Hot press molded member and method for manufacturing same
By generating enriched layers and Kirkendall holes in the hot-pressed steel parts, combined with specific process steps, the problems of insufficient hydrogen embrittlement resistance and coating corrosion resistance of the steel parts after hot-pressed molding are solved, and high strength is achieved. Lightweight and resistant to hydrogen embrittlement.
Patent Information
- Application Number
- CN202380038660.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-19
- Filing Date
- 2023-04-26
- Publication Date
- 2024-12-03
AI Technical Summary
After the existing hot-pressed steel parts are quickly cooled at high temperatures, there are problems of low hydrogen embrittlement resistance and delayed fracture. Changes in process parameters affect the mechanical characteristics of the plate, resulting in insufficient hydrogen embrittlement resistance and coating corrosion resistance.
By generating a specific level of enrichment layer and Kirkendall hole in the plating layer, the uneven diffusion rate of Al and Fe in the diffusion layer is controlled, and the residual diffusion hydrogen remaining in the steel is reduced. Reheating at 1050-1300°C and 800-950 The process steps of ℃ fine rolling, 500-700℃ coiling, pickling treatment, continuous annealing and plating are formed to achieve excellent hydrogen embrittlement resistance and coating corrosion resistance.
It effectively reduces the amount of hydrogen diffused in the steel parts after thermoforming, improves hydrogen embrittlement resistance and coating corrosion resistance, and ensures that the components are avoided while being high in strength and lightweight.
Smart Images

Figure CN119072555A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a hot press forming component mainly used for automobile body components and a manufacturing method thereof. Background Art
[0002] In recent years, hot press forming parts are widely used in structural parts of automobiles, the purpose of which is to improve fuel efficiency and protect passengers by reducing the weight of automobiles. In particular, the hot press forming parts can be applied to bumpers, doors, or pillar reinforcements that require extremely high strength or energy absorption capacity, and a representative technology related to this hot forming technology is Patent Document 1 (U.S. Patent Gazette No. 6296805).
[0003] In Patent Document 1, an Al-Si plated steel sheet is heated to 850°C or higher, and then hot-formed by a press and rapidly cooled to form the structure of the component into martensite, thereby ensuring ultra-high strength with high tensile strength. When such ultra-high strength steel for hot forming is applied, since it is formed at a high temperature, it is easy to form a complex shape, and the strength is increased by rapid cooling in the mold, so that a lightweight effect due to high strength can be expected.
[0004] However, it is known that the martensitic structure has low resistance to hydrogen embrittlement. In particular, in parts manufactured after hot forming, there is residual stress due to rapid cooling after heating, and when the amount of diffusible hydrogen in the steel increases, delayed fracture due to hydrogen embrittlement may occur, so there is a disadvantage that the application of the parts is limited. In order to overcome these disadvantages, various studies are being conducted.
[0005] In addition, since changes in process parameters during the manufacturing process of the rolled plate may cause changes in the overall or local mechanical properties of the plate, a steel composition that is less sensitive to changes in specific manufacturing parameters is required to produce a plate with good mechanical properties and uniformity, and delayed fracture caused by hydrogen embrittlement needs to be prevented. In particular, when stress is generated, diffused hydrogen present at the grain boundaries will become a cause of promoting the generation of grain boundary cracks, so a solution that can reduce the amount of diffused hydrogen in the steel after hot press forming (or hot stamping) has begun to be considered.
[0006] (Patent Document 1) U.S. Patent Publication No. 6296805 Summary of the invention
[0007] 1. Technical issues to be resolved
[0008] An object of one aspect of the present invention is to provide a thermoformed component and a method for manufacturing the same.
[0009] An object of one aspect of the present invention is to provide a hot press formed component having excellent hydrogen embrittlement resistance and a method for manufacturing the same. More specifically, the object is to provide a hot press formed component and a method for manufacturing the same, in which the amount of diffusible hydrogen remaining in the steel after hot forming is reduced by generating an enrichment layer and Kirkendall voids above a specific level in the coating layer, thereby having excellent hydrogen embrittlement resistance after hot forming.
[0010] Alternatively, another aspect of the present invention aims to provide a hot press-formed component having excellent hydrogen embrittlement resistance and coating corrosion resistance, and a method for producing the same.
[0011] Alternatively, an object of one aspect of the present invention is to provide a hot press-formed component and a method for manufacturing the same, in which, in a hot press-formed component mainly used for an automobile body component, the diffusion rates of Al and Fe in the diffusion layer are made uneven, thereby promoting the formation of Kirkendall voids in the plating layer, thereby reducing the amount of diffusible hydrogen remaining in the steel after hot pressing, thereby having excellent hydrogen embrittlement resistance after hot pressing.
[0012] The technical problems of the present invention are not limited to the above contents. The technical problems of the present invention can be understood from the overall content of this specification, and those skilled in the art of the present invention can easily understand the additional technical problems of the present invention from the overall content of this specification.
[0013] (II) Technical solution
[0014] One aspect of the present invention provides a hot press-formed component, the hot press-formed component comprising: a base steel plate; and a coating layer, the coating layer being disposed on at least one surface of the base steel plate, wherein the average number per unit area of Kirkendall voids having a major diameter of 0.5 μm to 5 μm existing in a region of the coating layer within 20 μm from an interface between the base steel plate and the coating layer satisfies 8 / 1000 μm 2 Up to 100 pieces / 1000μm 2 .
[0015] In addition, another aspect of the present invention provides a method for manufacturing a hot-formed part, the manufacturing method comprising the following steps: reheating a steel billet at 1050-1300° C., wherein the steel billet comprises, by weight%, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less (except 0%), S: 0.02% or less (except 0%), N: 0.02% or less (except 0%), Ti: 0-0.1%, B: 0.0 001-0.01%, Mo: 0-1.00%, V: 0-1.00%, Ca: 0-0.01%, Nb: 0-0.1%, W: 0-1%, REM: 0-0.3%, the balance of Fe and other inevitable impurities; the reheated steel billet is finish rolled at 800-950°C to obtain a hot-rolled steel plate; the hot-rolled steel plate is coiled at 500-700°C; the coiled hot-rolled steel plate is pickled so that the product of the acid concentration and the pickling time is 800-10000g / L seconds; continuously annealing the pickled steel sheet while controlling the average heating rate of each zone to satisfy the following equations 1 to 3; immersing the continuously annealed steel sheet in a plating bath composed of aluminum or an aluminum alloy for plating; and heat treating the plated steel sheet at Ac3 to 950°C for 1 to 1000 seconds, and then hot pressing.
[0016] [Formula 1]
[0017] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec
[0018] [Formula 2]
[0019] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec
[0020] [Formula 3]
[0021] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec
[0022] (In the above formula 1, the first zone refers to the interval until the surface temperature of the steel plate reaches 500°C, the second zone refers to the interval from 500°C to 700°C, and the third zone refers to the interval until the surface temperature of the steel plate reaches the maximum temperature.)
[0023] One aspect of the present invention provides a hot press-formed component, comprising: a base steel plate; and a coating layer, the coating layer being disposed on at least one side of the base steel plate, wherein the hot press-formed component satisfies the following relational expression 2-1.
[0024] [Equation 2-1]
[0025] 9.5≤D B2 / D A2 ≤11.0
[0026] (In the relational expression 2-1, the D B2 D represents the area corresponding to the atomic content ratio of aluminum (Al) in the hot press formed part being 0.25 to 0.45 Fe / D Al The absolute value of D A2 D represents the range in which the atomic content ratio of aluminum (Al) in the hot press formed part is 0.01 to 0.2 Fe / D Al The absolute value of D Fe represents the diffusion rate of iron (Fe), the D Al Indicates the diffusion rate of aluminum (Al).
[0027] In addition, another aspect of the present invention provides a method for manufacturing a hot press-formed component, the manufacturing method comprising the following steps: reheating a steel billet at 1050-1300° C., wherein the steel billet comprises, by weight%, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less (excluding 0%), S: 0.02% or less (excluding 0%), N: 0.02% or less (excluding 0%), Ti: 0.1% or less (including 0%), B: 0.0001-0.01%, Mo: 1 .00% or less (including 0%), V: 1.00% or less (including 0%), Ca: 0.01% or less (including 0%), Nb: 0.1% or less (including 0%), W: 1% or less (including 0%), REM: 0.3% or less (including 0%), the balance of Fe and other inevitable impurities; the reheated steel billet is finish rolled at 800-950°C to obtain a hot-rolled steel plate; the hot-rolled steel plate is coiled at 500-700°C; the coiled hot-rolled steel plate is pickled so that the product of the acid concentration and the pickling time is 800-10000g / L seconds; continuously annealing the pickled steel sheet while controlling the average heating rate of each zone to satisfy the following equations 1 to 3; immersing the continuously annealed steel sheet in a plating bath composed of aluminum or an aluminum alloy for plating; and heat treating the plated steel sheet at Ac3 to 950°C for 1-1000 seconds, and then hot pressing, wherein during the continuous annealing, the heat treatment area at 700°C or above satisfies 5000°C·seconds to 25000°C·seconds according to time.
[0028] [Formula 1]
[0029] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec
[0030] [Formula 2]
[0031] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec
[0032] [Formula 3]
[0033] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec
[0034] (In the above formula 1, the first zone refers to the interval until the surface temperature of the steel plate reaches 500°C, the second zone refers to the interval from 500°C to 700°C, and the third zone refers to the interval until the surface temperature of the steel plate reaches the maximum temperature.)
[0035] (III) Beneficial effects
[0036] According to one aspect of the present invention, a hot press-formed component having excellent hydrogen embrittlement resistance and a method for manufacturing the same can be provided.
[0037] Alternatively, according to another aspect of the present invention, a hot press-formed component having excellent hydrogen embrittlement resistance and coating corrosion resistance and a method for manufacturing the same can be provided.
[0038] Alternatively, according to one aspect of the present invention, a hot press-formed component and a method for manufacturing the same can be provided. In the hot press-formed component mainly used for automobile body parts, the diffusion rates of Al and Fe in the diffusion layer are made uneven, thereby promoting the formation of Kirkendall voids in the coating layer, thereby reducing the amount of diffusible hydrogen remaining in the steel after hot forming, thereby having excellent hydrogen embrittlement resistance after hot press forming.
[0039] Various beneficial advantages and effects of the present invention are not limited to the above contents, and the above advantages and effects can be more easily understood in the course of describing specific embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 : is a photograph showing a cross-sectional test piece in a direction perpendicular to the rolling direction of the hot press-formed component obtained in Example 1 of the present invention, which was taken with a scanning electron microscope (SEM).
[0041] Figure 2 : is a photograph showing a cross-sectional test piece in a direction perpendicular to the rolling direction of the hot press-formed component obtained in Example 2-1 according to one specific embodiment of the present invention, taken with a scanning electron microscope (SEM).
[0042] Figure 3 : is a diagram schematically showing a heat treatment area according to time in a heat treatment interval above 700° C. in a continuous annealing step according to a specific embodiment of the present invention (ie, a surface layer enrichment heat treatment area).
[0043] Figure 4 is a schematic diagram showing lnC vs. (vs.) x in the coating of a hot press formed part according to a specific embodiment of the present invention. 2 . Best Mode for Carrying Out the Invention
[0044] Below, the preferred embodiment of the present invention is described. However, the embodiment of the present invention can be modified into various other forms, and the scope of the present invention is not limited to the embodiment described below. In addition, the embodiment of the present invention is provided to more completely describe the present invention to those skilled in the art.
[0045] The inventors have found that defects caused by hydrogen-induced delayed fracture can be suppressed by reducing the amount of diffusible hydrogen absorbed during the heat treatment of hot press forming. Specifically, in the step of heating a slab having a coating composed of aluminum or an aluminum alloy during hot press forming, water vapor present in the heat treatment furnace is adsorbed on the surface of the slab. Subsequently, during the formation of an austenite phase with a high hydrogen solubility at high temperature, hydrogen generated by water dissociation is absorbed in the steel. However, when the rapid cooling caused by hot press forming occurs and the phase is transformed into a martensitic phase, the solubility of hydrogen decreases sharply, and the alloy coating formed by the alloying of the coating acts as an obstacle that prevents hydrogen from being difficult to release. Therefore, a large amount of diffusible hydrogen content remains in the steel, thereby increasing the possibility of cracks due to hydrogen-induced delayed fracture. Therefore, reducing the amount of diffusible hydrogen absorbed during heat treatment is an important factor in suppressing defects.
[0046] Therefore, the inventors have carefully studied and confirmed that if various enrichment layers are formed on the surface of the base iron, Kirkendall voids above a certain level can be formed in the coating layer. The Kirkendall voids thus formed effectively block the diffusible hydrogen diffusing in the steel by trapping hydrogen that penetrates into the steel during hot press forming, thereby effectively reducing the content of diffusible hydrogen, and ultimately judging that the effect of improving hydrogen embrittlement resistance can be expected.
[0047] In addition, in order to ensure hydrogen embrittlement resistance, the inventors found that the amount of diffusible hydrogen in the hot-formed parts must meet 0.2 ppm to ensure excellent hydrogen embrittlement resistance. This is because even if the parts with a diffusible hydrogen amount of 0.2 ppm or less are subjected to stress of the same yield strength for 120 hours and the test piece is subjected to bending stress, cracks in the parts will not occur.
[0048] Next, a hot press-formed component according to one aspect of the present invention will be described in detail.
[0049] According to one aspect of the present invention, a hot press-formed component includes: a base steel plate; and a coating layer provided on at least one side of the base steel plate.
[0050] First, the alloy composition of the base steel sheet according to one aspect of the present invention will be described below. It should be noted that in the present invention, when each element is expressed as a content, it represents weight % unless otherwise specified.
[0051] Carbon (C): 0.02-0.5 wt%
[0052] The C is an element that improves the strength of the heat-treated parts and improves the hardenability. As an element necessary for adjusting the strength, it is necessary to add it appropriately. If the content of C is less than 0.02%, the hardenability is low, it is difficult to ensure sufficient strength, and it is difficult to apply to hot-pressed parts, so it is necessary to add more than 0.02% of the C. In addition, if the content of the C exceeds 0.5%, the strength rises excessively, brittleness may be caused, and weldability deteriorates, so the upper limit of the content of the C is preferably less than 0.5%.
[0053] Silicon (Si): 0.001-2% by weight
[0054] The Si must be added as a deoxidizer during the steelmaking process, and as a solid solution strengthening element and an element that inhibits the formation of carbides, it is not only effective for homogenizing the internal structure, but also helps to improve the strength of hot press-formed parts, and the Si is added as an element effective for material homogenization. However, if the Si content is less than 0.001%, not only the above effects cannot be expected, but also excessive process costs for controlling the Si content are generated. If the Si content exceeds 2%, the plateability is greatly reduced due to excessive Si oxides generated on the surface of the steel sheet during the annealing process, so the Si content of less than 2% is added.
[0055] Manganese (Mn): 0.1-4 wt%
[0056] The Mn can not only ensure the desired strength due to the solid solution strengthening effect, but also needs to be added to suppress the formation of ferrite during hot press forming by improving hardenability. If the Mn content is less than 0.1%, it is difficult to obtain a sufficient hardenability effect, and too many other expensive alloy elements are required for insufficient hardenability, resulting in a problem of a significant increase in manufacturing costs. In addition, if the Mn content exceeds 4%, the band structure arranged along the rolling direction on the fine structure is aggravated, causing the inhomogeneity of the internal structure, which may lead to a deterioration in collision resistance, so the Mn content of less than 4% is added.
[0057] Phosphorus (P): 0.05% by weight or less (except 0%)
[0058] The P exists in the steel as an impurity. If the maximum content of the P exceeds 0.05%, the weldability of the hot-formed parts and the physical properties of the material due to high-temperature grain boundary segregation deteriorate, so the upper limit of the P is set to 0.05%. However, considering that the P is inevitably included as an impurity, the lower limit of the P content does not include 0%, or may be 0.5 ppm.
[0059] Sulfur (S): 0.02% by weight or less (except 0%)
[0060] The S, as an impurity, is an element that hinders the ductility, impact properties and weldability of the parts, so the maximum content of the S is limited to 0.02%. However, considering that it is inevitably included as an impurity, the lower limit of the S content does not include 0%, or may be 1 ppm.
[0061] Aluminum (Al): 0.001-1% by weight
[0062] The Al is an element that plays a deoxidizing role with Si in the steelmaking process to improve the cleanliness of steel. If the Al content is less than 0.001%, it is not only difficult to obtain the above-mentioned effect, but also too high a manufacturing process cost is invested in order to control the Al content, so it is not preferred. In addition, if the Al content exceeds 1%, the high-temperature ductility is reduced due to the formation of too many AlN precipitates during the continuous casting process, thereby generating slab cracks and possibly causing manufacturing problems, so the upper limit of the Al content is set to 1%.
[0063] Nitrogen (N): 0.02% by weight or less (except 0%)
[0064] The N is contained in the steel as an impurity. However, if the N content exceeds 0.02%, AlN is formed together with the added Al, and slab cracks are easily generated, so the upper limit of the N content is set to 0.02%. However, considering that the N is inevitably contained as an impurity, the lower limit of the N content does not include 0%, or may be 1 ppm.
[0065] Titanium (Ti): 0.1% or less (including 0%)
[0066] The Ti combines with nitrogen remaining in the steel as an impurity to generate TiN, thereby playing a protective role in ensuring that B of hardenability will not become a compound. Therefore, the Ti can be selectively added to ensure the above-mentioned effect, and by adding the Ti to form TiC precipitates, precipitation strengthening and grain refinement effects can be expected. However, if the content of the Ti exceeds 0.1%, coarse TiN is formed in large quantities, and the material of the steel is deteriorated, so the upper limit of the content of Ti is set to 0.1%. On the other hand, although not particularly limited, as an example, the lower limit of the content of the Ti can be 0.001%, and the content of the Ti can be selectively 0.001-0.1%.
[0067] Boron (B): 0.0001-0.01%
[0068] The B is an element that can effectively improve the hardenability and segregates at the original austenite grain boundaries, thereby suppressing the brittleness of the hot-formed parts caused by the grain boundary segregation of impurities P and / or S. However, in order to control the B content to less than 0.0001%, it is necessary to invest too high a process cost, so it is not preferred. In addition, if the B content exceeds 0.01%, due to Fe 23 The formation of CB6 complex may induce brittleness during hot rolling, so the upper limit of the B content is set to 0.01%.
[0069] Molybdenum (Mo): 1.00% or less (including 0%)
[0070] The Mo is an element that can effectively improve hardenability, and the Mo can be selectively included. In order to suppress the problem of excessively high manufacturing cost, the upper limit of the amount of addition of the Mo can be 1.00%. On the other hand, although not particularly limited, as an example, the lower limit of the Mo content can be 0.001%, and the Mo content can be selectively 0.001-1.00%.
[0071] Vanadium (V): 1.00% or less (including 0%)
[0072] The V is an element that can improve hydrogen embrittlement resistance by reducing grain boundaries by forming carbides, and the V can be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of V added can be 1.00%. On the other hand, although not particularly limited, as an example, the lower limit of the V content can be 0.001%, and the V content can be selectively 0.001-1.00%.
[0073] Calcium (Ca): 0.01% or less (including 0%)
[0074] Ca is an element added to improve the cleanliness of steel by removing a certain level of P and S during steelmaking, and the Ca may be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of Ca added may be 0.01%. On the other hand, although not particularly limited, as an example, the lower limit of the Ca content may be 0.001%, and the Ca content may be selectively 0.001-0.01%.
[0075] Niobium (Nb): 0.1% or less (including 0%)
[0076] Nb is an element that can improve hydrogen embrittlement resistance by reducing grain boundaries by forming carbides, and the Nb can be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of Nb added can be 0.1%. On the other hand, although not particularly limited, as an example, the lower limit of the Nb content can be 0.001%, and the Nb content can be selectively 0.001-0.1%.
[0077] Tungsten (W): 1% or less (including 0%)
[0078] W is an element that can improve hydrogen embrittlement resistance by forming carbides to make the grain boundaries fine, and can be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of W added can be 1%. On the other hand, although not particularly limited, as an example, the lower limit of the W content can be 0.001%, and the W content can be selectively 0.001-1%.
[0079] Rare earth elements (REM): 0.3% or less (including 0%)
[0080] Rare earth elements (REM) are elements that may be included in steelmaking. If the rare earth element exceeds 0.3%, REM is excessively segregated at the grain boundaries, and hydrogen embrittlement resistance may be deteriorated. Therefore, the content of the REM may be selectively 0.3% or less. On the other hand, although not particularly limited, as an example, the lower limit of the content of the REM may be 0.001%, and the content of the REM may be selectively 0.001-0.3%.
[0081] The first group of elements: 0.005-1% by weight
[0082] The base steel plate may further include 0.005 wt % to 1 wt % of one or more first group elements selected from Sb, Sn, As, Bi, Cu, and Ni, each independently.
[0083] When the first group of elements is added, in the coating of the hot press formed part, there may be a region where the concentration of the first group of elements is enriched in the surface area from the interface between the base steel plate and the coating to the coating side direction. With the formation of such a region enriched in the first group of elements, the diffusion rate of aluminum (Al) and iron (Fe) that diffuse mutually during high temperature heat treatment becomes uneven, thereby promoting the formation of Kirkendall voids in the coating after hot press forming. Therefore, if the content of each of the first group of elements is less than 0.005%, the enriched layer cannot be fully formed, and the above-mentioned Kirkendall voids cannot be fully generated, and it may be difficult to expect the effect of improving hydrogen embrittlement resistance. On the other hand, if the content of each of the first group of elements exceeds 1%, not only the cost of the alloy iron increases, but also too many voids are formed in the coating, and the coating peels off due to the stress applied during hot forming, which may cause the coating corrosion resistance to deteriorate.
[0084] Alternatively, in order to further improve the above effects, the lower limit of the content of the first group of elements may be 0.008%, or the upper limit of the content of the first group of elements may be 0.95%.
[0085] Alternatively, according to one aspect of the present invention, in order to further improve the above effect, the first group of elements may include 0.005-0.1% of each of the elements selected from Sb, Sn, As and Bi. Alternatively, in order to further improve the above effect, the lower limit of the content of the one or more elements selected from Sb, Sn, As and Bi may be 0.01%, or the upper limit of the content of the one or more elements selected from Sb, Sn, As and Bi may be 0.09%.
[0086] In addition, according to one aspect of the present invention, in order to further improve the above-mentioned effect, the first group of elements may include 0.05-1% of one or more elements selected from Cu and Ni, each independently. Alternatively, in order to further improve the above-mentioned effect, the lower limit of the content of the one or more elements selected from Cu and Ni may be 0.1%, or the upper limit of the content of the one or more elements selected from Cu and Ni may be 0.9%.
[0087] The balance other than the above components is iron (Fe), and as long as it is a component that can be contained in the steel sheet for hot press forming, there is no particular restriction on further addition. In addition, in the conventional manufacturing process, undesirable impurities may inevitably be mixed from the raw materials or the surrounding environment, and therefore these impurities cannot be excluded. These impurities are well known to those skilled in the art of conventional manufacturing processes, and therefore all of them are not particularly described in this specification.
[0088] In the present invention, the type of the coating is not particularly limited, and as long as it is a coating applied to an existing hot-forming plated steel sheet, it can be applied to the present invention without limitation. As an example, the coating can be an aluminum or aluminum alloy coating, and the coating can preferably contain: Si: 6-12%, Fe: 4% or less (including 0%), the balance of Al and other inevitable impurities.
[0089] Alternatively, as another example, in the case of hot-dip coating, hot-dip aluminum coating, hot-dip Al-Si coating, hot-dip Al-Si-Mg coating, hot-dip Al-Zn coating, hot-dip Al-Mg coating, etc. can be applied. As alloyed hot-dip coating, alloyed hot-dip aluminum coating, alloyed hot-dip Al-Si coating, alloyed hot-dip Al-Si-Mg coating, alloyed hot-dip Al-Zn coating, alloyed hot-dip Al-Mg coating, etc. can be exemplified. The coating may also contain at least one of Mn, Cr, Cu, Mo, Ni, Sb, Sn, Ti, Ca, Sr, Mg, Be, Li, and Na. The coating adhesion amount is not particularly limited, for example, it is set to an adhesion amount within a conventional range.
[0090] In the coating layer of the hot press-formed component, the average number per unit area of Kirkendall voids having a major diameter of 0.5 μm to 5 μm existing in a region within 20 μm from the interface between the base steel sheet and the coating layer satisfies 8 / 1000 μm 2 Up to 100 pieces / 1000μm 2 .
[0091] Kirkendall voids are formed along the coating side direction from the interface between the base iron and the coating generated by the addition of the above-mentioned first group of elements and impurities. Among the Kirkendall voids thus formed, Kirkendall voids of a specific size (long diameter of 0.5 μm to 5 μm) formed in an area within 20 μm from the interface between the base iron and the coating play a role in suppressing hydrogen embrittlement that may occur in the parts after hot forming by reducing the amount of diffusible hydrogen that penetrates into the steel during the hot press forming process. That is, Kirkendall voids with a long diameter of less than 0.5 μm cannot effectively capture hydrogen absorbed during the heat treatment for hot press forming, so that the effect of improving hydrogen embrittlement resistance is minimal. In addition, Kirkendall voids with a long diameter exceeding 5 μm become defects, causing coating peeling, and due to the peeling of part of the coating during hot forming, the corrosion resistance of the coating is deteriorated.
[0092] Therefore, the inventors have carefully studied and found that excellent hydrogen embrittlement resistance and coating corrosion resistance can be ensured by keeping the average number of Kirkendall voids per unit area of a specific size within an appropriate range. Specifically, if the average number of Kirkendall voids per unit area is less than 8 / 1000 μm 2If the average number of Kirkendall voids per unit area exceeds 100 / 1000 μm, the diffused hydrogen cannot be sufficiently prevented from penetrating, thereby causing a problem of deterioration in the hydrogen embrittlement resistance of the component. 2 , the stress applied during hot press forming causes the plating to peel off, resulting in a problem of deterioration in the corrosion resistance of the parts.
[0093] According to one aspect of the present invention, in order to further improve the above effect, the lower limit of the average number of Kirkendall voids per unit area may be 10 / 1000 μm 2 , or 18 / 1000μm 2 .
[0094] According to one aspect of the present invention, in order to further improve the above effect, the upper limit of the average number of Kirkendall voids per unit area may be 95 / 1000 μm 2 , or 92 / 1000μm 2 .
[0095] In addition, the same contents as those known in the technical field can be applied to the Kirkendall cavity, and therefore it is not defined separately in this specification.
[0096] In this specification, there is no particular limitation on the method for measuring the average number of Kirkendall voids per unit area, but as an example, measurement can be performed by observing a cross section of the structure (for example, collecting a test piece in a direction perpendicular to the rolling direction) using a scanning electron microscope (SEM; Scanning Electron Microscopy).
[0097] At this time, the interface between the base steel sheet and the coating can also be distinguished based on the contrast difference observed by SEM / OM, but can also be distinguished based on component analysis by SEM-EDS, EPMA, etc. That is, when measuring through the base steel sheet-coating by line profile, etc., the interface between the base steel sheet and the coating can be set to a site where the Al content is 2 wt%. If the Al content exceeds 2%, it can be classified as the coating, and if the Al content is 2% or less, it can be classified as the base iron.
[0098] In addition, when a parallel line is drawn at 20 μm from the interface line that distinguishes the interface between the base steel sheet and the coating layer in the coating side direction, as shown in FIG. Figure 1 As shown, a portion having a black contrast existing in a region within 20 μm from the interface ( 100 ) between the base steel sheet and the coating layer can be identified as a Kirkendall void 11 .
[0099] In the present specification, the major diameter of the Kirkendall voids refers to an equivalent circle diameter when an ideal circle having the same area as that of each Kirkendall void is assumed.
[0100] In addition, the method for measuring the average number of Kirkendall voids per unit area is not particularly limited, and can be measured using a conventional method. 2 3 test pieces of the same area, and then measure the 1000 μm 2 The number of Kirkendall voids completely contained in the area of , and then the average number of Kirkendall voids per unit area can be measured by taking their average value. However, the number of the plurality of test pieces can be two or more, so there is no particular limitation on the number.
[0101] According to one aspect of the present invention, the base steel sheet of the hot press-formed component may further include one or more first group elements selected from Sn, As, Bi, Cu and Ni, and may satisfy the following Relationship 1.
[0102] [Equation 1]
[0103]
[0104] (In the relational formula 1, the X 镀层(coat) represents the average content of X in the coating. 最大(max) represents the maximum value of the X content in the coating. In addition, the X represents one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni.
[0105] The above X 镀层 and X 最大 is a unit for expressing the content. When calculating the above relational formula 1, as long as the units are consistent with each other, there is no particular limitation on the units. As an example, it can be % by weight. 镀层 and X 最大 The measuring method is not particularly limited.
[0106] However, as an example, the X 镀层 and X 最大 The measurement can be performed by analyzing the change in the content of the first group of elements along the thickness direction of the base steel sheet side from any point on the coating surface using glow discharge spectroscopy (GDS). At this time, it should be noted that for any first group of elements, each element satisfies the value of the above-mentioned relational expression 1.
[0107] X as the average content of X in the coating 镀层In the GDS curve, when the area from the coating surface to the interface between the base steel sheet and the coating is divided at the same interval along the thickness direction (for example, the direction perpendicular to the rolling direction), it can be measured by calculating the average value of the X content at each point. At this time, the interface between the base steel sheet and the coating can be determined as a point on the GDS curve where the Al content is 2 wt%.
[0108] According to one aspect of the present invention, when the hot press formed part fails to satisfy the above-mentioned relational expression 1, since the difference in diffusion gradients between Fe and Al cannot be sufficiently formed during the hot forming process, it may be difficult to sufficiently promote the formation of Kirkendall voids in the coating layer. Therefore, it is difficult to achieve the effect of reducing the amount of diffusible hydrogen in the steel, and thus it may be difficult to expect to ensure the effect of the present invention.
[0109] Next, the "method for producing a thermoformed component" will be described.
[0110] Reheating of slabs
[0111] First, the steel slab is reheated at 1050-1300° C. If the reheating temperature is lower than 1050° C., the slab structure cannot be sufficiently homogenized, so it is difficult to perform resolidification when using precipitated elements. On the other hand, if the reheating temperature exceeds 1300° C., too much oxide layer is formed, resulting in an increase in the manufacturing cost for removing the oxide layer and an increase in the possibility of surface defects after finish rolling.
[0112] Finish rolling
[0113] The reheated steel slab is finished rolled at 800-950°C to obtain a hot rolled steel sheet. If the finishing rolling temperature is lower than 800°C, two-phase rolling is performed, and ferrite is introduced into the surface layer of the steel sheet, making it difficult to control the sheet shape. On the other hand, if the finishing rolling temperature exceeds 950°C, coarsening of hot rolled grains may occur.
[0114] Rolling
[0115] After the finish rolling is terminated, the hot rolled steel sheet is coiled at 500-700°C and then cooled to produce a hot rolled coil. If the coiling temperature is lower than 500°C, the entire or part of the steel sheet forms martensite, which not only makes it difficult to control the shape of the coil, but also causes a problem of reduced cold rolling properties due to excessive increase in the strength of the hot rolled steel sheet. On the other hand, if the coiling temperature exceeds 700°C, too many coarse carbides are formed, and when stress is generated in the hot formed part, cracks are promoted, so there is a problem of reduced collision resistance.
[0116] Pickling
[0117] The coiled hot-rolled steel sheet is pickled so that the product of the acid concentration and the pickling time is 800-10000g / L As the steel sheet after the above-mentioned reheating, finishing rolling and coiling steps, when the above-mentioned first group of elements are added, the enriched area of the first group of elements is formed in the coating, and in the pickling process, when 800-10000g / L When the product of the acid concentration and the pickling time is within the second range, the formation of the above-mentioned enriched area can be effectively promoted, thereby achieving the effect of reducing the amount of diffusible hydrogen in the steel.
[0118] Specifically, when the product of the acid concentration and the pickling time is less than 800 g / L When the acid concentration and pickling time exceed 10000g / L, the scale produced during the finishing rolling process cannot be fully removed, which may cause product quality problems. If the concentration of acid is less than 10000 g / L, all or part of the enriched area will be lost during the pickling process, and the expected effect may not be achieved. In addition, since it may increase the manufacturing cost, the upper limit of the product of the acid concentration and the pickling time is set to 10000 g / L. However, when there is more than one pickling tank and the corresponding acid concentrations and pickling times are different, the value can be expressed by adding the product of the acid concentration and the pickling time of each pickling tank.
[0119] According to one aspect of the present invention, the acid that can be used in the pickling treatment step can be applied to an acid that can be conventionally used in the technical field. Representatively, the acid includes hydrochloric acid (HCl), sulfuric acid (H2SO4), etc. In particular, in the present invention, compared with the use of other acids, the pickling ability is excellent and the process cost is economical when hydrochloric acid (HCl) is used, and the possibility of generating surface foreign matter after pickling is small, so that the surface quality is easily ensured.
[0120] In addition, although not particularly limited, according to one aspect of the present invention, the concentration of the acid may be in the range of 40-500 g / L. If the concentration of the acid is less than 40 g / L, the surface oxide scale generated during the hot rolling process cannot be fully removed within the limited pickling time, and defects may be generated on the surface of the steel plate. On the other hand, if the concentration of the acid exceeds 500 g / L, it may be difficult to exert the desired effect of the invention in the final hot press-formed part due to the loss of the enriched area, and defects in the surface portion caused by over-pickling may be caused.
[0121] In addition, although not particularly limited, according to one aspect of the present invention, the pickling time may be 5-60 seconds (s). If the pickling time is less than 5 seconds, the surface scale of the steel plate cannot be fully removed, which may cause surface defects. If the pickling time exceeds 60 seconds, the productivity is reduced due to the loss of the enriched area, which may increase the process cost.
[0122] In addition, although not particularly limited, according to one aspect of the present invention, the pickling temperature may be 40-120°C, and more preferably may be 50-100°C. If the pickling temperature is lower than 40°C, the pickling force is insufficient, which may adversely affect the quality of the product. On the other hand, if the pickling temperature exceeds 120°C, not only the fixed cost for maintaining the high temperature is increased, but also due to the high temperature, the vaporization amount of the pickling solution increases, and there may be a problem of increased cost for replenishing the lost pickling solution.
[0123] Continuous annealing
[0124] The pickled steel sheet is continuously annealed, and the average heating rate of each zone is controlled to satisfy the following equations 1 to 3.
[0125] [Formula 1]
[0126] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec
[0127] [Formula 2]
[0128] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec
[0129] [Formula 3]
[0130] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec
[0131] (In the above formula 1, the first zone refers to the interval until the surface temperature of the steel plate reaches 500°C, the second zone refers to the interval from 500°C to 700°C, and the third zone refers to the interval until the surface temperature of the steel plate reaches the maximum temperature.)
[0132] In the present invention, by performing continuous annealing so that the average heating rate of each zone during the continuous annealing satisfies Formulas 1 to 3, the added first group of elements can be effectively diffused into the coating area in contact with the base steel plate, thereby effectively forming and promoting the enrichment area of the first group of elements.
[0133] During the continuous annealing, each zone can be divided based on the surface temperature of the steel plate. The interval from the starting point (normal temperature) to the temperature at which the surface temperature of the steel plate reaches 500°C can be defined as the first zone (Zone 1). Next, the temperature interval from 500°C to 700°C can be defined as the second zone (Zone 2). In addition, the temperature interval from 700°C to the maximum annealing target temperature desired by the steel plate can be defined as the third zone (Zone 3). That is, by making the annealing temperature condition from the starting point to the maximum annealing target temperature satisfy the above formulas 1 to 3, the first group of elements as the added elements for enrichment are fully enriched in the surface part, thereby ensuring excellent hydrogen embrittlement resistance after the heat treatment for hot forming. Specifically, by rapidly increasing the average heating rate of the first zone, the time of maintaining at high temperature can be further ensured, and since the diffusion rate of the enriched elements to the coating area in contact with the base steel plate at high temperature is fast, the surface enriched elements can be fully formed in the hot pressed part after annealing. At this time, it should be noted that the first zone to the third zone are arranged in sequence in the conveying direction of the steel plate.
[0134] In addition, for the average heating rate of each zone, the surface temperature of the steel plate can be measured by the non-contact heat treatment temperature in the middle or end of each zone. If the surface temperature of the steel plate at each measurement position and the plate passing time according to the line speed (Linespeed) are known, the average heating rate of each zone can be obtained by inverse calculation.
[0135] Plating
[0136] The steel sheet after the continuous annealing is immersed in a plating bath composed of aluminum or an aluminum alloy for plating. At this time, the plating bath can be an aluminum plating bath or an aluminum-based plating bath, for example, an Al-Si plating bath. Specifically, after annealing, a plated steel sheet can be manufactured by passing the hot-rolled steel sheet through a plating bath composed of aluminum or an aluminum alloy. At this time, the plating conditions can be applied to the present invention without restriction as long as they are the plating conditions commonly applied to steel sheets for hot press forming, but as an example, the composition of the plating bath can include Si: 6-12%, Fe: 4% or less (including 0%), the remainder of Al and other inevitable impurities.
[0137] At this time, although not particularly limited, the plating amount in the plating step is preferably 20-140 g / m 2 If the coating weight on one side is less than 20g / m 2 , it is difficult to ensure the corrosion resistance required for hot-formed parts. If the coating weight on one side exceeds 140g / m 2, the manufacturing cost increases due to excessive plating adhesion, and it is difficult to plate the coating evenly over the entire width and length of the coil.
[0138] Cold Rolling
[0139] According to one aspect of the present invention, after the pickling treatment, the method may further include cold rolling the hot-rolled steel sheet to produce a cold-rolled steel sheet.
[0140] Hot Press Forming
[0141] A method for manufacturing a final component having excellent hydrogen embrittlement resistance and collision resistance by hot forming and die quenching using a coated steel sheet manufactured by the above method is described. A slab for hot forming is manufactured using a coated steel sheet manufactured according to the composition and manufacturing method of the above steel. The slab is heated above the austenite single phase region temperature, more specifically, within a temperature range of above the Ac3 temperature and below 975°C. At this time, if the heating temperature is lower than the Ac3 temperature, it is difficult to ensure strength and collision resistance due to the presence of untransformed ferrite according to the two-phase region. On the other hand, if the heating temperature exceeds 975°C, too much oxide is generated on the surface of the component, it is difficult to ensure spot weldability, and the manufacturing cost for maintaining high temperature increases. On the other hand, the Ac3 temperature can be similarly defined as known in the technical field.
[0142] Then, the heated slab is preferably kept in the above temperature range for 1-1000 seconds. If the holding time is less than 1 second, it is difficult to achieve uniform temperature distribution throughout the slab temperature, which may cause material deviation at each position. On the other hand, if the holding time exceeds 1000 seconds, as in the case of exceeding the heating temperature, it is difficult to ensure spot weldability due to excessive oxides generated on the surface of the component, and the manufacturing cost of the component increases.
[0143] In addition, although not particularly limited, according to one aspect of the present invention, the heated slab is transported to a press machine, and hot forming and die quenching may be performed at a cooling rate of -20°C or more. At this time, if the cooling rate is less than -20°C, a ferrite phase is introduced during the cooling process and generated at the grain boundary, which may reduce strength and collision resistance. There is no particular limitation on the transport, hot press forming and cooling steps of the slab, and a conventional hot press forming method may be directly applied.
[0144] In addition, the [hot press formed component] according to another aspect of the present invention will be described in detail below.
[0145] The inventors have found that defects caused by hydrogen-induced delayed fracture can be suppressed by reducing the amount of diffusible hydrogen absorbed during heat treatment of hot press forming. Specifically, in the step of heating a slab having a coating composed of aluminum or an aluminum alloy during hot press forming, water vapor present in a heat treatment furnace is adsorbed on the surface of the slab. Subsequently, hydrogen generated by water dissociation is absorbed in the steel during the formation of an austenite phase having a high hydrogen solubility at high temperature. However, when rapid cooling caused by hot press forming occurs and the steel is transformed into a martensitic phase, the solubility of hydrogen decreases sharply, and the alloy coating formed while the coating is alloyed acts as an obstacle to the release of hydrogen.
[0146] Therefore, a large amount of diffusible hydrogen content remains in the steel, thereby increasing the possibility of cracking due to hydrogen-induced delayed fracture. Therefore, reducing the amount of diffusible hydrogen occluded during heat treatment is an important factor in suppressing defects.
[0147] Therefore, the inventors have carefully studied and found that when various enrichment layers are formed on the surface of the base iron, Kirkendall voids above a certain level can be formed in the coating layer. The Kirkendall voids thus formed effectively block the diffusible hydrogen diffusing in the steel by capturing hydrogen that penetrates into the steel during hot press forming, thereby effectively reducing the content of diffusible hydrogen and ultimately predicting that the effect of improving hydrogen embrittlement resistance can be expected.
[0148] In addition, in order to ensure hydrogen embrittlement resistance, the inventors have found that the amount of diffusible hydrogen in the hot-formed parts must meet a level of 0.25 ppm or less to ensure excellent hydrogen embrittlement resistance. This is because even if a part with a diffusible hydrogen amount of 0.25 ppm or less is subjected to stress of the same yield strength for 120 hours and the test piece is subjected to bending stress, cracks in the part will not occur.
[0149] According to one aspect of the present invention, a hot press-formed component includes: a base steel plate; and a coating layer provided on at least one side of the base steel plate.
[0150] First, the alloy composition of the exemplary base steel sheet of the present invention is described below, but the alloy composition of the base steel sheet is not particularly limited. It should be noted that in the present invention, when each element is expressed as a content, it represents weight % unless otherwise specified.
[0151] Carbon (C): 0.02-0.5 wt%
[0152] The C is an element that improves the strength of the heat-treated parts and improves the hardenability. As an element necessary for adjusting the strength, it is necessary to add it appropriately. If the content of C is less than 0.02%, the hardenability is low, it is difficult to ensure sufficient strength, and it is difficult to apply to hot-pressed parts, so it is necessary to add more than 0.02% of the C. In addition, if the content of the C exceeds 0.5%, the strength rises excessively, brittleness may be caused, and weldability deteriorates, so the upper limit of the content of the C is set to less than 0.5%.
[0153] Silicon (Si): 0.001-2% by weight
[0154] The Si must be added as a deoxidizer during the steelmaking process, and as a solid solution strengthening element and an element that inhibits the formation of carbides, it is not only effective for homogenizing the internal structure, but also helps to improve the strength of hot press-formed parts, and the Si is added as an element effective for material homogenization. However, if the Si content is less than 0.001%, not only the above effects cannot be expected, but also excessive process costs for controlling the Si content are generated. If the Si content exceeds 2%, the plateability is greatly reduced due to excessive Si oxides generated on the surface of the steel sheet during the annealing process, so the Si content of less than 2% is added.
[0155] Manganese (Mn): 0.1-4 wt%
[0156] The Mn can not only ensure the desired strength due to the solid solution strengthening effect, but also needs to be added to suppress the formation of ferrite during hot press forming by improving hardenability. If the Mn content is less than 0.1%, it is difficult to obtain a sufficient hardenability effect, and too many other expensive alloy elements are required for insufficient hardenability, resulting in a problem of a significant increase in manufacturing costs. In addition, if the Mn content exceeds 4%, the banded structure arranged along the rolling direction on the fine structure is aggravated, causing the inhomogeneity of the internal structure, which may lead to a deterioration in collision resistance, so the Mn content of less than 4% is added.
[0157] Phosphorus (P): 0.05% by weight or less (except 0%)
[0158] The P exists in the steel as an impurity. If the maximum content of the P exceeds 0.05%, the weldability of the hot-formed parts and the physical properties of the material due to high-temperature grain boundary segregation deteriorate, so the upper limit of the P is set to 0.05%. However, considering that the P is inevitably included as an impurity, the lower limit of the P content does not include 0%, or may be 0.5 ppm.
[0159] Sulfur (S): 0.02% by weight or less (except 0%)
[0160] The S, as an impurity, is an element that hinders the ductility, impact properties and weldability of the parts, so the maximum content of the S is limited to 0.02%. However, considering that it is inevitably included as an impurity, the lower limit of the S content does not include 0%, or may be 1 ppm.
[0161] Aluminum (Al): 0.001-1% by weight
[0162] The Al is an element that plays a deoxidizing role with Si in the steelmaking process to improve the cleanliness of steel. If the Al content is less than 0.001%, it is not only difficult to obtain the above-mentioned effect, but also too high a manufacturing process cost is invested in order to control the Al content, so it is not preferred. In addition, if the Al content exceeds 1%, the high-temperature ductility is reduced due to the formation of too many AlN precipitates during the continuous casting process, thereby generating slab cracks and possibly causing manufacturing problems, so the upper limit of the Al content is set to 1%.
[0163] Nitrogen (N): 0.02% by weight or less (except 0%)
[0164] The N is contained in the steel as an impurity. However, if the N content exceeds 0.02%, AlN is formed together with the added Al, and slab cracks are easily generated, so the upper limit of the N content is set to 0.02%. However, considering that the N is inevitably contained as an impurity, the lower limit of the N content does not include 0%, or may be 1 ppm.
[0165] Titanium (Ti): 0.1% or less (including 0%)
[0166] The Ti combines with nitrogen remaining in the steel as an impurity to form TiN, thereby playing a protective role in ensuring that B, which is used to ensure hardenability, does not become a compound. Therefore, the Ti can be selectively added to ensure the above-mentioned effect, and by adding the Ti to form TiC precipitates, precipitation strengthening and grain refinement effects can be expected. However, if the content of the Ti exceeds 0.1%, a large amount of coarse TiN is formed, and the quality of the steel is deteriorated, so the upper limit of the Ti content is set to 0.1%.
[0167] Boron (B): 0.0001-0.01%
[0168] The B is an element that can effectively improve the hardenability and segregates at the original austenite grain boundaries, thereby suppressing the brittleness of the hot-formed parts caused by the grain boundary segregation of impurities P and / or S. However, in order to control the B content to less than 0.0001%, it is necessary to invest too high a process cost, so it is not preferred. In addition, if the B content exceeds 0.01%, due to Fe 23The formation of CB6 complex may induce brittleness during hot rolling, so the upper limit of the B content is set to 0.01%.
[0169] Molybdenum (Mo): 1.00% or less (including 0%)
[0170] The Mo is an element that can effectively improve hardenability and can be selectively included. In order to suppress the problem of excessively high manufacturing cost, the upper limit of the addition amount of the Mo can be 1.00%.
[0171] Vanadium (V): 1.00% or less (including 0%)
[0172] The V is an element that can improve hydrogen embrittlement resistance by reducing grain boundaries by forming carbides, and the V can be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of V added can be 1.00%.
[0173] Calcium (Ca): 0.01% or less (including 0%)
[0174] Ca is an element added in order to improve the cleanliness of steel by removing a specific level of P and S during steelmaking. Ca may be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of Ca added may be 0.01%.
[0175] Niobium (Nb): 0.1% or less (including 0%)
[0176] Nb is an element that can improve hydrogen embrittlement resistance by reducing grain boundaries by forming carbides, and the Nb may be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of Nb added may be 0.1%.
[0177] Tungsten (W): 1% or less (including 0%)
[0178] W is an element that can improve hydrogen embrittlement resistance by forming carbides to refine grain boundaries. W can be selectively included. In order to suppress the problem of excessively high manufacturing costs, the upper limit of the amount of W added can be 1%.
[0179] Rare earth elements (REM): 0.3% or less (including 0%)
[0180] Rare earth metals (REM) are elements that can be included during steelmaking and can be selectively included. However, if the content of rare earth elements exceeds 0.3%, REM will be excessively segregated at the grain boundaries and hydrogen embrittlement resistance may deteriorate, so the content of rare earth elements can be set to 0.3% or less.
[0181] The first group of elements: 0.005-1% by weight
[0182] The base steel plate may further include 0.005 wt % to 1 wt % of one or more first group elements selected from Sb, Sn, As, Bi, Cu, and Ni, each independently.
[0183] When the first group of elements is added, in the coating of the hot press formed part, there may be a region where the concentration of the first group of elements is enriched in the surface area from the interface between the base steel plate and the coating to the coating side direction. With the formation of such a region enriched in the first group of elements, the diffusion rate of aluminum (Al) and iron (Fe) that diffuse mutually during high temperature heat treatment becomes uneven, thereby promoting the formation of Kirkendall voids in the coating after hot press forming. Therefore, if the content of each of the first group of elements is less than 0.005%, the enriched layer cannot be fully formed, and the above-mentioned Kirkendall voids cannot be fully generated, and it may be difficult to expect the effect of improving hydrogen embrittlement resistance. On the other hand, if the content of each of the first group of elements exceeds 1%, not only the cost of the alloy iron increases, but also too many voids are formed in the coating, and the coating peels off due to the stress applied during hot forming, which may cause the coating corrosion resistance to deteriorate.
[0184] In addition, according to one aspect of the present invention, in order to further improve the above-mentioned effects, the first group of elements may include one or more elements selected from Sb, Sn, As and Bi, each independently in an amount of 0.005-0.1%.
[0185] In addition, according to one aspect of the present invention, in order to further improve the above-mentioned effects, the first group of elements may include one or more elements selected from Cu and Ni in an amount of 0.05-1% each independently.
[0186] The balance other than the above components is iron (Fe), and as long as it is a component that can be contained in the steel sheet for hot press forming, there is no particular restriction on further addition. In addition, in the conventional manufacturing process, undesirable impurities may inevitably be mixed from the raw materials or the surrounding environment, and therefore these impurities cannot be excluded. These impurities are well known to those skilled in the art of conventional manufacturing processes, and therefore all of them are not particularly described in this specification.
[0187] In the present invention, the type of the coating is not particularly limited, and any coating that is used for conventional hot-forming plated steel sheets can be used in the present invention without limitation.
[0188] However, as an example, the coating may be an aluminum or aluminum alloy coating, and the coating may preferably contain: Si: 6-12%, Fe: 4% or less (including 0%), the balance of Al and other inevitable impurities.
[0189] Alternatively, as another example, in the case of hot-dip coating, hot-dip aluminum coating, hot-dip Al-Si coating, hot-dip Al-Si-Mg coating, hot-dip Al-Zn coating, hot-dip Al-Mg coating, etc. can be applied. As alloyed hot-dip coating, alloyed hot-dip aluminum coating, alloyed hot-dip Al-Si coating, alloyed hot-dip Al-Si-Mg coating, alloyed hot-dip Al-Zn coating, alloyed hot-dip Al-Mg coating, etc. can be exemplified. The coating may also contain at least one of Mn, Cr, Cu, Mo, Ni, Sb, Sn, Ti, Ca, Sr, Mg, Be, Li, and Na. The coating adhesion amount is not particularly limited, for example, it is set to an adhesion amount within a conventional range.
[0190] In addition, the hot press-formed part may satisfy the following relational expression 2-1.
[0191] [Equation 2-1]
[0192] 9.5≤D B2 / D A2 ≤11.0
[0193] (In the relational expression 2-1, the D B2 D represents the area corresponding to the atomic content ratio of aluminum (Al) in the hot press formed part being 0.25 to 0.45 Fe / D Al The absolute value of D A2 D represents the range in which the atomic content ratio of aluminum (Al) in the hot press formed part is 0.01 to 0.2 Fe / D Al The absolute value of D Fe represents the diffusion rate of iron (Fe), the D Al Indicates the diffusion rate of aluminum (Al).
[0194] In addition, in the region corresponding to the atomic content ratio of aluminum (Al) in the hot press formed part being 0.25 to 0.45 or the region corresponding to the atomic content ratio of aluminum (Al) being 0.01 to 0.2, the diffusion rates (Diffusivity) of iron (Fe) and aluminum (Al) can be obtained by a conventional method known in the technical field using the following relationship A, and therefore, this is not particularly limited in the present invention.
[0195] [Relation A]
[0196]
[0197] (In the above relational expression A, C represents the atomic content ratio of each element in iron (Fe) and aluminum (Al), A is a constant, x represents the depth in the thickness direction from the coating surface to a specific position (cm), and D represents the diffusion rate (cm 2 / second), t represents time (seconds).
[0198] Specifically, as shown in the relation A, a conventional relation for obtaining the diffusion rate (corresponding to "D" in the following relation) is used, and the lnC versus x is plotted for the same time (i.e., under the same conditions as t). 2 The slope of the graph is (-1 / 4×D×t), and the diffusion rate (D) can then be obtained from its slope value.
[0199] The above lnC to x 2 An example of a graph is Figure 4 The detailed method for measuring the diffusion rate is as follows. First, the content change curve of aluminum (Al) and iron (Fe) in the hot press formed parts is measured using glow discharge spectroscopy (GDS). At this time, Figure 4 The portion indicated by “A2” in the graph represents a region corresponding to an atomic content ratio of aluminum (Al) of 0.01 to 0.2 (ie, a region in which the atomic % content of Al is 1-20%).
[0200] in addition, Figure 4 The portion indicated by “B2” indicates a region corresponding to an atomic content ratio of aluminum (Al) of 0.25 to 0.45 (ie, a region in which the atomic % content of Al is 25-45%).
[0201] That is, after measuring the content change curves of each element of Al and Fe, based on the above standards, Figure 4 In A2 and B2, plot lnC versus x for each part. 2 The Al and Fe content diagrams are obtained by measuring the slopes of each element, thereby obtaining the diffusion rate of each element of Al and Fe in the A2 part, and the diffusion rate of each element of Al and Fe in the B2 part can be obtained. Fe / D Al The absolute value of D B2 and D in Part A2 Fe / D Al The absolute value of D A2 , we can get the value D of the relation 2-1 B2 / D A2 When D defined by the relation 2-1 B2 / D A2When the value of is less than 9.5, Kirkendall voids above a certain level cannot be generated, making it difficult to effectively capture hydrogen that penetrates during hot press forming, thereby increasing the amount of diffusible hydrogen in the steel and possibly causing a problem of deterioration in the hydrogen embrittlement resistance of the component. On the other hand, when D defined by the above relational expression 2-1 is B2 / D A2 When the value of exceeds 11.0, excessive Kirkendall voids may be formed, and plating peeling may occur due to stress applied during hot press molding, and corrosion resistance may deteriorate.
[0202] In this manual, D B2 and D A2 represents the diffusion rate of Al and Fe in their respective phases during heat treatment. If the D B2 / D A2 As the value of increases, the generation of Kirkendall voids at the interface between the B2 and A2 parts can be promoted by causing uneven diffusion rates of Fe / Al in the B2 and A2 parts.
[0203] Although not particularly limited, according to one embodiment of the present invention, in the hot press-formed component, the fine structure of the base steel plate may include one or more selected from martensite and bainite, or the fine structure of the base steel plate may also be composed of one or more selected from martensite and bainite.
[0204] Although not particularly limited, according to one embodiment of the present invention, in the coating layer of the hot press-formed part, the average number per unit area of Kirkendall voids having a diameter of 0.5 μm to 5 μm present in a region within 20 μm from the interface between the base steel sheet and the coating layer satisfies 7 / 1000 μm. 2 Up to 100 pieces / 1000μm 2 .
[0205] Kirkendall voids are formed along the coating side direction from the interface between the base iron and the coating generated by the addition of the above-mentioned first group of elements and impurities. Among the Kirkendall voids thus formed, Kirkendall voids of a specific size (i.e., a diameter of 0.5 μm to 5 μm) formed in an area within 20 μm from the interface between the base iron and the coating (toward the coating side direction) play a role in suppressing hydrogen embrittlement that may occur in the parts after hot forming by reducing the amount of diffusible hydrogen that penetrates into the steel during the hot press forming process. That is, Kirkendall voids with a diameter of less than 0.5 μm cannot effectively capture hydrogen absorbed during the heat treatment for hot press forming, so that the improvement effect of hydrogen embrittlement resistance is minimal. In addition, Kirkendall voids with a diameter exceeding 5 μm become defects, causing coating peeling, and due to the peeling of part of the coating during hot forming, the corrosion resistance of the coating is deteriorated.
[0206] Therefore, the inventors have carefully studied and found that excellent hydrogen embrittlement resistance and coating corrosion resistance can be ensured by keeping the average number of Kirkendall voids per unit area of a specific size within an appropriate range. Specifically, if the average number of Kirkendall voids per unit area is less than 8 / 1000 μm 2 If the average number of Kirkendall voids per unit area exceeds 100 / 1000 μm, the diffused hydrogen cannot be sufficiently prevented from penetrating, thereby causing a problem of deterioration in the hydrogen embrittlement resistance of the component. 2 , the stress applied during hot press forming causes the plating to peel off, resulting in a problem of deterioration in the corrosion resistance of the parts.
[0207] According to one aspect of the present invention, in order to further improve the above effect, the lower limit of the average number of Kirkendall voids per unit area may be 10 / 1000 μm 2 , or 18 / 1000μm 2 .
[0208] According to one aspect of the present invention, in order to further improve the above effect, the upper limit of the average number of Kirkendall voids per unit area may be 95 / 1000 μm 2 , or 92 / 1000μm 2 .
[0209] In addition, the same contents as those known in the technical field can be applied to the Kirkendall cavity, and therefore it is not defined separately in this specification.
[0210] In this specification, there is no particular limitation on the method for measuring the average number of Kirkendall voids per unit area, but as an example, measurement can be performed by observing a cross section of the structure (for example, collecting a test piece in a direction perpendicular to the rolling direction) using a scanning electron microscope (SEM).
[0211] At this time, the interface between the base steel sheet and the coating can also be distinguished based on the contrast difference observed by SEM / OM, but can also be distinguished based on component analysis by SEM-EDS, EPMA, etc. That is, when measuring through the base steel sheet-coating by line profile, etc., the interface between the base steel sheet and the coating can be set to a site where the Al content is 2 wt%. If the Al content exceeds 2%, it can be classified as the coating, and if the Al content is 2% or less, it can be classified as the base iron.
[0212] In addition, when a parallel line is drawn at 20 μm from the interface line that distinguishes the interface between the base steel sheet and the coating layer in the coating side direction, as shown in FIG. Figure 2As shown, a portion having a black contrast existing in a region within 20 μm from the interface between the base steel sheet and the plating layer can be identified as a Kirkendall void.
[0213] In the present specification, the diameter of the Kirkendall voids refers to an equivalent circle diameter when an ideal circle having the same area as that of each Kirkendall void is assumed.
[0214] In addition, the method for measuring the average number of Kirkendall voids per unit area is not particularly limited, and can be measured using a conventional method. 2 3 test pieces of the same area, and then measure the 1000 μm 2 The number of Kirkendall voids completely contained in the area of , and then the average number of Kirkendall voids per unit area can be measured by taking their average value. However, the number of the plurality of test pieces can be two or more, so there is no particular limitation on the number.
[0215] Although not particularly limited, according to one embodiment of the present invention, in the hot press-formed component, the base steel plate further includes one or more first group elements selected from Sn, As, Bi, Cu and Ni (i.e., corresponding to X in the following relational expression 2-2), and the hot press-formed component can satisfy the following relational expression 2-2.
[0216] [Equation 2-2]
[0217]
[0218] (In the relational expression 2-2, the X 镀层 represents the average content of X in the coating. 最大 represents the maximum value of the X content in the coating. In addition, the X represents one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni.
[0219] The above X 镀层 and X 最大 is a unit for expressing the content. When calculating the above relational expression 2-2, as long as the units are consistent with each other, there is no particular limitation on the units. As an example, it can be wt%. 镀层 and X 最大 The measuring method is not particularly limited.
[0220] However, as an example, the X 镀层 and X 最大The measurement can be performed by analyzing the change in the content of the first group of elements along the thickness direction of the base steel sheet side from any point on the coating surface using glow discharge spectroscopy (GDS). At this time, it should be noted that for any first group of elements, each element satisfies the value of the relationship 2-2.
[0221] X as the average content of X in the coating 镀层 In the GDS curve, when the area from the coating surface to the interface between the base steel sheet and the coating is divided at the same interval along the thickness direction (for example, the direction perpendicular to the rolling direction), it can be measured by calculating the average value of the X content at each point. At this time, the interface between the base steel sheet and the coating can be determined as a point on the GDS curve where the Al content is 2 wt%.
[0222] According to one embodiment of the present invention, when the hot press formed part fails to satisfy the above relationship 2-2, since the diffusion gradient difference between Fe and Al cannot be sufficiently formed during the hot forming process, it may be difficult to sufficiently promote the formation of Kirkendall voids in the coating layer. Therefore, it is difficult to achieve the effect of reducing the amount of diffusible hydrogen in the steel, and it may be difficult to expect to ensure the effect of the present invention.
[0223] Next, a method for producing a hot press-formed component according to another aspect of the present invention will be described.
[0224] Reheating of slabs
[0225] First, the steel slab is reheated at 1050-1300° C. If the reheating temperature is lower than 1050° C., the slab structure cannot be sufficiently homogenized, so it is difficult to perform resolidification when using precipitated elements. On the other hand, if the reheating temperature exceeds 1300° C., too much oxide layer is formed, resulting in an increase in the manufacturing cost for removing the oxide layer and an increase in the possibility of surface defects after finish rolling.
[0226] Finish rolling
[0227] The reheated steel slab is finished rolled at 800-950°C to obtain a hot rolled steel sheet. If the finishing rolling temperature is lower than 800°C, two-phase rolling is performed, and ferrite is introduced into the surface layer of the steel sheet, making it difficult to control the sheet shape. On the other hand, if the finishing rolling temperature exceeds 950°C, coarsening of hot rolled grains may occur.
[0228] Rolling
[0229] After the finish rolling is terminated, the hot rolled steel sheet is coiled at 500-700°C and then cooled to produce a hot rolled coil. If the coiling temperature is lower than 500°C, the entire or part of the steel sheet forms martensite, which not only makes it difficult to control the shape of the coil, but also causes a problem of reduced subsequent cold rolling performance due to excessive increase in the strength of the hot rolled steel sheet. On the other hand, if the coiling temperature exceeds 700°C, too many coarse carbides are formed, and when stress is generated in the hot formed part, cracks are promoted, so there is a problem of reduced collision resistance.
[0230] Pickling
[0231] The coiled hot-rolled steel sheet is pickled so that the product of the acid concentration and the pickling time is 800-10000 g / L·second. As the steel sheet after the above-mentioned reheating, finish rolling and coiling steps, when the above-mentioned first group of elements is added, the enriched area of the first group of elements is formed in the coating layer, and in the pickling treatment process, when the product of the acid concentration and the pickling time in the range of 800-10000 g / L·second is applied, the formation of the above-mentioned enriched area can be effectively promoted, thereby achieving the effect of reducing the amount of diffusible hydrogen in the steel.
[0232] Specifically, when the product of the acid concentration and the pickling time is less than 800 g / L·second, the scale produced during the finishing rolling process cannot be fully removed, which may cause quality problems of the product. On the other hand, when the product of the acid concentration and the pickling time exceeds 10000 g / L·second, all or part of the enriched area is lost during the pickling process, and the expected effect may not be achieved. In addition, since it may lead to an increase in manufacturing costs, the upper limit of the product of the acid concentration and the pickling time is set to 10000 g / L·second. However, when there is more than one pickling tank and the corresponding acid concentration and pickling time are different, the value can be expressed by adding the product of the acid concentration and the pickling time of each pickling tank.
[0233] According to one aspect of the present invention, the acid that can be used in the pickling treatment step can be applied to an acid that can be conventionally used in the technical field. Representatively, the acid includes hydrochloric acid (HCl), sulfuric acid (H2SO4), etc. In particular, in the present invention, compared with the use of other acids, the pickling ability is excellent and the process cost is economical when hydrochloric acid (HCl) is used, and the possibility of generating surface foreign matter after pickling is small, so that the surface quality is easily ensured.
[0234] In addition, although not particularly limited, according to one aspect of the present invention, the concentration of the acid may be in the range of 40-500 g / L. If the concentration of the acid is less than 40 g / L, the surface oxide scale generated during the hot rolling process cannot be fully removed within the limited pickling time, and defects may be generated on the surface of the steel plate. On the other hand, if the concentration of the acid exceeds 500 g / L, it may be difficult to exert the desired effect of the invention in the final hot press-formed part due to the loss of the enriched area, and defects in the surface portion caused by over-pickling may be caused.
[0235] In addition, although not particularly limited, according to one aspect of the present invention, the pickling time may be 5-60 seconds. If the pickling time is less than 5 seconds, the surface scale of the steel plate cannot be fully removed, which may cause surface defects. If the pickling time exceeds 60 seconds, the productivity is reduced due to the loss of the enriched area, which may increase the process cost.
[0236] In addition, although not particularly limited, according to one aspect of the present invention, the pickling temperature may be 40-120°C, and more preferably may be 50-100°C. If the pickling temperature is lower than 40°C, the pickling force is insufficient, which may adversely affect the quality of the product. On the other hand, if the pickling temperature exceeds 120°C, not only the fixed cost for maintaining the high temperature is increased, but also due to the high temperature, the vaporization amount of the pickling solution increases, and there may be a problem of increased cost for replenishing the lost pickling solution.
[0237] Continuous annealing
[0238] The pickled steel sheet is continuously annealed, and the average heating rate of each zone is controlled to satisfy the following equations 1 to 3.
[0239] [Formula 1]
[0240] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec
[0241] [Formula 2]
[0242] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec
[0243] [Formula 3]
[0244] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec
[0245] (In the above formula 1, the first zone refers to the interval until the surface temperature of the steel plate reaches 500°C, the second zone refers to the interval from 500°C to 700°C, and the third zone refers to the interval until the surface temperature of the steel plate reaches the maximum temperature.)
[0246] In the present invention, by performing continuous annealing so that the average heating rate of each zone during the continuous annealing satisfies Formulas 1 to 3, the added first group of elements can be effectively diffused into the coating area in contact with the base steel plate, thereby effectively forming and promoting the enrichment area of the first group of elements.
[0247] During the continuous annealing, each zone can be divided based on the surface temperature of the steel plate. The interval from the starting point (normal temperature) until the surface temperature of the steel plate reaches 500°C can be defined as the first zone. Then, the temperature interval from 500°C to 700°C can be defined as the second zone. In addition, the temperature interval from 700°C to the maximum annealing target temperature desired by the steel plate can be defined as the third zone. That is, by making the annealing temperature condition from the starting point to the maximum annealing target temperature satisfy the above formulas 1 to 3, the first group of elements as the added elements for enrichment are fully enriched in the surface part, thereby ensuring excellent hydrogen embrittlement resistance after the heat treatment for hot forming. Specifically, by rapidly increasing the average heating rate of the first zone, the time of keeping at high temperature can be further ensured, and since the diffusion rate of the enriched elements to the coating area in contact with the base steel plate at high temperature is fast, the surface enriched elements can be fully formed in the hot pressed part after annealing. At this time, the first zone to the third zone may be arranged sequentially in the conveying direction of the steel plate.
[0248] For the average heating rate of each zone, the surface temperature of the steel plate can be measured by the non-contact heat treatment temperature in the middle or end of each zone, but it is not limited to this. If the surface temperature of the steel plate at each measurement position and the plate passing time according to the line speed are known, the average heating rate of each zone can be obtained by inverse calculation.
[0249] In addition, during the continuous annealing, control is performed so that the heat treatment area at 700° C. or above is 5000° C.·second to 25000° C.·second in terms of time.
[0250] In the present invention, the pickled steel sheet needs to be heat treated in the continuous annealing step so that the maximum temperature of the steel sheet exceeds 700°C, and Figure 3 As shown, the heat treatment area (i.e., corresponding to Figure 3 The "surface enrichment heat treatment area" must meet the range of 5000℃·sec or more and 25000℃·sec or less. As a result, the added first group of elements can be effectively diffused into the coating area in contact with the base steel sheet, so the enrichment area of the first group of elements can be effectively formed and promoted.
[0251] If the heat treatment area according to the time (i.e., the surface enrichment heat treatment area) is less than 5000°C·second, the enrichment layer of the added first group of elements cannot be fully enriched in the surface part, and thus the effects of the invention, such as improving hydrogen embrittlement resistance after hot forming, may not be achieved. If the heat treatment area according to the time exceeds 25000°C·second, not only the process cost and time for continuous annealing are increased, but also the plating property is deteriorated, and uneven or no plating may occur.
[0252] Plating
[0253] The steel sheet after the continuous annealing can be plated. As an example, the steel sheet can be immersed in a plating bath composed of aluminum or an aluminum alloy for plating. At this time, the plating bath can be an aluminum plating bath or an aluminum-based plating bath, for example, an Al-Si plating bath. Specifically, after annealing, a plated steel sheet can be manufactured by passing the hot-rolled steel sheet through a plating bath composed of aluminum or an aluminum alloy. At this time, the plating conditions can be applied to the present invention without restriction as long as they are the plating conditions commonly applied to steel sheets for hot press forming, but as an example, the composition of the plating bath can include Si: 6-12%, Fe: 4% or less (including 0%), the remainder of Al and other inevitable impurities.
[0254] At this time, although not particularly limited, the plating amount in the plating step can be set to 20-140 g / m 2 If the coating weight on one side is less than 20g / m 2 If the coating weight on one side exceeds 140 g / m2, it may be difficult to ensure the corrosion resistance required for hot-formed parts. 2 , the manufacturing cost increases due to excessive plating adhesion, and it may be difficult to plate the coating uniformly over the entire width and length of the coil.
[0255] Cold Rolling
[0256] According to one aspect of the present invention, after the pickling treatment, the method may further include cold rolling the hot-rolled steel sheet to produce a cold-rolled steel sheet.
[0257] Hot Press Forming
[0258] A method for manufacturing a final component having excellent hydrogen embrittlement resistance and collision resistance by hot forming and die quenching using a coated steel sheet manufactured by the above method is described. A slab for hot forming is manufactured using a coated steel sheet manufactured according to the composition and manufacturing method of the above steel. The slab is heated above the austenite single phase region temperature, more specifically, within a temperature range of above the Ac3 temperature and below 975°C. At this time, if the heating temperature is lower than the Ac3 temperature, it is difficult to ensure strength and collision resistance due to the presence of untransformed ferrite according to the two-phase region. On the other hand, if the heating temperature exceeds 975°C, too much oxide is generated on the surface of the component, it is difficult to ensure spot weldability, and the manufacturing cost for maintaining high temperature increases. On the other hand, the Ac3 temperature can be similarly defined as known in the technical field, so it is not defined separately in the present invention.
[0259] Then, the heated slab is preferably kept in the above temperature range for 1-1000 seconds. If the holding time is less than 1 second, it is difficult to achieve uniform temperature distribution throughout the slab temperature, which may cause material deviation at each position. On the other hand, if the holding time exceeds 1000 seconds, as in the case of exceeding the heating temperature, it is difficult to ensure spot weldability due to excessive oxides generated on the surface of the component, and the manufacturing cost of the component increases.
[0260] In addition, although not particularly limited, according to one aspect of the present invention, the heated slab is conveyed to a press machine, and hot forming and die quenching may be performed at a cooling rate of 20°C / sec or more. At this time, if the cooling rate is less than 20°C / sec, a ferrite phase is introduced during the cooling process and generated at the grain boundary, which may reduce strength and collision resistance. There is no particular limitation on the conveying, hot press forming and cooling steps of the slab, and a conventional hot press forming method may be directly applied. DETAILED DESCRIPTION
[0261] The present invention is described in more detail below by way of examples. However, it should be noted that the following examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. This is because the scope of the present invention is determined by the contents described in the claims and the contents reasonably derived therefrom.
[0262] (Experimental Example 1)
[0263] A steel billet having a thickness of 40 mm was manufactured by vacuum melting, and the steel billet had a composition of 0.22% C, 0.2% Si, 1.2% Mn, 0.03% Al, 0.01% P, 0.002% S, 0.03% Ti, and 0.004% N in weight %, and the first group of elements were added as additional elements as shown in Table 1 below.
[0264] This slab was kept at 1200°C for 1 hour, then hot rolled at a hot rolling end temperature of 900°C, and coiled at a coiling temperature of 600°C. Then, cold rolling including a pickling process was performed. Next, the cold-rolled steel sheet obtained by cold rolling was sequentially subjected to pickling treatment, continuous annealing, and plating. At this time, the pickling conditions within the scope of the present invention and the continuous annealing conditions for each zone were applied. More specifically, the HCl concentration × pickling time was 4000 g / L. The annealing conditions for each zone used in the annealing were all as follows: formula (1): 3.0°C / second, formula (2): 0.5°C / second, and formula (3): 0.3°C / second.
[0265] Then, the plated film was immersed in a plating bath composed of 9% Al, 2% Si, Fe and the balance of trace impurities. In addition, in this embodiment, after applying a temperature of 930°C and a heating time of 6 minutes, the transport time to the mold was applied for 10 seconds, and then hot forming and mold quenching were applied.
[0266] In order to confirm whether the enrichment layer in the test piece prepared as described above is fully formed on the surface of the substrate layer, GDS850A (model name, manufactured by LECO), DC and RF equipment are used, and glow discharge spectroscopy (GDS; Glow Discharge Optical Emission Spectrometry) is used to analyze the content of the first group of elements shown in Table 1.
[0267] Refer to the GDS analysis results and measure the X of each first group element. 最大 and X 镀层 The weight % content was calculated and the ratio was shown in the following Table 1.
[0268] In addition, in order to confirm the Kirkendall voids within 20 μm in the coating direction, an electron microscope (scanning electron microscope (SEM)) was used to observe the cross section of the structure (the test piece was collected in the direction perpendicular to the rolling direction). The photographs thus observed were taken at a magnification of ×1000, such as Figure 1 (Measurement of the hot press formed part obtained in Example 1) shows that the portion with black contrast existing in the interior of the range can be identified as Kirkendall voids. Applying this magnification, and wrapping with a rectangle of 20 μm thickness × 50 μm length, the average number of Kirkendall voids confirmed in the range is measured and defined as the number / 1000 μm. 2 , and the results are shown in Table 1.
[0269] In order to evaluate the amount of diffusible hydrogen in materials having various Kirkendall voids, a thermal desorption analysis (TDA) device (Bruker G8: model name) was used for measurement. The conditions for analyzing the amount of diffusible hydrogen are to increase the temperature to 400°C at 20°C / min and measure the diffusible hydrogen curve by maintaining the time for the diffusible hydrogen peak to appear sufficiently. The total amount of diffusible hydrogen in the steel can be obtained by integrating these curves, and the results are shown in Table 1.
[0270] Then, in order to confirm the influence of Kirkendall voids in the coating on the corrosion resistance of the coating, after forming a scratch (Scribe) of w 0.5×L50mm, a 10-cycle corrosion resistance test (test) was performed according to the VDA233-102 standard, and then the peeling width of the corrosion part around the scratch was measured according to the ISO4628-8 standard. At this time, in the following Table 1, if the measured peeling width meets 2.5mm or less, it is marked as "good", and if the measured peeling width exceeds 2.5mm, it is marked as "bad".
[0271] [Table 1]
[0272]
[0273] As shown in Table 1, the amount of diffusible hydrogen changes as the average number per unit area of Kirkendall voids having a major axis of 0.5 μm to 5 μm existing in a region within 20 μm from the interface between the base steel sheet and the coating layer changes.
[0274] At this time, in the coating layer, the average number per unit area of Kirkendall voids having a major diameter of 0.5 μm to 5 μm existing in a region within 20 μm from the interface between the base steel sheet and the coating layer satisfies 8 / 1000 μm. 2 Up to 100 pieces / 1000μm 2 In the case of Examples 1 to 18, the amount of diffusible hydrogen in the hot press formed parts was 0.2 ppm or less, and it was confirmed that the parts had excellent hydrogen embrittlement resistance and good coating corrosion resistance.
[0275] In addition, further, for Examples 1 to 18, in the coating layer, it was also confirmed that the average number per unit area of Kirkendall voids with a major diameter of 2 μm to 6 μm existing in the region within 20 μm from the interface between the base steel plate and the coating layer satisfied 10 / 1000 μm. 2 Up to 100 pieces / 1000μm 2 .
[0276] In addition, the average number of Kirkendall voids having a major diameter of 0.5 μm to 5 μm present in a region within 20 μm from the interface between the base steel sheet and the coating layer is less than 8 per 1000 μm. 2 In the case of Comparative Examples 1, 3, 5, 7, 9 and 11, the hydrogen absorbed during the hot press forming process cannot be well captured, so the amount of diffused hydrogen exceeds 0.2 ppm, making it difficult to ensure hydrogen embrittlement resistance.
[0277] Even if the composition of the present invention is satisfied, the average number per unit area of Kirkendall voids having a major diameter of 0.5 to 5 μm existing in a region within 20 μm from the interface between the base steel sheet and the coating layer exceeds 100 / 1000 μm. 2 In the case of Comparative Examples 2, 4, 6, 8, 10 and 12, the amount of diffusible hydrogen was reduced. However, due to the formation of too many Kirkendall voids, the interfacial bonding strength of the coating was weakened, and part of the coating peeled off during hot forming or coating scribing, so that the corrosion resistance of the coating was excessively deteriorated and defects occurred.
[0278] (Experimental Example 2)
[0279] The main components of the composition of the steel used in the present invention include: C: 0.22%, Si: 0.25%, Mn: 1.25%, Cr: 0.2%, Al: 0.03%, P: 0.01%, S: 0.002%, Ti: 0.03%, B: 0.0025%, N: 0.004%. As shown in Table 2 below, a base steel plate to which various first group elements are added is prepared, and a slab with a thickness of 40 mm having each composition is manufactured by vacuum melting. This slab is kept at a temperature of 1200°C for 1 hour, then hot rolled at a hot rolling end temperature of 900°C, and coiled at a coiling temperature of 600°C. Next, the cold-rolled steel sheet obtained by cold rolling is sequentially subjected to pickling treatment, continuous annealing, and plating. At this time, the pickling conditions within the scope of the present invention and the continuous annealing conditions of each zone are applied. More specifically, the HCl concentration×pickling time is 4000 g / L·second (wherein, the pickling is carried out with an HCl concentration of 200 g / L and a pickling time of 20 seconds, and the pickling temperature is all 80°C), and the annealing conditions of each zone for annealing are all applied: first zone: 3.0°C / second, second zone: 0.5°C / second, third zone: 0.3°C / second.
[0280] In addition, during the plating, the plate is plated by immersing in a plating bath consisting of 9% Al, 2% Si, Fe, and the balance being trace amounts of impurities.
[0281] Then, hot press forming is performed after heat treatment at Ac3 to 950°C, where the heating time is 6 minutes, the conveying time to the mold is 10 seconds, and then the mold is quenched.
[0282] In order to confirm the Kirkendall voids within 20 μm in the coating direction, an electron microscope (scanning electron microscope (SEM)) was used to observe the cross section of the structure (the test piece was collected in the direction perpendicular to the rolling direction). The photographs thus observed were taken at a magnification of ×1000, such as Figure 2 (Measurement of hot press molded parts) shows that the portion with black contrast existing inside the range can be identified as Kirkendall voids. Applying this magnification, and wrapping with a rectangle of 20 μm thickness × 50 μm length, the average number of Kirkendall voids confirmed in the range is measured and defined as the number / 1000 μm. 2 , and the results are shown in the table.
[0283] In order to evaluate the amount of diffusible hydrogen in materials having various Kirkendall voids, a thermal desorption analysis (TDA) device (Bruker G8: model name) was used for measurement. The amount of diffusible hydrogen was measured 3 days after the hot forming heat treatment. The conditions for analyzing the amount of diffusible hydrogen were to increase the temperature to 400°C at 20°C / min and measure the diffusible hydrogen curve by maintaining the time for which the diffusible hydrogen peak appears sufficiently. The total amount of diffusible hydrogen in the steel can be obtained by integrating these curves, and the results are shown in the table.
[0284] In addition, in order to evaluate hydrogen embrittlement resistance, bending stress was applied to a test piece with a width of 14.5 mm and a length of 73 mm, and a strain of 0.7% was applied to the entire outermost ring. Then, the fracture time after immersion in 0.1N hydrochloric acid was measured. When the test piece did not fracture for more than 120 hours, it was considered good, and when the test piece fractured in less than 120 hours, it was considered poor.
[0285] In order to confirm whether the enrichment layer in the test piece prepared as described above is fully formed on the surface of the substrate layer, GDS850A (model name, manufactured by LECO), DC and RF equipment are used, and the content of the first group of elements shown in Table 2 is analyzed by glow discharge spectroscopy (GDS).
[0286] In addition, in order to evaluate the adhesion of the electrodeposition coating, the ISO2409 standard was applied, and a 10×10 (1 mm wide) grid was cut on the coated surface with a blade, and the adhesion test tape was placed parallel to the grid pattern and peeled off after lamination, and then the area of the peeled coating layer was observed using a magnifying glass. At this time, when the separated area is less than 5% of the grid area, it is evaluated as good, and when the separated area is more than 5% of the grid area, it is evaluated as poor, and is shown in the following Table 2.
[0287] [Table 2]
[0288]
[0289] As can be seen from the results in Table 2, in the case of Examples 2-1 to 2-12 satisfying Relational Expression 2-1 according to the present invention, it was confirmed that the hydrogen embrittlement resistance was excellent due to the reduction in the amount of diffusible hydrogen, and the electrodeposition coating adhesion was also excellent.
[0290] In addition, in the case of Comparative Examples 2-1 to 2-15 that do not satisfy the relational expression 2-1, it was confirmed that one or more characteristics of hydrogen embrittlement resistance and electrodeposition coating adhesion were inferior compared to the examples.
[0291] In addition, although not particularly limited, in the case of the additional Examples 2-2, 2-3, 2-5, 2-6, 2-8, 2-9, 2-11 and 2-12, the average number per unit area of Kirkendall voids having a diameter of 2 μm to 6 μm present in the region of the coating within 20 μm from the interface between the base steel sheet and the coating along the coating side direction satisfies 10 / 1000 μm. 2 Up to 100 pieces / 1000μm 2 In addition, referring to the GDS analysis results, when measuring the X of each first group element 最大 and X 镀层 When the weight % content is , it is confirmed that the above-mentioned Examples 2-2, 2-3, 2-5, 2-6, 2-8, 2-9, 2-11, and 2-12 satisfy the relationship 2-2.
[0292] [Explanation of Reference Numerals]
[0293] 11: Kirkendall Hollow
[0294] 100: Interface between base steel plate and coating
Claims
1. A hot press formed part, include: Base steel plate; as well as a coating, wherein the coating is provided on at least one side of the base steel plate, The average number of Kirkendall voids per unit area having a major diameter of 0.5 μm to 5 μm in the region of the coating layer within 20 μm from the interface between the base steel sheet and the coating layer satisfies 8 / 1000 μm. 2 Up to 100 pieces / 1000μm 2 .
2. The hot press formed part according to claim 1, in, The average number of Kirkendall voids per unit area satisfies 10 / 1000 μm 2 Up to 95 / 1000μm 2 .
3. The hot press formed part according to claim 1, in, The average number of Kirkendall voids per unit area satisfies 18 / 1000 μm 2 Up to 92 pieces / 1000μm 2 .
4. The thermoformed component according to claim 1, in, The base steel plate comprises, by weight%, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less and excluding 0%, S: 0.02% or less and excluding 0%, N: 0.02% or less and excluding 0%, Ti: 0.1% or less and including 0%, B: 0.0001-0.01%, Mo: 1.00% or less and including 0%, V: 1.00% or less and including 0%, Ca: 0.01% or less and including 0%, Nb: 0.1% or less and including 0%, W: 1% or less and including 0%, REM: 0.3% or less and including 0%, and the balance of Fe and other inevitable impurities.
5. The thermoformed component according to claim 1, in, The base steel plate further includes 0.005-1 wt % of each of the first group of elements independently selected from the group consisting of Sb, Sn, As, Bi, Cu and Ni.
6. The thermoformed component according to claim 1, in, The base steel plate further comprises one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni, The first group of elements includes one or more elements selected from Sb, Sn, As and Bi in an amount of 0.005-0.1% each independently. The first group of elements includes one or more elements selected from Cu and Ni, each independently accounting for 0.05-1%.
7. The thermoformed component according to claim 1, in, The base steel plate further comprises one or more first group elements selected from Sn, As, Bi, Cu and Ni, and the hot press formed part satisfies the following relational expression 1: [Equation 1] In the relational expression 1, the X 镀层 represents the average content of X in the coating, in units of weight%; the X 最大 represents the maximum value of the X content in the coating layer, and the unit is % by weight, wherein X represents one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni.
8. The thermoformed component according to claim 1, in, The average number per unit area of Kirkendall voids having a major diameter of 2 to 6 μm in a region of the coating layer within 20 μm from the interface between the base steel sheet and the coating layer satisfies 10 / 1000 μm 2 Up to 100 pieces / 1000μm 2 .
9. A method for manufacturing a thermoformed part, wherein The following steps are involved: The steel billet is reheated at 1050-1300° C., and the steel billet contains, in terms of weight %, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less and excluding 0%, S: 0.02% or less and excluding 0%, N: 0.02% or less and excluding 0%, Ti: 0.1% or less and including 0%, B: 0.0001-0.01%, Mo: 1.00% or less and including 0%, V: 1.00% or less and including 0%, Ca: 0.01% or less and including 0%, Nb: 0.1% or less and including 0%, W: 1% or less and including 0%, REM: 0.3% or less and including 0%, and the balance of Fe and other inevitable impurities; The reheated steel slab is finish rolled at 800-950°C to obtain a hot rolled steel plate; The hot rolled steel sheet is coiled at 500-700° C. The hot rolled steel sheet is pickled to make the product of the acid concentration and the pickling time be 800-10000 g / L. Second; The pickled steel plate is continuously annealed while controlling the average heating rate of each zone to satisfy the following equations 1 to 3; immersing the continuously annealed steel sheet in a plating bath composed of aluminum or an aluminum alloy for plating; and The plated steel sheet is heat treated at Ac3 to 950°C for 1 to 1000 seconds and then hot-pressed. [Formula 1] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec [Formula 2] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec [Formula 3] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec In Formula 1, the first zone refers to a range until the surface temperature of the steel plate reaches 500° C., the second zone refers to a range from 500° C. to 700° C., and the third zone refers to a range until the surface temperature of the steel plate reaches the maximum temperature.
10. A thermoformed component, include: Base steel plate; as well as a coating, wherein the coating is provided on at least one side of the base steel plate, Wherein, the hot press formed part satisfies the following relational expression 2-1: [Equation 2-1] 9.5≤D B2 / D A2 ≤11.0 In the relational expression 2-1, D B2 D represents the area corresponding to the atomic content ratio of aluminum (Al) in the hot press formed part being 0.25 to 0.45 Fe / D Al The absolute value of D A2 D represents the range in which the atomic content ratio of aluminum (Al) in the hot press formed part is 0.01 to 0.2 Fe / D Al The absolute value of D Fe represents the diffusion rate of iron (Fe), the D Al Indicates the diffusion rate of aluminum (Al).
11. The thermoformed component according to claim 10, in, The microstructure of the base steel plate is composed of one or more selected from martensite and bainite.
12. The thermoformed component according to claim 10, in, The average number of Kirkendall voids having a diameter of 0.5 μm to 5 μm in a region within 20 μm from the interface between the base steel sheet and the coating layer in the coating layer side direction satisfies 7 per 1000 μm. 2 Up to 100 pieces / 1000μm 2 .
13. The thermoformed component according to claim 12, in, The average number of Kirkendall voids per unit area satisfies 10 / 1000 μm 2 Up to 95 / 1000μm 2 .
14. The thermoformed component according to claim 12, in, The average number of Kirkendall voids per unit area satisfies 18 / 1000 μm 2 Up to 92 pieces / 1000μm 2 .
15. The thermoformed component according to claim 10, in, The base steel plate comprises, by weight%, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less and excluding 0%, S: 0.02% or less and excluding 0%, N: 0.02% or less and excluding 0%, Ti: 0.1% or less and including 0%, B: 0.0001-0.01%, Mo: 1.00% or less and including 0%, V: 1.00% or less and including 0%, Ca: 0.01% or less and including 0%, Nb: 0.1% or less and including 0%, W: 1% or less and including 0%, REM: 0.3% or less and including 0%, and the balance of Fe and other inevitable impurities.
16. The thermoformed component according to claim 10, in, The base steel plate contains 0.005 wt % to 1 wt % of one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni, each independently.
17. The thermoformed component according to claim 10, in, The base steel plate contains one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni, The first group of elements includes one or more elements selected from Sb, Sn, As and Bi in an amount of 0.005-0.1% each independently. The first group of elements includes one or more elements selected from Cu and Ni, each independently accounting for 0.05-1%.
18. The thermoformed component according to claim 10, in, The base steel plate further comprises one or more first group elements selected from Sn, As, Bi, Cu and Ni, and the hot press formed part satisfies the following relational expression 2-2: [Equation 2-2] In the relational expression 2-2, X 镀层 represents the average content of X in the coating, in units of weight%; the X 最大 represents the maximum value of the X content in the coating layer, and the unit is % by weight, wherein X represents one or more first group elements selected from Sb, Sn, As, Bi, Cu and Ni.
19. The thermoformed component according to claim 10, in, The average number of Kirkendall voids having a diameter of 2 to 6 μm in the coating layer within 20 μm from the interface between the base steel sheet and the coating layer in the coating layer side direction satisfies 10 per 1000 μm. 2 Up to 100 pieces / 1000μm 2 .
20. A method for manufacturing a hot press formed component, wherein The following steps are involved: The steel billet is reheated at 1050-1300° C., and the steel billet contains, in terms of weight %, C: 0.02-0.5%, Si: 0.001-2%, Al: 0.001-1%, Mn: 0.1-4%, P: 0.05% or less and excluding 0%, S: 0.02% or less and excluding 0%, N: 0.02% or less and excluding 0%, Ti: 0.1% or less and including 0%, B: 0.0001-0.01%, Mo: 1.00% or less and including 0%, V: 1.00% or less and including 0%, Ca: 0.01% or less and including 0%, Nb: 0.1% or less and including 0%, W: 1% or less and including 0%, REM: 0.3% or less and including 0%, and the balance of Fe and other inevitable impurities; The reheated steel slab is finish rolled at 800-950°C to obtain a hot rolled steel plate; The hot rolled steel sheet is coiled at 500-700° C. The coiled hot-rolled steel sheet is pickled so that the product of the acid concentration and the pickling time is 800-10000 g / L·second; The pickled steel plate is continuously annealed while controlling the average heating rate of each zone to satisfy the following equations 1 to 3; immersing the continuously annealed steel sheet in a plating bath composed of aluminum or an aluminum alloy for plating; and The plated steel sheet is heat treated at Ac3 to 950°C for 1 to 1000 seconds and then hot-pressed. Wherein, during the continuous annealing, the heat treatment area at 700°C or above satisfies 5000°C·second to 25000°C·second according to the time, [Formula 1] 1.5℃ / sec≤Average heating rate of the first zone (℃ / sec)≤10.0℃ / sec [Formula 2] 0.5℃ / sec≤Average heating rate of the second zone (℃ / sec)≤1.0℃ / sec [Formula 3] 0.01℃ / sec≤Average heating rate of the third zone (℃ / sec)≤0.4℃ / sec In Formula 1, the first zone refers to a range until the surface temperature of the steel plate reaches 500° C., the second zone refers to a range from 500° C. to 700° C., and the third zone refers to a range until the surface temperature of the steel plate reaches the maximum temperature.