorcinol epoxy resin, phenol novolac epoxy resin, trisphenol methane epoxy resin, aryl glycidyl ether epoxy resins including biphenol (biphenyl), benzophenone, fluorene, naphthalene and anthracene, and alicyclic polyol polyglycidyl ether epoxy resins, but are not limited thereto.
[0070] Glycidylamine epoxy resin is an epoxy resin obtained by reacting a compound having an amino group with epichlorohydrin. Examples of the glycidylamine epoxy resin include tetraglycidyldiaminodiphenylmethane epoxy resin, triglycidylaminophenol epoxy resin, triglycidylaminocresol epoxy resin, diglycidylaniline epoxy resin, tetraglycidylmeta-xylylenediamine epoxy resin, but are not limited thereto.
[0071] Examples of the glycidyl ester type epoxy resin include polyglycidyl esters of polyvalent carboxylic acids such as diglycidyl esters of phthalic acid, isophthalic acid, terephthalic acid, tetrahydrophthalic acid, or hexahydrophthalic acid, but are not limited thereto.
[0072] In one example, an epoxy resin containing an oxazolidone ring may be blended into the molten resin. Alternatively, an isocyanate compound may be blended into the molten resin to form an oxazolidone ring.
[0073] Examples of alicyclic epoxy resins include, but are not limited to, epoxy resins obtained by epoxidizing a compound having multiple cycloolefin skeletons using peracetic acid or the like, and epoxy resins obtained by prepolymerizing a difunctional cycloolefin oxide having a polymerizable functional group such as a (meth)acryloyl group or an allyl group.
[0074] The solidification temperature of the molten resin is, for example, in the range of 30°C to 150°C, or may be in the range of 40°C to 100°C.
[0075] The viscosity of the molten resin when used as a bundled liquid is preferably 10 Pa·s or less, more preferably 5 Pa·s or less, and may be 3 Pa·s or less, 2 Pa·s or less, 1 Pa·s or less, etc. There is no particular lower limit for the viscosity, and it may be, for example, 0.01 Pa·s or more, or 0.1 Pa·s or more.
[0076] The shape of the carbon fiber bundle formed by the action of the bundling liquid can be changed according to the viscosity of the bundling liquid. Therefore, the greater the temperature dependence of the viscosity of the molten resin used as the bundling liquid, the stricter the temperature management is required in the bundling process.
[0077] The viscosity is a value measured using a rotational viscometer (e.g., HAAKE MARS 40 manufactured by Thermo Fisher Scientific) under the conditions of constant stress, 300 Pa of stress value, 1.59 Hz of frequency, 25 mm of plate diameter, parallel plate type, and 0.5 mm of plate gap. However, it is not a problem in practice that a viscosity value less than 1 Pa·s can be replaced by a value measured using a B-type rotational viscometer known for its ease of operation.
[0078] The solidification temperature and viscosity of the molten resin when melted can be controlled by the type and content of the epoxy resin blended into the molten resin.
[0079] In a preferred example, the molten resin is a melt of an epoxy resin having a melting point. The epoxy resin having a melting point has a low viscosity in a liquid state and a small temperature dependency, and is therefore easy to use as a beam forming liquid.
[0080] In epoxy resins having a melting point, monomers have a rigid skeleton, and their molecular weights are often 1,000 or less. In addition, the content of oligomers is usually small.
[0081] Whether or not the epoxy resin has a melting point can be easily confirmed by ordinary DSC measurement.
[0082] The amount of the molten resin mixed with the carbon fiber wool may be, for example, 25 to 150 parts by weight relative to 100 parts by weight of the carbon fiber wool. By sufficiently mixing, a plurality of isolated carbon fiber bundles that are not bonded to each other can be formed.
[0083] The number of carbon fiber filaments constituting one carbon fiber bundle may be, for example, 1 to 20K, but is not limited thereto.
[0084] The method of mixing the carbon fiber wool and the molten resin is not limited, but stirring is preferably performed in order to efficiently mix them in a short time.
[0085] The stirring can preferably use a powder stirring mixer known as a Henschel mixer. The stirring mixer can be a type that only has a stirring paddle (stirring blade) or a type that is provided with a chopper. In a stirring mixer with a jacket, the temperature of the stirring tank can be adjusted by flowing a heat medium inside the jacket.
[0086] The stirring tank can be pre-heated before the carbon fiber wool is added, and can be maintained at a temperature at which the viscosity of the molten resin falls within the above-mentioned preferred range.
[0087] The preheating of the carbon fiber wool before being put into the stirring tank can be performed arbitrarily. It is preferred that the carbon fiber wool be heated to a temperature at which the viscosity of the molten resin falls within the above-mentioned preferred range before being put into the stirring tank.
[0088] The molten resin is preferably temperature-controlled before being put into the stirring tank so that the viscosity is within the above-mentioned preferred range. In other examples, the molten resin can also be obtained by heating the solid resin in the stirring tank to melt it. In this case, the molten resin can be temperature-controlled in the stirring tank so that the viscosity is within the above-mentioned preferred range.
[0089] The epoxy curing agent is mixed into the molten resin. The timing of mixing the epoxy curing agent into the molten resin is preferably before mixing the molten resin with the carbon fiber wool, or simultaneously with mixing the molten resin with the carbon fiber wool.
[0090] The epoxy curing agent that is liquid at the temperature at which the molten resin and the carbon fiber wool are mixed is preferably mixed into the molten resin before the molten resin and the carbon fiber wool are mixed.
[0091] The epoxy curing agent that is solid at the temperature at which the molten resin and the carbon fiber wool are mixed is preferably mixed into the molten resin before or while the molten resin and the carbon fiber wool are mixed.
[0092] When the epoxy resin is mixed into the molten resin while the molten resin is mixed with the carbon fiber wool, it is preferred to first mix the carbon fiber wool and the epoxy curing agent, and then add the molten resin to the obtained mixture and further mix.
[0093] When two or more epoxy curing agents are used, all of them may be mixed with the molten resin at the same time, or one part and the other part may be mixed with the molten resin at different times.
[0094] The epoxy curing agent to be mixed with the molten resin can be selected from common epoxy curing agents such as dicyandiamide, phenols including novolac, amines, carboxylic anhydrides, thiols, and imidazoles.
[0095] When the epoxy curing agent is not mixed, the viscosity of the molten resin decreases as the temperature rises. When the epoxy curing agent is mixed, the same tendency is shown before the curing reaction starts due to the action of the epoxy curing agent, but once the curing reaction starts, the viscosity of the molten resin increases sharply. Therefore, when the epoxy curing agent mixed in the molten resin is mixed with the molten resin heated to a viscosity that is reduced to a level that can be used as a bundled liquid, the curing reaction must not start immediately after mixing.
[0096] It can be seen from this that when the solidification temperature of the molten resin is low, the selection range of the epoxy curing agent that can be used is widened. From this viewpoint, the solidification temperature of the molten resin is preferably below 120°C, more preferably below 100°C, further preferably below 90°C, and may also be below 80°C, below 70°C or below 60°C.
[0097] The epoxy curing agent that can be preferably used is called a latent curing agent, and has the following properties: it is a solid with low solubility in epoxy resin at room temperature, but when heated to a specified temperature, it melts or dissolves in the epoxy resin and exhibits a function as a curing agent. The specified temperature varies depending on the type of latent curing agent. Among the latent curing agents, there are latent curing agents with a melting point of 100°C or more, further 150°C, and further 200°C or more, which are epoxy curing agents that can be particularly preferably used in the manufacturing method of the embodiment.
[0098] Various imidazoles, dicyandiamide and boron trifluoride-amine complexes are typical examples of latent curing agents.
[0099] Imidazoles refer to compounds having an imidazole ring, and include substituted imidazoles in which the hydrogen atom of imidazole is substituted with a substituent, imidazolium salts, imidazole complexes, and the like.
[0100] Preferred examples of substituted imidazoles include substituted imidazoles having an aromatic ring which may be a heteroaromatic ring in the molecule, such as 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-p-tolyl-4-methyl-5-hydroxymethylimidazole, 2-p-tolyl-4,5-dihydroxymethylimidazole, 2-m-tolyl-4-methyl-5-hydroxymethylimidazole, 2-m-tolyl-4,5-dihydroxymethylimidazole and 1-cyanoethyl-2-phenylimidazole.
[0101] Imidazolium salts such as 1-cyanoethyl-2-ethyl-4-methylimidazolium trimellitate, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimellitate are also preferred examples of the imidazole-based latent curing agent.
[0102] Isocyanuric acid adducts of various substituted imidazoles such as 2-phenylimidazole, 2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole and 2-phenyl-4-methyl-5-hydroxymethylimidazole, in particular, isocyanuric acid adducts of substituted imidazoles having a triazine ring such as 2,4-diamino-6-(2'-methylimidazolyl-(1'))-ethyl-s-triazine, 1-(4,6-diamino-s-triazine-2-yl)ethyl-2-undecylimidazole and 2,4-diamino-6-[2-(2-ethyl-4-methyl-1-imidazolyl)ethyl]-s-triazine are particularly preferred imidazole-based latent curing agents.
[0103] Amine adducts are also one of the preferred examples of latent curing agents. Amine adducts are obtained by reacting imidazole and / or tertiary amine with epoxy resin and / or isocyanate to increase the molecular weight, and have low solubility in epoxy resin.
[0104] The latent curing agent mixed in the molten resin may be one kind or two or more kinds.
[0105] In one example, a curing accelerator may be mixed with the epoxy curing agent in the molten resin.
[0106] When dicyandiamide is used as the epoxy curing agent, examples of the curing accelerator that can be preferably used together include urea derivatives such as 4,4′-methylenebis(phenyldimethylurea) and 2,4-bis(3,3-dimethylureido)toluene.
[0107] In addition to the epoxy curing agent, various additives such as low shrinkage agent, antioxidant, internal mold release agent, colorant, modifier (such as rubber, elastomer or thermoplastic resin), flame retardant, antibacterial agent, etc. can be mixed into the molten resin as needed.
[0108] As in the case of the epoxy curing agent, an additive that is liquid at the temperature when the molten resin and the carbon fiber wool are mixed is preferably mixed into the molten resin before the molten resin and the carbon fiber wool are mixed. In addition, an additive that is solid at the temperature when the molten resin and the carbon fiber wool are mixed may be mixed with the molten resin before the molten resin and the carbon fiber wool are mixed, or may be mixed into the molten resin while the molten resin and the carbon fiber wool are mixed.
[0109] The flame retardant that can be mixed with the molten resin is described below.
[0110] As a preferable flame retardant, a phosphorus-containing flame retardant is mentioned.
[0111] Examples of the phosphorus-containing flame retardant include non-halogen phosphates such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, triphenyl phosphate, tricresyl phosphate, cresyl diphenyl phosphate, octyl diphenyl phosphate, and aromatic polyphosphates.
[0112] Other examples of phosphorus-containing flame retardants include tris(chloroethyl)phosphate, tris(dichloropropyl)phosphate, tris(chloropropyl)phosphate, bis(2,3-dibromopropyl)2,3-dichloropropyl phosphate, tris(2,3-dibromopropyl)phosphate, bis(chloropropyl)octyl phosphate, halogenated alkyl polyphosphates, and halogenated alkyl polyphosphates.
[0113] As another example of phosphorus-containing flame retardants, metal salts of phosphinates can be cited. The metal salts of phosphinates mentioned here include not only metal salts of phosphinates without organic groups, but also metal salts of organic phosphinates such as diphenylphosphinates, monophenylphosphinates, dialkylphosphinates, monoalkylphosphinates, and alkylphenylphosphinates, and metal salts of diphosphinates such as methane (dimethylphosphinates) and benzene-1,4-di (methylphosphinates).
[0114] Examples of the dialkylphosphinic acid include dimethylphosphinic acid, ethylmethylphosphinic acid, diethylphosphinic acid, and methyl-n-propylphosphinic acid.
[0115] Examples of the monoalkylphosphinic acid include methylphosphinic acid, ethylphosphinic acid, and n-propylphosphinic acid.
[0116] As an example of the alkylphenylphosphinic acid, methylphenylphosphinic acid can be mentioned.
[0117] The metal salt of phosphinate may be aluminum salt, zinc salt, calcium salt, magnesium salt, etc., but is not limited thereto.
[0118] Other examples of the phosphorus-containing flame retardant include red phosphorus, ammonium polyphosphate, melamine phosphate, guanidine phosphate, and guanidine urea phosphate.
[0119] In addition to the phosphorus-containing flame retardant, a non-phosphorus-containing flame retardant may be mixed in the molten resin.
[0120] Examples of phosphorus-free flame retardants include melamine compounds such as melamine cyanurate, triazine compounds, guanidine compounds, nitrogen flame retardants such as ammonium phosphate and ammonium carbonate, hydrated metal compounds such as aluminum hydroxide and magnesium hydroxide, and organic metal salt flame retardants such as ferrocene and acetylacetone metal complexes.
[0121] In a preferred example, by selecting a material containing a flame retardant and containing no halogen in the molten resin and all materials mixed in the molten resin, the CBC as a final product can be made flame retardant and halogen-free.
[0122] The weight ratio of carbon fiber wool to the total weight of molten resin, all materials mixed in the molten resin, and carbon fiber wool can be 20% or more and less than 30%, 30% or more and less than 40%, 40% or more and less than 50%, 50% or more and less than 60%, 60% or more and less than 70%, or 70% or more and less than 80%. This ratio is roughly equal to the fiber weight content in CBC as the final product. In fact, since the carbon fiber wool composed of virgin carbon fiber contains a sizing agent, the value obtained by multiplying the weight ratio of the carbon fiber in the carbon fiber wool by the above ratio becomes the fiber weight content of CBC.
[0123] (iv) Cooling process
[0124] In the cooling step, the carbon fiber bundle formed in the bundling step is cooled to solidify the molten resin contained in the carbon fiber bundle as a bundling liquid, thereby completing the CBC. The cooling may be forced cooling or natural cooling.
[0125] In one example, the carbon fiber bundle formed in the stirring tank of the stirring mixer may be cooled while being stirred in the stirring tank without being taken out from the stirring tank.
[0126] In another example, the carbon fiber bundle formed in the stirring tank of the stirring mixer may be taken out from the stirring tank and cooled in another place, such as a disc pelletizer, a conveying pipe, or a conveyor belt.
[0127] The temperature of the final CBC is usually reduced to below room temperature.
[0128] The carbon fiber bundle is unstable at the stage before the contained molten resin solidifies. When a large number of carbon fiber bundles at this stage are stored in a large container, the carbon fibers may adhere to each other due to their own weight near the bottom of the container.
[0129] The higher the solidification temperature of the molten resin, the earlier the solidification of the molten resin in the cooling process occurs. Therefore, the higher the solidification temperature of the molten resin, the faster the carbon fiber bundle becomes a stable state. From this point of view, the solidification temperature of the molten resin is preferably 40°C or more, more preferably 50°C or more, and may also be 60°C or more, 70°C or more, or 80°C or more.
[0130] 1.2. Method using recycled carbon fiber as starting material
[0131] In the method for producing CBC described in 1.1. above, all or part of the virgin carbon fibers as the starting material may be replaced with recycled carbon fibers.
[0132] Preferred examples of recycled carbon fibers are carbon fibers recovered from scraps of SMC (sheet molding compound) or waste CFRP obtained by curing SMC. Carbon fibers contained in SMC have substantially all the same fiber length, which is generally in the range of 3 mm to 60 mm.
[0133] For example, when the scraps or waste are dry-distilled at a temperature preferably above 600°C, and then heated to, for example, 550°C or above, preferably 600°C or above in an oxidizing atmosphere, so that the matrix resin is completely thermally decomposed, the carbon fibers consisting of regenerated carbon fibers having almost all the same fiber lengths become cotton-like and remain. The regenerated carbon fibers are thermally degraded and have a lower strength than virgin carbon fibers, but have sufficient strength when used as a reinforcing material for FRP.
[0134] As another method for recovering carbon fibers from CFRP waste, there is a method of decomposing the matrix resin using a subcritical fluid or a supercritical fluid. In order to obtain cotton-like regenerated carbon fibers, the matrix resin is completely removed. The resin residue that is not completely removed can be removed by heat treatment in an oxidizing atmosphere. The regenerated carbon fibers obtained by this method also undergo thermal degradation, so they are lower in strength than virgin carbon fibers.
[0135] As another method for recovering carbon fibers from CFRP waste, a method of decomposing the matrix resin by microwave heating can also be used.
[0136] In the regenerated carbon fiber bundle taken out from the waste of SMC and CFRP by thermally decomposing the matrix resin, a small amount of carbon as a thermal decomposition product of the matrix resin may remain. The carbon fiber bundle in which the carbon fiber filaments are mutually bonded by a small amount of residual carbon can be defibrated by stirring in a dry state, for example, using a stirring mixer.
[0137] As another method for recovering carbon fiber from SMC scraps, there is a method of washing out the uncured matrix resin using a solvent that can be a subcritical fluid or a supercritical fluid. According to this method, it is possible to obtain regenerated carbon fiber having the same strength as virgin carbon fiber and without thermal degradation.
[0138] The regenerated carbon fiber recovered from the CFRP or SMC scraps obtained by solidifying SMC by the above method is generally a short fiber having a fiber length in the range of 3 mm to 60 mm, and does not need to be further cut when used in the manufacture of CBC, and the sizing agent is also removed. When only such regenerated carbon fiber is used as the starting material, after the (ii) defibration step is performed as needed, the aforementioned (iii) bundling step and (iv) cooling step can be performed in the same manner as when the virgin carbon fiber is used as the starting material.
[0139] The scraps of UD prepreg (Uni-Directional prepreg) or fabric prepreg, and the waste of CFRP obtained by curing UD prepreg or fabric prepreg are cut in such a way that the carbon fibers contained therein have a length within the range of 3 mm to 60 mm, and the recycled carbon fibers are recovered by performing the above-exemplified treatment, which can also be preferably used in the method for manufacturing CBC of the embodiment.
[0140] Sometimes fibers other than carbon fibers are mixed into the carbon fiber wool obtained by recycling. For example, mixing of glass fibers can be confirmed in carbon fiber wool recovered from CFRP, which uses a carbon fiber cloth including a coil composed of glass fibers as a reinforcement material.
[0141] When using regenerated carbon fiber as the starting material, it can be used after removing the fibers other than the carbon fiber mixed in, but it is not essential. That is, in the manufacturing method of the embodiment, carbon fiber wool mixed with fibers other than the carbon fiber can also be used as the starting material.
[0142] For example, from the viewpoint of reducing the load on the environment, carbon fiber wool mixed with glass fibers is preferably used in a state containing glass fibers unless there is a practical problem.
[0143] On the other hand, from the viewpoint of stabilizing the quality of CBC, the content of fibers other than carbon fibers in the carbon fiber cotton as a starting material is preferably less than 10 wt %, more preferably less than 5 wt %, and further preferably less than 1 wt %.
[0144] 2. Carbon fiber bundle composite materials
[0145] Another embodiment of the present invention is a CBC produced by the production method described in the above Item 1. The CBC is composed of a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition.
[0146] Due to the process of aggregating the short carbon fibers into a bundle under the action of a bundling liquid, the positions of the front ends of the plurality of short carbon fibers at each end of the bundle are inconsistent. The uncured solid epoxy resin composition contains an epoxy curing agent.
[0147] The number of short carbon fibers (filaments) forming the bundle may be, for example, 1000 to 20000. All short carbon fibers forming the bundle may have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
[0148] Carbon fibers with too short a fiber length have low effect as a reinforcing material when used for FRP, and therefore most of the short carbon fibers forming the bundle preferably have a fiber length of 3 mm or more, more preferably 5 mm or more, and even more preferably 10 mm or more.
[0149] In order to improve the strength of CFRP molded using CBC, it is effective to limit the content of carbon fibers less than a certain length.
[0150] In a preferred example, the CBC does not contain carbon fibers having a fiber length of less than 3 mm, or even if it contains carbon fibers having a fiber length of less than 3 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the CBC.
[0151] In a more preferred example, the CBC does not contain carbon fibers having a fiber length of less than 5 mm, or even if it contains carbon fibers having a fiber length of less than 5 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the CBC.
[0152] In a more preferred example, the CBC does not contain carbon fibers having a fiber length of less than 10 mm, or even if it contains carbon fibers having a fiber length of less than 10 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the CBC.
[0153] In the case of a CBC in which the short carbon fibers forming the bundle all have the same fiber length L (mm), the bundle length generally exceeds L (mm).
[0154] Depending on the bundle length and the length and number of short carbon fibers contained, the shape of the CBC can be spindle-shaped, needle-shaped or wire-shaped.
[0155] In the CBC of the embodiment, by being composed only of short carbon fibers having the same fiber length, it is possible to suppress quality variations between production lots. In this case, the difference between the maximum and minimum fiber lengths of the short carbon fibers forming the bundle is preferably within 5 mm, more preferably within 4 mm, and further preferably within 3 mm.
[0156] The filament diameter of the short carbon fibers forming the bundle is not particularly limited, and may be, for example, within the range of filament diameters generally possessed by PAN-based carbon fibers, for example, within the range of 5 μm to 15 μm.
[0157] The uncured solid epoxy resin composition contained in the CBC of the embodiment may contain one or more epoxy resins. Examples of epoxy resins that may be contained include, but are not limited to, glycidyl ether type, glycidyl amine type, glycidyl ester type, and alicyclic type epoxy resins.
[0158] The uncured solid epoxy resin composition may also contain an epoxy resin having an oxazolidone ring.
[0159] The uncured solid epoxy resin composition contained in the CBC of the embodiment is formed by solidifying the molten resin used as the bundle forming liquid when manufacturing the CBC, so the epoxy resin that can be contained in the solid epoxy resin composition is the same as the epoxy resin that can be mixed in the molten resin. For the same reason, the components other than the epoxy resin that can be contained in the solid epoxy resin composition are the same as the various components other than the epoxy resin that can be mixed in the molten resin.
[0160] The uncured solid epoxy resin composition contained in the CBC of the embodiment is solid at least at a temperature in the range of 15 to 25°C (so-called room temperature), preferably at 40°C, and more preferably at 50°C.
[0161] The fiber weight content in the CBC of the embodiment may be 40 wt % or more and less than 50 wt %, 50 wt % or more and less than 60 wt %, 60 wt % or more and less than 70 wt %, or 70 wt % or more and 80 wt % or less.
[0162] The carbon fibers contained in the CBC of the embodiment may be all carbon fibers that have not been thermally degraded, may be carbon fibers that have partially not been thermally degraded and the remainder that have been thermally degraded, or may be carbon fibers that have entirely been thermally degraded.
[0163] A typical example of carbon fiber that is not thermally degraded is virgin carbon fiber.
[0164] A typical example of thermally degraded carbon fibers is recycled carbon fibers recovered from CFRP waste, and thermal degradation occurs during the process of thermally decomposing and removing the matrix resin.
[0165] In the CBC of the embodiment, fibers other than carbon fibers may be mixed into the bundle consisting of a plurality of short carbon fibers. Such a CBC is obtained, for example, when regenerated carbon fibers are used as the starting material. When regenerated carbon fibers mixed with glass fibers are used as the starting material, a CBC consisting of a plurality of short carbon fibers bundled together with the glass fibers and an uncured solid epoxy resin composition can be obtained.
[0166] When the fiber bundles contained in the CBC include fibers other than carbon fibers, the content thereof is preferably less than 10 wt %, more preferably less than 5 wt %, and further preferably less than 1 wt %.
[0167] The CBC of the embodiment is a prepreg material for molding CFRP. As a molding method when using the CBC of the embodiment to manufacture a CFRP product, a press molding method can be preferably exemplified, but is not limited. For example, a molding method other than the press molding method such as an autoclave molding method can also be used.
[0168] 3. Carbon fiber bundle composite sheet
[0169] Using the CBC of the embodiment, for example, the following first to third steps are sequentially performed to produce a CBC sheet as a sheet-shaped thermosetting molding material.
[0170] Step 1: Prepare the first protective film and the second protective film.
[0171] Step 2: Spread CBC on the first protective film to make the CBC layer accumulate.
[0172] Step 3: After covering the CBC layer with the second protective film, the CBC layer is heated and pressed by a double belt press or a roller press, thereby fusing the CBCs to each other to form a sheet.
[0173] As the first protective film and the second protective film, release paper generally used in the production of carbon fiber prepreg can be preferably used.
[0174] When the CBC layer is heated and pressurized in the third step, the temperature is adjusted so that the solid epoxy resin composition contained in the CBC does not solidify and lose fluidity.
[0175] Figure 1 : is a conceptual diagram of a manufacturing apparatus that can be used to manufacture a CBC sheet through the above steps.
[0176] The manufacturing apparatus includes: a section for spreading CBC on a first protective film rolled out from a roll to deposit a CBC layer; a section for covering the CBC layer with a second protective film rolled out from a roll; a section for heating and pressurizing the CBC layer; and a section for winding a CBC sheet.
[0177] The orientation of CBC in the CBC layer can be random or biased in one direction. For example, the lower the travel speed of the first protective film, the closer the orientation of CBC is to random. If the travel speed of the first protective film is increased, the CBC tends to be oriented along its travel direction.
[0178] In one example, the fiber weight content of the CBC sheet can be adjusted by adding uncured epoxy resin when manufacturing the CBC sheet. Therefore, before depositing the CBC layer, the surface of the first protective film may be coated with the uncured epoxy resin to be added. Alternatively or in addition, the surface of the second protective film may be coated with the uncured epoxy resin to be added before covering the CBC layer.
[0179] The weight per unit area of the CBC sheet can be appropriately designed according to the application. The weight per unit area can be, for example, 300 g / m 2 Above and less than 500g / m 2 , 500g / m 2 Above and less than 1000g / m 2 1000g / m 2 Above and less than 2000g / m 2 , 2000g / m 2 Above and less than 4000g / m 2 , 4000g / m 2 Above and less than 6000g / m 2 , 6000g / m 2 Above and less than 8000g / m 2 , or 8000g / m 2 Above and less than 10000g / m 2 .
[0180] The thickness of the CBC sheet may be designed to be, for example, 0.5 mm or more and less than 1.5 mm, 1.5 mm or more and less than 3 mm, or 3 mm or more and 5 mm or less, but is not limited thereto.
[0181] The CBC sheet of the embodiment is a prepreg material for molding CFRP. As a molding method when using the CBC sheet of the embodiment to manufacture a CFRP product, a press molding method can be preferably exemplified, but it is not limited thereto, and a molding method other than the press molding method such as an autoclave molding method can also be used.
[0182] 4. Summary of implementation methods
[0183] Embodiments of the present invention include, but are not limited to, the following embodiments.
[0184] [Implementation 1] A method for manufacturing a carbon fiber bundle composite material, comprising: mixing carbon fiber cotton composed of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing at least one epoxy curing agent into the molten resin.
[0185] [Embodiment 2] The manufacturing method according to Embodiment 1, wherein the mixing uses a stirring mixer.
[0186] [Embodiment 3] The manufacturing method according to Embodiment 1 or 2, wherein the molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a disc pelletizer.
[0187] [Embodiment 4] The manufacturing method according to Embodiment 1 or 2, wherein the molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a conveying pipe or on a conveyor belt.
[0188] [Implementation 5] A manufacturing method according to any one of implementations 1 to 4, wherein at least a portion of the at least one epoxy curing agent is mixed into the molten resin before the molten resin is mixed with the carbon fiber wool, or while the molten resin is mixed with the carbon fiber wool.
[0189] [Embodiment 6] The manufacturing method according to any one of Embodiments 1 to 5, wherein the molten resin is a melt of a resin that is solid at a temperature in the range of at least 15 to 25°C.
[0190] [Embodiment 7] The production method according to any one of Embodiments 1 to 6, wherein the molten resin is a melt of a resin that is solid at 40°C.
[0191] [Embodiment 8] The production method according to any one of Embodiments 1 to 7, wherein a flame retardant is mixed into the molten resin.
[0192] [Implementation 9] A manufacturing method according to any one of implementations 1 to 8, wherein all carbon fibers contained in the carbon fiber cotton have a fiber length of less than 60 mm, less than 50 mm, less than 40 mm, less than 30 mm, or less than 20 mm.
[0193] [Implementation 10] A manufacturing method according to any one of implementations 1 to 9, wherein the carbon fiber cotton does not contain carbon fibers with a fiber length less than 3 mm, or even if it contains carbon fibers with a fiber length less than 3 mm, the amount thereof is less than 5wt% of all carbon fibers contained in the carbon fiber cotton.
[0194] [Implementation 11] A manufacturing method according to any one of implementations 1 to 9, wherein the carbon fiber cotton does not contain carbon fibers with a fiber length less than 5 mm, or even if it contains carbon fibers with a fiber length less than 5 mm, the amount thereof is less than 5wt% of all carbon fibers contained in the carbon fiber cotton.
[0195] [Implementation 12] A manufacturing method according to any one of implementations 1 to 9, wherein the carbon fiber cotton does not contain carbon fibers with a fiber length less than 10 mm, or even if it contains carbon fibers with a fiber length less than 10 mm, the amount thereof is less than 5wt% of all carbon fibers contained in the carbon fiber cotton.
[0196] [Embodiment 13] A manufacturing method according to any one of Embodiments 1 to 12, wherein a portion of the carbon fibers contained in the carbon fiber cotton is provided by defibration of a chopped carbon fiber bundle.
[0197] [Implementation 14] A manufacturing method according to any one of implementations 1 to 8, wherein all the carbon fibers contained in the carbon fiber cotton are provided by defibration of chopped carbon fiber bundles.
[0198] [Implementation 15] According to the manufacturing method described in implementation 14, the fiber length of the chopped carbon fiber bundle is greater than 3 mm, greater than 5 mm, or greater than 10 mm.
[0199] [Implementation 16] The manufacturing method according to implementation 14 or 15, wherein the fiber length of the chopped carbon fiber bundle is 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
[0200] [Embodiment 17] A manufacturing method according to any one of Embodiments 1 to 16, wherein all of the short carbon fibers are carbon fibers that have not undergone thermal degradation.
[0201] [Embodiment 18] A manufacturing method according to any one of Embodiments 1 to 13, wherein the short carbon fibers include thermally degraded carbon fibers.
[0202] [Implementation 19] A manufacturing method according to any one of implementations 1 to 13 and 18, wherein fibers other than carbon fibers are mixed into the carbon fiber cotton, and the fibers other than carbon fibers may be glass fibers.
[0203] [Implementation 20] A manufacturing method according to any one of implementations 1 to 19, wherein the carbon fiber bundle containing the molten resin is an isolated fiber bundle.
[0204] [Embodiment 21] A carbon fiber bundle composite material produced by the production method described in any one of Embodiments 1 to 20.
[0205] [Embodiment 22] A carbon fiber bundle composite material, which is composed of a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition, wherein the positions of the front ends of the plurality of short carbon fibers are inconsistent at each end of the bundle, and the uncured solid epoxy resin composition contains at least one epoxy curing agent.
[0206] [Embodiment 23] The carbon fiber bundle composite material according to Embodiment 22, wherein the uncured solid epoxy resin composition is solid at least at a temperature in the range of 15 to 25°C.
[0207] [Embodiment 24] The carbon fiber bundle composite material according to Embodiment 22, wherein the uncured solid epoxy resin composition is solid at 40°C.
[0208] [Embodiment 25] A carbon fiber bundle composite material according to any one of Embodiments 22 to 24, wherein the bundle is isolated.
[0209] [Embodiment 26] The carbon fiber bundle composite material according to Embodiment 25 has a needle-like or linear shape.
[0210] [Implementation 27] A carbon fiber bundle composite material according to any one of implementations 22 to 26, wherein all of the plurality of short carbon fibers have a fiber length of less than 60 mm, less than 50 mm, less than 40 mm, less than 30 mm, or less than 20 mm.
[0211] [Embodiment 28] The carbon fiber bundle composite material according to any one of Embodiments 22 to 27, which has a bundle length of 3 mm or more, 5 mm or more, or 10 mm or more.
[0212] [Implementation 29] According to any one of implementations 22 to 28, the carbon fiber bundle composite material does not contain carbon fibers with a fiber length less than 3 mm, or even if it contains carbon fibers with a fiber length less than 3 mm, the amount is less than 5wt% of all the carbon fibers in the carbon fiber bundle composite material.
[0213] [Implementation 30] According to any one of implementations 22 to 27, the carbon fiber bundle composite material has a bundle length of 5 mm or more or 10 mm or more, does not contain carbon fibers with a fiber length less than 5 mm, or even if it contains carbon fibers with a fiber length less than 5 mm, the amount is less than 5wt% of all carbon fibers in the carbon fiber bundle composite material.
[0214] [Implementation 31] According to any one of implementations 22 to 27, the carbon fiber bundle composite material has a bundle length of more than 10 mm, does not contain carbon fibers with a fiber length less than 10 mm, or even if it contains carbon fibers with a fiber length less than 10 mm, the amount is less than 5wt% of all carbon fibers in the carbon fiber bundle composite material.
[0215] [Embodiment 32] A carbon fiber bundle composite material according to any one of Embodiments 22 to 31, wherein the difference between the maximum and minimum fiber lengths of the plurality of short carbon fibers is within 5 mm.
[0216] [Embodiment 33] The carbon fiber bundle composite material according to Embodiment 25 has a spindle shape.
[0217] [Embodiment 34] A carbon fiber bundle composite material according to any one of Embodiments 22 to 33, wherein the at least one epoxy curing agent contains a latent curing agent.
[0218] [Implementation 35] A carbon fiber bundle composite material according to any one of implementations 22 to 34, wherein the fiber weight content is greater than 40 wt% and less than 50 wt%, greater than 50 wt% and less than 60 wt%, greater than 60 wt% and less than 70 wt%, or greater than 70 wt% and less than 80 wt%.
[0219] [Embodiment 36] A carbon fiber bundle composite material according to any one of Embodiments 22 to 35, wherein all of the plurality of short carbon fibers are carbon fibers that have not undergone thermal degradation.
[0220] [Embodiment 37] A carbon fiber bundle composite material according to any one of Embodiments 22 to 35, wherein the plurality of short carbon fibers include thermally degraded carbon fibers.
[0221] [Embodiment 38] A carbon fiber bundle composite material according to any one of Embodiments 22 to 35 and 37, wherein the plurality of short carbon fibers form the bundle together with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers.
[0222] [Embodiment 39] A carbon fiber bundle composite sheet is formed by mutually fusing a plurality of carbon fiber bundle composite materials according to any one of Embodiments 21 to 38.
[0223] [Implementation 40] A carbon fiber bundle composite sheet, comprising a plurality of carbon fiber composite materials described in any one of implementations 21 to 38, wherein the carbon fiber bundle composite materials are respectively welded to at least one other carbon fiber bundle composite material.
[0224] [Implementation 41] A method for manufacturing a carbon fiber bundle composite sheet comprises: welding the carbon fiber bundle composite materials described in any one of a plurality of implementations 21 to 38 to each other.
[0225] [Embodiment 42] A manufacturing method according to embodiment 41, wherein uncured epoxy resin is added to the carbon fiber bundle composite material during the welding.
[0226] [Embodiment 43] A manufacturing method according to any one of Embodiments 1 to 20, wherein the molten resin is a melt of an epoxy resin having a melting point.
[0227] [Implementation 44] A carbon fiber bundle composite material is manufactured by the manufacturing method described in Implementation 43.
[0228] [Embodiment 45] A carbon fiber bundle composite material according to any one of Embodiments 22 to 38, wherein the uncured solid epoxy resin composition has a melting point.
[0229] [Embodiment 46] A carbon fiber bundle composite sheet, which is formed by welding a plurality of carbon fiber bundle composite materials described in Embodiment 45 to each other.
[0230] [Implementation 47] A carbon fiber bundle composite sheet, which comprises a plurality of carbon fiber composite materials described in Implementation 45, wherein the carbon fiber bundle composite materials are respectively welded to at least one other carbon fiber bundle composite material.
[0231] [Implementation 48] A method for manufacturing a carbon fiber bundle composite sheet, comprising: welding a plurality of carbon fiber bundle composite materials described in Implementation 45 to each other.
[0232] [Implementation 49] A manufacturing method according to implementation 48, wherein uncured epoxy resin is added to the carbon fiber bundle composite material during the welding.
[0233] 5. Experimental Results
[0234] The results of experiments conducted by the present inventors are described below.
[0235] The materials used in each experiment are as follows.
[0236] Carbon fiber: Used were cotton-like carbon fibers obtained by drying short carbon fibers with a fiber length of 6 mm sized with water at 120° C. for 1 hour and then unraveling them by hand.
[0237] Epoxy resin: YX4000 produced by Mitsubishi Chemical Corporation, which is a biphenyl type epoxy resin having a nominal melting point of 105° C. The viscosity of the epoxy resin at 120° C. was measured using a B-type rotational viscometer (Brookfield LVDV-1, spindle S61, 50 rpm) and found to be 0.048 Pa·s.
[0238] Epoxy curing agent: Powdered epoxy curing agent DICY7 produced by Mitsubishi Chemical Corporation was used. Dicyandiamide, which is a component of the epoxy curing agent, has a melting point of about 210°C.
[0239] [Experiment 1]
[0240] 10 g of epoxy resin powder and 0.3 g of epoxy curing agent were placed in a container (polypropylene bottle with a cap) and mixed, and then the container was kept in a constant temperature bath at 120° C. for 10 minutes to obtain a molten epoxy resin in which the epoxy curing agent was dispersed. 23 g of carbon fiber was immediately placed in the container taken out of the constant temperature bath, and then the container was shaken by hand to mix the molten epoxy resin with the carbon fiber.
[0241] After the temperature of the container dropped during the shaking and the epoxy resin solidified, the container was placed in a 120°C thermostat again and kept for 10 minutes to melt the epoxy resin. The container was shaken outside the thermostat until the epoxy resin solidified again. This operation was repeated 4 times, and the cotton-like carbon fiber was mixed with the epoxy resin without any residue. Figure 2 As shown, a carbon fiber bundle composite material having a shape close to a spindle shape was obtained. The length of the carbon fiber bundle composite material was generally in the range of 1 to 3 cm.
[0242] [Experiment 2]
[0243] Except that the amount of carbon fiber was changed from 23 g to 10 g, the molten epoxy resin in which the epoxy curing agent was dispersed was mixed with the carbon fiber in the same manner as in Experiment 1. The operation repeated 4 times in Experiment 1 was repeated 2 times, and as a result, the cotton-like carbon fiber was mixed with the epoxy resin without any residue, as shown in FIG. Figure 3 As shown, a linear carbon fiber bundle composite material was obtained. The length of the carbon fiber bundle composite material was generally in the range of 4 to 10 cm.
[0244] [Experiment 3]
[0245] Except that the amount of carbon fiber was changed from 23 g to 30 g, the molten epoxy resin in which the epoxy curing agent was dispersed was mixed with the carbon fiber in the same manner as in Experiment 1. The operation repeated 4 times in Experiment 1 was repeated 10 times, and as a result, the cotton-like carbon fiber was mixed with the epoxy resin without any residue, as shown in FIG. Figure 4 As shown, a needle-shaped carbon fiber bundle composite material was obtained. The length of the carbon fiber bundle composite material was approximately in the range of 1 to 2 cm.
[0246] [Experiment 4]
[0247] Using a pressing mold consisting of a cavity and a core, pressing was performed at a temperature of 120°C and a pressure of 8 MPa for 10 minutes, thereby forming a carbon fiber bundle composite sheet with a length and width of 100 mm×60 mm and a thickness of 1.8 mm from the spindle-shaped carbon fiber bundle composite material 15g obtained in Experiment 1.
[0248] The appearance of the obtained carbon fiber bundle composite sheet is shown in Figure 5 The carbon fiber bundle composite sheet had softness just after being taken out of the pressing mold at a temperature of 120° C., but lost its softness when the temperature dropped to room temperature.
[0249] [Experiment 5]
[0250] The carbon fiber bundle composite sheet obtained in Experiment 4 was sandwiched between two metal flat plates and pressed at a temperature of 180° C. and a pressure of 8 MPa for 120 minutes to form a CFRP plate.
[0251] The obtained CFRP plate had a length and width of 105 mm×70 mm and a thickness of 1.5 mm. This indicates that the carbon fiber composite sheet was slightly fluidized during molding.
[0252] The CFRP plate did not soften even when heated to 120° C., indicating that the epoxy resin contained in the CFRP plate was cured.
[0253] The present invention has been described above based on specific embodiments, but each embodiment is proposed as an example and does not limit the scope of the present invention. Each embodiment described in this specification can be variously modified within the scope of the invention effect, and can be combined with the features described in other embodiments within the scope of implementation.
[0254] This application is based on Japanese Patent Application No. 2022-33126 filed on March 4, 2022 and Japanese Patent Application No. 2022-180699 filed on November 11, 2022, the entireties of which are incorporated herein by reference.
[0255] Industrial Applicability
[0256] The CBC and CBC sheets of the embodiments can be preferably used to manufacture various CFRP parts used in transportation equipment such as automobiles, motorcycles, bicycles, ships, railway vehicles, manned aircraft, unmanned aircraft, as well as sporting goods, leisure goods, home appliances, agricultural machinery, building materials, etc.
Claims
1. A method for manufacturing a carbon fiber bundle composite material, comprising: Mixing carbon fiber wool composed of short carbon fibers with a molten resin containing an epoxy resin component to obtain a carbon fiber bundle containing the molten resin; solidifying the molten resin contained in the carbon fiber bundle; and mixing at least one epoxy curing agent into the molten resin.
2. The manufacturing method according to claim 1, wherein: The mixing is performed using a stirring mixer.
3. The manufacturing method according to claim 1 or 2, wherein: The molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a disc pelletizer.
4. The manufacturing method according to claim 1 or 2, wherein: The molten resin is solidified by cooling the carbon fiber bundle containing the molten resin in a conveying tube or on a conveyor belt.
5. The production method according to any one of claims 1 to 4, wherein At least a portion of the at least one epoxy curing agent is mixed into the molten resin before or while the molten resin and the carbon fiber wool are mixed.
6. The production method according to any one of claims 1 to 5, wherein The molten resin is a melt of a resin that is solid at least at a temperature in the range of 15 to 25°C.
7. The production method according to any one of claims 1 to 6, wherein The molten resin is a melt of a resin that is solid at 40°C.
8. The production method according to any one of claims 1 to 7, wherein A flame retardant is mixed into the molten resin.
9. The production method according to any one of claims 1 to 8, wherein All of the carbon fibers contained in the carbon fiber cotton have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
10. The production method according to any one of claims 1 to 9, wherein: The carbon fiber wool does not contain carbon fibers having a fiber length of less than 3 mm, or even if it contains carbon fibers having a fiber length of less than 3 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
11. The production method according to any one of claims 1 to 9, wherein The carbon fiber wool does not contain carbon fibers having a fiber length of less than 5 mm, or even if it contains carbon fibers having a fiber length of less than 5 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
12. The production method according to any one of claims 1 to 9, wherein The carbon fiber wool does not contain carbon fibers having a fiber length of less than 10 mm, or even if it contains carbon fibers having a fiber length of less than 10 mm, the amount thereof is less than 5 wt % of all carbon fibers contained in the carbon fiber wool.
13. The production method according to any one of claims 1 to 12, wherein: At least a portion of the carbon fibers contained in the carbon fiber wool is provided by defibration of chopped carbon fiber bundles.
14. The production method according to any one of claims 1 to 8, wherein All the carbon fibers contained in the carbon fiber wool are provided by defibration of chopped carbon fiber bundles.
15. The manufacturing method according to claim 14, wherein: The fiber length of the chopped carbon fiber bundle is 3 mm or more, 5 mm or more, or 10 mm or more.
16. The manufacturing method according to claim 14 or 15, wherein: The fiber length of the chopped carbon fiber bundle is 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less.
17. The production method according to any one of claims 1 to 16, wherein: All of the short carbon fibers are carbon fibers that have not been thermally degraded.
18. The production method according to any one of claims 1 to 13, wherein The short carbon fibers include thermally degraded carbon fibers.
19. The production method according to any one of claims 1 to 13 and 18, wherein Fibers other than carbon fibers are mixed into the carbon fiber cotton, and the fibers other than carbon fibers may be glass fibers.
20. The production method according to any one of claims 1 to 19, wherein The carbon fiber bundles containing the molten resin are isolated fiber bundles.
21. A carbon fiber bundle composite material produced by the production method according to any one of claims 1 to 20.
22. A carbon fiber bundle composite material, which is composed of a plurality of short carbon fibers forming a bundle and an uncured solid epoxy resin composition, wherein the positions of the front ends of the plurality of short carbon fibers are inconsistent at each end of the bundle, and the uncured solid epoxy resin composition contains at least one epoxy curing agent.
23. The carbon fiber bundle composite material according to claim 22, wherein: The uncured solid epoxy resin composition is solid at least at a temperature in the range of 15 to 25°C.
24. The carbon fiber bundle composite material according to claim 22, wherein: The uncured solid epoxy resin composition is solid at 40°C.
25. The carbon fiber bundle composite material according to any one of claims 22 to 24, wherein The bundle is isolated.
26. The carbon fiber bundle composite material according to claim 25, which has a needle-like or thread-like shape.
27. The carbon fiber bundle composite material according to any one of claims 22 to 26, wherein The plurality of short carbon fibers all have a fiber length of 60 mm or less, 50 mm or less, 40 mm or less, 30 mm or less, or 20 mm or less. 28 . The carbon fiber bundle composite material according to claim 22 , which has a bundle length of 3 mm or more, 5 mm or more, or 10 mm or more.
29. The carbon fiber bundle composite material according to any one of claims 22 to 28, wherein No carbon fiber having a fiber length of less than 3 mm is contained, or even if carbon fiber having a fiber length of less than 3 mm is contained, the amount thereof is less than 5 wt % of all carbon fibers in the carbon fiber bundle composite material.
30. The carbon fiber bundle composite material according to any one of claims 22 to 27, which has a bundle length of 5 mm or more or 10 mm or more, does not contain carbon fibers with a fiber length of less than 5 mm, or even if it contains carbon fibers with a fiber length of less than 5 mm, the amount thereof is less than 5 wt% of all carbon fibers in the carbon fiber bundle composite material.
31. The carbon fiber bundle composite material according to any one of claims 22 to 27, which has a bundle length of 10 mm or more, does not contain carbon fibers with a fiber length of less than 10 mm, or even if it contains carbon fibers with a fiber length of less than 10 mm, the amount thereof is less than 5 wt% of all carbon fibers in the carbon fiber bundle composite material.
32. The carbon fiber bundle composite material according to any one of claims 22 to 31, wherein In the plurality of short carbon fibers, a difference between a maximum value and a minimum value of the fiber length is within 5 mm.
33. The carbon fiber bundle composite material according to claim 25, which has a spindle shape.
34. The carbon fiber bundle composite material according to any one of claims 22 to 33, wherein The at least one epoxy curing agent comprises a latent curing agent.
35. The carbon fiber bundle composite material according to any one of claims 22 to 34, wherein The fiber weight content is 40 wt% or more and less than 50 wt%, 50 wt% or more and less than 60 wt%, 60 wt% or more and less than 70 wt%, or 70 wt% or more and 80 wt% or less.
36. The carbon fiber bundle composite material according to any one of claims 22 to 35, wherein All of the plurality of short carbon fibers are carbon fibers that have not been thermally degraded.
37. The carbon fiber bundle composite material according to any one of claims 22 to 35, wherein The plurality of short carbon fibers include carbon fibers that have been thermally degraded.
38. The carbon fiber bundle composite material according to any one of claims 22 to 35 and 37, wherein The plurality of short carbon fibers form the bundle together with fibers other than carbon fibers, and the fibers other than carbon fibers may be glass fibers.
39. A carbon fiber bundle composite sheet, which is formed by mutually fusing a plurality of carbon fiber bundle composite materials according to any one of claims 21 to 38.
40. A carbon fiber bundle composite sheet, comprising a plurality of carbon fiber composite materials according to any one of claims 21 to 38, wherein the carbon fiber bundle composite materials are respectively welded to at least one other carbon fiber bundle composite material.
41. A method for manufacturing a carbon fiber bundle composite sheet, comprising: A plurality of carbon fiber bundle composite materials according to any one of claims 21 to 38 are fused to each other.
42. The manufacturing method according to claim 41, wherein: During the welding, an uncured solid epoxy resin composition is added to the carbon fiber bundle composite material.
43. The production method according to any one of claims 1 to 20, wherein The molten resin is a melt of an epoxy resin having a melting point.
44. A carbon fiber bundle composite material produced by the production method according to claim 43.
45. The carbon fiber bundle composite material according to any one of claims 22 to 38, wherein The uncured solid epoxy resin composition has a melting point.
46. A carbon fiber bundle composite sheet, which is obtained by mutually welding a plurality of carbon fiber bundle composite materials according to claim 45.
47. A carbon fiber bundle composite sheet, comprising a plurality of carbon fiber composite materials according to claim 45, wherein the carbon fiber bundle composite materials are respectively welded with at least one other carbon fiber bundle composite material.
48. A method for manufacturing a carbon fiber bundle composite sheet, comprising: A plurality of carbon fiber bundle composite materials according to claim 45 are welded to each other.
49. The manufacturing method according to claim 48, wherein: During the welding, uncured epoxy resin is added to the carbon fiber bundle composite material.