Electroplating system and method with increased metal ion concentration

By conditioning anolyte and catholyte at elevated temperatures and forming precursors, the method addresses the inefficiencies in maintaining high metal ion concentrations, improving deposition rates and throughput in electroplating systems.

CN119072560APending Publication Date: 2024-12-03APPLIED MATERIALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380035956.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-03
Filing Date
2023-04-04
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Conventional electroplating systems face challenges in maintaining high metal ion concentrations in the catholyte solution while avoiding the reduction in transport rate due to increased acidity in the anolyte, leading to inefficiencies and complexity in replacing consumable anodes.

Method used

The method involves conditioning anolyte and catholyte at elevated temperatures and forming anolyte and catholyte precursors, which are then mixed with diluents to achieve higher metal ion concentrations, reducing the need for complex equipment and maintaining high metal ion concentrations in the electroplating process.

Benefits of technology

This approach allows for increased metal ion concentrations in the electroplating process, enhancing the deposition rate and throughput without the need for complex equipment, thus improving the efficiency and reducing system downtime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072560A_ABST
    Figure CN119072560A_ABST
Patent Text Reader

Abstract

An electroplating method may include providing an electrolyte feedstock to a first compartment of an electrochemical cell, the electrolyte feedstock including copper. These methods may include providing an acidic solution to a second compartment of the electrochemical cell. The first compartment and the second compartment may be separated by a diaphragm. These methods may include applying a current to an anode of an electrochemical cell. An anode of the electrochemical cell may be disposed adjacent the first compartment and opposite the diaphragm. The methods may include forming anolyte and catholyte precursors.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of and priority to U.S. Patent Application No. 63 / 327,264, filed on April 4, 2022, entitled “ELECTROPLATING SYSTEMS AND METHODS WITH INCREASED METAL ION CONCENTRATIONS,” which is hereby incorporated by reference in its entirety. Technical Field

[0003] The present technology relates to electroplating operations in semiconductor processing. More particularly, the present technology relates to systems and methods for performing enrichment and replenishment of an electroplating system. Background Art

[0004] Integrated circuits can be manufactured by processes that create alternating patterned layers of material on a substrate surface. After formation, etching, and other processing on the substrate, metal or other conductive materials are often deposited or formed to provide electrical connections between components. Because this metallization can be performed after many manufacturing operations, problems caused during metallization can result in expensive scrapped substrates or wafers.

[0005] Electroplating is performed in a plating chamber, where the device side of the wafer is in a liquid electrolyte bath, and the electrical contacts on the contact ring contact the conductive layer on the surface of the wafer. Current passes through the electrolyte and the conductive layer. Metal ions in the electrolyte plate out onto the wafer, producing a metal layer on the wafer. Plating chambers generally have consumable anodes, which are advantageous for bath stability and cost of ownership. For example, copper consumable anodes are commonly used when electroplating copper. Copper ions removed from the plating bath are replenished by copper removed from the anode, thereby maintaining the metal ion concentration in the plating bath. Although efficient in replacing the plated metal ions, the use of consumable anodes requires a more complex and expensive design to allow the consumable anodes to be replaced. Even more complexity is added when the consumable anode is combined with a diaphragm to avoid reducing the quality of the electrolyte, or when the consumable anode is oxidized during idle state operation.

[0006] Therefore, there is a need for improved systems and methods that can be used to produce high quality devices and structures while protecting both the substrate and the electroplating bath. The present technology can address these and other needs. Summary of the invention

[0007] Embodiments of the present technology may include electroplating methods. These methods may include providing a first portion of an electrolyte raw material to a first compartment of an electrochemical cell, the electrolyte raw material including copper. These methods may include providing a second portion of the electrolyte raw material or an acidic solution to a second compartment of the electrochemical cell. The first compartment and the second compartment may be separated by a diaphragm. These methods may include supplying current to an anode of the electrochemical cell. The anode of the electrochemical cell may be disposed adjacent to the first compartment and opposite to the diaphragm. These methods may include forming an anode electrolyte and a cathode electrolyte precursor.

[0008] In some embodiments, the electrolyte raw material may be characterized by a copper ion concentration of less than or about 50.0 g / L. The acidic solution may be characterized by an acid concentration of less than or about 110.0 g / L. The anolyte and cathode electrolyte precursors may be characterized by a copper ion concentration of greater than or about 70.0 g / L. These methods may include forming the anolyte by mixing the anolyte and cathode electrolyte precursors with a diluent. The diluent may be or include deionized water. The anolyte may be characterized by a copper ion concentration of greater than or about 60.0 g / L. The anolyte may be characterized by an acid concentration of less than or about 20.0 g / L. These methods may include forming the cathode electrolyte by mixing the anolyte and cathode electrolyte precursors with additional electrolyte raw materials and evaporating water. The cathode electrolyte may be characterized by a copper ion concentration of greater than or about 60.0 g / L. The cathode electrolyte may be characterized by an acid concentration of greater than or about 90.0 g / L. When forming the anolyte and cathode electrolyte precursors, the temperature may be maintained at greater than or about 40°C. These methods may include removing a portion of the acidic solution from the second compartment and replacing it with a new acidic solution. This new acidic solution can maintain the hydrogen ion concentration in the second compartment. These methods can include providing additional electrolyte raw material or additional acidic solution to a third compartment of the electrochemical cell. The second compartment and the third compartment can be separated by a diaphragm. The first compartment and the second compartment of the electrochemical cell can be existing electroplating chamber compartments.

[0009] Embodiments of the present disclosure may include electroplating methods. These methods may include providing an electrolyte raw material to a first compartment and a second compartment of an existing electroplating chamber. The first compartment and the second compartment may be separated by a diaphragm. These methods may include applying an electric current to an anode, which is located in the existing electroplating chamber. The anode may be disposed near the first compartment and opposite to the diaphragm. These methods may include increasing the concentration of copper ions in the electrolyte raw material in the first compartment to form a cathode electrolyte. These methods may include directing the cathode electrolyte to a storage tank, which is fluidly connected to the existing electroplating chamber. These methods may include providing a diluted electrolyte raw material to the first compartment. These methods may include increasing the concentration of copper ions in the electrolyte raw material in the first compartment to form an anode electrolyte.

[0010] In some embodiments, the methods may include directing a cathode electrolyte from a storage tank to a cathode electrolyte tank after forming the anode electrolyte. The methods may include directing an anode electrolyte from a first compartment to an anode electrolyte tank. The methods may include converting the existing electroplating chamber to a production mode after forming the anode electrolyte. The cathode electrolyte and the anode electrolyte may each be characterized by a copper ion concentration greater than or about 65.0 g / L. The current applied to the anode of the existing electroplating chamber may be greater than or about 40 amperes. The temperature may be maintained at greater than or about 40° C. while forming the cathode electrolyte and the anode electrolyte. The existing electroplating chamber may be operated to electroplate copper material from the cathode electrolyte onto a substrate.

[0011] Embodiments of the present disclosure may include electroplating methods. These methods may include converting an existing electroplating chamber from a production mode to an up concentration mode. These methods may include providing an electrolyte feedstock to a first compartment and a second compartment of the existing electroplating chamber. The first compartment and the second compartment are separated by a diaphragm. These methods may include applying an electric current to an anode, the anode being located in the existing electroplating chamber. The anode may be disposed adjacent to the first compartment and opposite to the diaphragm. These methods may include increasing the concentration of copper ions in the electrolyte feedstock in the first compartment to form a cathode electrolyte. These methods may include directing the cathode electrolyte to a storage tank, the storage tank being fluidically connected to the existing electroplating chamber. These methods may include providing a dilute electrolyte feedstock to the first compartment. These methods may include increasing the concentration of copper ions in an anode electrolyte precursor to form an anode electrolyte. These methods may include converting the existing electroplating chamber from an up concentration mode to a production mode.

[0012] In some embodiments, the cathode electrolyte and the anode electrolyte can each be characterized by a copper ion concentration of greater than or about 65.0 g / L.

[0013] This technique can provide several advantages over conventional techniques. For example, the present technique can generate and maintain an electroplating operation at a high metal ion concentration, thereby increasing the rate of electroplating of the metal on the substrate. In addition, by forming the anolyte and catholyte precursors, the present technique can reduce the amount of the initial solution containing metal ions required to increase the metal ion concentration in the cathode electrolyte of the electroplating bath. These and other embodiments and many of their advantages and features are described in more detail in conjunction with the following description and the accompanying figures.

[0014] BRIEF DESCRIPTION OF THE DRAWINGS

[0015] A further understanding of the nature and advantages of the disclosed embodiments may be obtained by referring to the remaining portions of the specification and the accompanying drawings.

[0016] Figure 1Depicted are exemplary operations in a method of operating an electroplating system in accordance with some embodiments of the present technology.

[0017] Figure 2 A schematic diagram of an electroplating processing system according to some embodiments of the present technology is shown.

[0018] Figure 3 Depicted are exemplary operations in another method of operating an electroplating system in accordance with some embodiments of the present technology.

[0019] Figure 4 Schematic diagrams are shown of supplementary components according to some embodiments of the present technology.

[0020] Several figures are included for illustration purposes. It will be understood that these figures are for illustrative purposes and are not to be considered to be to scale unless specifically noted as being to scale. Additionally, these figures are provided as illustrations to aid understanding and may not include all aspects or information as compared to actual representations and may include exaggerated material for illustrative purposes.

[0021] In the drawings, similar elements and / or features may have the same numerical reference symbol. In addition, multiple elements of the same kind may be distinguished by adding a letter that distinguishes the similar elements and / or features after the reference symbol. If only the leading numerical reference symbol is used in the specification, the description applies to any similar element and / or feature having the same leading numerical reference symbol, regardless of the suffix letter. DETAILED DESCRIPTION

[0022] The metal deposition rate of many electroplated metals increases with higher metal ion concentrations in aqueous solution. Conventional techniques for increasing the metal ion concentration of aqueous electroplating solutions include adding more initial liquid to the electroplating solution and evaporating some of the water from the solution. Evaporation increases both the metal ion concentration and the acid concentration. Metal compounds such as metal salts dissolve to increase the metal ion concentration, but this is not always possible in electroplating systems. Unfortunately, each of these techniques creates problems for electroplating systems that use an anolyte and a catholyte solution separated by an ion-selective membrane that allows metal ions to pass from the anolyte to the catholyte where metal electroplating occurs on the substrate surface.

[0023] In electroplating systems that include both anolyte and catholyte solutions, the increase in metal ion concentration is usually targeted to the catholyte because it is in direct contact with the plating surface of the substrate. For most initial liquids, the increased metal ions are also accompanied by increased acid. The increased acid in the anolyte can reduce the rate at which metal ions are transported from the anolyte through the ion-selective membrane to the catholyte. Due to the increased acidity in the anolyte, the rate of metal ion transport from the anolyte to the catholyte may be reduced by 50% or more.

[0024] Embodiments of the present technology address these issues by conditioning the anolyte and catholyte at elevated temperatures, which can increase their metal ion concentrations. In embodiments, the anolyte and catholyte can be conditioned in an existing electroplating chamber. This can reduce the amount of equipment required to perform an electroplating operation. In additional embodiments, anolyte and catholyte precursors can be formed, which can then be used to form the anolyte and catholyte, respectively. These embodiments can allow electroplating operations to be performed at higher metal ion concentrations than in conventional techniques, and can increase throughput in electroplating operations.

[0025] Figure 1 1 shows an exemplary operation of an electroplating method 100 according to some embodiments of the present technology. The method can be performed in a variety of processing systems, including an electroplating system according to embodiments of the present technology described below, including Figure 2 . For purposes of illustration, exemplary operations of method 100 will be described in conjunction with relevant elements of electroplating system 200. It will be understood that method 100 may also include one or more optional operations that may or may not be particularly relevant to some embodiments of methods according to the present technology. It will also be understood that any electroplating system operated according to method 100 may also include one or more additional elements or features discussed throughout the present disclosure.

[0026] Before the method 100 begins, the system 200 may be in a tool production mode, and in particular, the plating chamber 202 of the system 200 may be in a tool production mode. Figure 2Only one plating chamber 202 is shown in the system 200, but it is contemplated that the system 200 may include any number of plating chambers, such as two chambers, three chambers, four chambers, five chambers, ten chambers, fifteen chambers, twenty chambers, or more chambers. Prior to the start of the method 100, the plating chamber 202 may be in operation to electroplate material on a substrate or wafer. The method 100 may use an existing system 200 and an existing plating chamber 202 to condition and form both a cathode electrolyte solution and an anode electrolyte solution for use during a tool production mode. Thus, prior to the method 100, the system 200 may be switched from a tool production mode to a concentration mode. The method 100 may include providing an electrolyte feedstock to the existing plating chamber 202 at operation 105. The electrolyte feedstock may be provided to a first compartment 202a of the plating chamber 202 and to a second compartment 202b of the plating chamber 202. However, it is contemplated that recycled cathode electrolyte and / or recycled anode electrolyte may be provided to the first compartment 202a and / or the second compartment 202b as a replacement or supplement for the electrolyte raw material. In an embodiment, an acidic solution may be provided to the second compartment 202b of the electroplating chamber 202. Regardless of the material, the second compartment 202b may include both acid and metal ions. The second compartment 202b may include a new virgin makeup solution (VMS), or may include a used cathode electrolyte from a previous production operation. The first compartment 202a and the second compartment 202b of the electroplating chamber 202 may be separated by an ion selective membrane 208. The ion selective membrane 208 may selectively allow cations to pass between the first compartment 202a and the second compartment 202b of the electroplating chamber 202, while blocking other components from migrating between the first compartment 202a and the second compartment 202b of the electroplating chamber 202.

[0027] In order to convert the plating chamber 202 from the tool production mode to the concentration mode, a burn-in plate 206 can be positioned in the plating chamber 202. In addition, a bulk plating material 204 can be provided in the plating chamber 202, such as metal particles. The bulk plating material 204 can be simply referred to as an anode. More specifically, the burn-in plate 206 can be positioned in the second compartment 202b or disposed near the second compartment 202b. The bulk plating material 204 can be positioned in the first compartment 202a or disposed near the first compartment 202a.

[0028] The electrolyte feedstock can be any solution used to form a cathode electrolyte solution and an anode electrolyte solution. The electrolyte feedstock can be characterized by a metal ion concentration of less than or about 60.0 g / L, such as less than or about 58.0 g / L, less than or about 56.0 g / L, less than or about 54.0 g / L, less than or about 52.0 g / L, less than or about 50.0 g / L, less than or about 48.0 g / L, less than or about 46.0 g / L, less than or about 44.0 g / L, less than or about 42.0 g / L, less than or about 40.0 g / L, or less. In addition, the electrolyte raw material can be characterized by an acid concentration of less than or about 120.0 g / L, such as less than or about 118.0 g / L, less than or about 116.0 g / L, less than or about 114.0 g / L, less than or about 112.0 g / L, less than or about 110.0 g / L, less than or about 108.0 g / L, less than or about 106.0 g / L, less than or about 104.0 g / L, less than or about 102.0 g / L, less than or about 100.0 g / L, or less. The electrolyte raw material can be selected based on the desired metal ion concentration and acid concentration of the cathode electrolyte and the anode electrolyte.

[0029] During the method 100, the electrolyte raw material can be continuously circulated between the first compartment 202a and the second compartment 202b of the electroplating chamber 202. During the circulation, the electrolyte raw materials in each of the first compartment 202a and the second compartment 202b of the electroplating chamber 202 can be maintained in a state of being separated from each other. Each electrolyte raw material can be recycled in the compartment to which it belongs, but not recycled between these compartments. In particular, the electrolyte raw material in the first compartment 202a can be continuously circulated through the bulk electroplating material 204. The electrolyte raw material in the second compartment 202b can be continuously circulated through the burn-in plate 206.

[0030] Method 100 may include applying current to anode in operation 110. The current applied to the anode of the existing electroplating chamber may be greater than or about 10 amperes. In a system 200 with more than one chamber, the current applied to the system may be proportionally adjusted based on the number of electroplating chambers 202 used. A higher current may increase the amount of metal ions produced by the anode. Therefore, a higher current may increase the production rate of copper ions. Thus, the current applied to the anode of the existing electroplating chamber 202 may be greater than or about 15 amperes, greater than or about 20 amperes, greater than or about 25 amperes, greater than or about 30 amperes, greater than or about 35 amperes, greater than or about 40 amperes, greater than or about 45 amperes, greater than or about 50 amperes, greater than or about 55 amperes, or greater. During operation 110, the metal ions from the anode may be concentrated into the electrolyte raw materials in the first compartment 202a. In addition, the metal ions of the part in the second compartment 202b may be electroplated on the burn-in plate 206.

[0031] The method 100 may include, at operation 115, increasing the concentration of metal ions, such as copper ions, in the electrolyte raw material in the first compartment 202a to form a cathode electrolyte. When the metal ion concentration in the electrolyte raw material increases, the solution of increased metal ions may be referred to as a forming cathode electrolyte. The metal ion concentration of the forming cathode electrolyte may be measured by a metal ion sensor 205c, which is located in the first compartment 202a of the electroplating chamber 202. The metal ion sensor 205c may be in fluid contact with the electrolyte raw material / forming cathode electrolyte. The metal ion concentration in the forming cathode electrolyte may increase until the metal ion concentration meets a desired threshold. In embodiments, the threshold value of the desired metal ion concentration may be greater than or about 65.0 g / L, greater than or about 67.5 g / L, greater than or about 70.0 g / L, greater than or about 72.5 g / L, greater than or about 75.0 g / L, greater than or about 77.0 g / L, greater than or about 77.5 g / L, greater than or about 80.0 g / L, or greater. During processing, the acid concentration in the formation cathode electrolyte may decrease. However, the acid concentration may be increased during subsequent processing, such as in the buffer tank after being sent away from the plating chamber 202. For example, a portion of the formation cathode electrolyte may be evaporated, such as a portion of the water in the formation cathode electrolyte. In addition, additional electrolyte raw materials and / or acidic solutions may be added to the formation cathode electrolyte to drive the metal ion concentration and / or acid concentration to a final target value.

[0032] Additional metal ion sensors 205b, 205c, and 205d may be disposed throughout the system 200 to monitor metal ion concentrations. The metal ion sensors 205b, 205c, and 205d may be implemented in the same manner as sensor 205a and may be disposed in the second compartment 202b, the cathode electrolyte cell 210, and the anode electrolyte cell 212.

[0033] Once the electrolyte feedstock in the first compartment 202a of the electroplating chamber 202 reaches the desired metal ion concentration and forms a cathode electrolyte, the method 100 may include directing the cathode electrolyte to a storage tank 211 at operation 120, the storage tank 211 being in fluid communication with the existing electroplating chamber 202. That is, operation 110 may continue until the metal ion concentration in the electrolyte feedstock has increased to the desired metal ion concentration to form the cathode electrolyte. The cathode electrolyte may then be stored. When storing the cathode electrolyte, the cathode electrolyte may be driven to a final metal ion concentration and acid concentration by evaporating water and adding electrolyte feedstock and / or acidic solution, and the anolyte is formed prior to use in the system during tool production mode.

[0034] During operation of method 100, and more particularly during operations 110 and 115, additional electrolyte raw material may be added to the formation cathode electrolyte. The additional electrolyte raw material may compensate for any formation cathode electrolyte that evaporates during method 100. Furthermore, the additional electrolyte raw material may maintain the acid concentration of the formation cathode electrolyte.

[0035] The method 100 may also include providing a diluted electrolyte feedstock to the first compartment 202a after storing the cathode electrolyte at operation 125. The diluted electrolyte feedstock may be characterized by a metal ion concentration of less than or about 40.0 g / L, less than or about 38.0 g / L, less than or about 36.0 g / L, less than or about 34.0 g / L, less than or about 32.0 g / L, less than or about 30.0 g / L, less than or about 28.0 g / L, less than or about 26.0 g / L, or less. The diluted electrolyte feedstock may be characterized by an acid concentration of less than or about 70.0 g / L, less than or about 68.0 g / L, less than or about 66.0 g / L, less than or about 64.0 g / L, less than or about 62.0 g / L, less than or about 60.0 g / L, less than or about 58.0 g / L, less than or about 56.0 g / L, or less. The dilute electrolyte raw materials may be selected based on the desired metal ion concentration and acid concentration of the final anolyte.

[0036] Method 100 may include increasing the concentration of metal ions, such as copper ions, in an anode electrolyte precursor at operation 130 to form an anode electrolyte. The concentration of metal ions in the anode electrolyte precursor may be performed in a manner similar to or identical to that of the cathode electrolyte. In particular, an electric current may be applied to the anode, which may produce metal ions concentrated in the anode electrolyte precursor in the second compartment 202b. In addition, hydrogen ions may migrate through the ion selective membrane 208 to the anode electrolyte precursor in the second compartment 202b at operation 130. The concentration of metal ions in the anode electrolyte precursor may be increased until the metal ion concentration meets a desired threshold. Similarly, the acid concentration in the anode electrolyte precursor may be reduced until the acid concentration meets a desired threshold. In embodiments, the desired threshold metal ion concentration may be greater than or about 65.0 g / L, greater than or about 67.5 g / L, greater than or about 70.0 g / L, greater than or about 72.5 g / L, greater than or about 75.0 g / L, greater than or about 77.0 g / L, greater than or about 77.5 g / L, greater than or about 80.0 g / L, or greater. Additionally, operation 130 may continue until the acid concentration meets the desired threshold. In embodiments, the anolyte may be characterized by an acid concentration of less than or about 10.0 g / L, less than or about 9.0 g / L, less than or about 8.0 g / L, less than or about 7.0 g / L, less than or about 6.0 g / L, less than or about 5.0 g / L, less than or about 4.0 g / L, less than or about 3.0 g / L, less than or about 2.0 g / L, less than or about 1.0 g / L, or less.

[0037] Once the anolyte precursor in the first compartment 202a of the plating chamber 202 reaches the desired metal ion concentration and acid concentration and forms the anolyte, the method 100 may include containing the anolyte in a storage tank 212 that is in fluid communication with the existing plating chamber 202. That is, operation 130 may continue until the metal ion concentration in the anolyte precursor has increased to the desired metal ion concentration and the acid concentration has decreased to the desired acid concentration to form the anolyte. The anolyte may then be stored prior to use in the system during the tool production mode. For example, the anolyte may be directed to or stored in the storage tank 212 while the plating chamber 202 is switched back to the production mode.

[0038] During operation of method 100, the temperature in some or all of the elements may be maintained at greater than or about 40° C. At temperatures less than 40° C., the solubility of the metal ions may decrease. In addition, at temperatures less than 40° C., the viscosity of the cathode electrolyte and / or the anode electrolyte may, for example, increase to a stage where the solution becomes difficult to transport. Thus, the temperature may be maintained at greater than or about 42° C., greater than or about 44° C., greater than or about 46° C., greater than or about 48° C., greater than or about 50° C., or greater.

[0039] At optional operation 135, the cathode electrolyte may be transported to its corresponding storage tank. For example, the cathode electrolyte may be transported to storage tank 210, which may be referred to as a cathode electrolyte tank. The anolyte may have been stored in storage tank 212 at the end of operation 130, which may be referred to as an anolyte tank. Tank 211 may be an intermediate buffer or storage tank that may be used after preparing the cathode electrolyte and during the production of the anolyte. That is, the prepared cathode electrolyte may be temporarily stored in tank 211 during the production of the anolyte. As described above, when the cathode electrolyte is stored in tank 211, the cathode electrolyte may achieve the final metal ion concentration and acid concentration target by evaporation and adding electrolyte raw materials and / or acidic solutions. After the anolyte is prepared, the anolyte is stored in the anolyte tank 212, and the cathode electrolyte may be transported from tank 211 to tank 210. Before the cathode electrolyte may be transported from tank 211 to tank 210, the sacrificial dilution electrolyte raw material used in the first compartment 202a may be withdrawn.

[0040] At optional operation 140, after forming the cathode electrolyte and the anolyte, the electroplating chamber 202 can be switched from the concentration mode to the tool production mode. After switching back to the tool production mode, the electroplating chamber 202 can be used to deposit a metal material using the formed cathode electrolyte and the anolyte. For example, the electroplating chamber 202 can be operable to electroplate a metal material from the formed cathode electrolyte onto a substrate or wafer, such as a copper material.

[0041] Figure 3 300 according to some embodiments of the present technology. This method can be performed in a variety of processing systems, including electroplating systems according to embodiments of the present technology described previously or described below, including Figure 1 The exemplary electroplating system 200 shown in FIG. Figure 4. For illustrative purposes, the exemplary operation of method 300 will be described in conjunction with the relevant elements of electroplating system 400. It will be understood that method 300 may also include one or more optional operations, which may be particularly relevant to some embodiments of methods according to the present technology, or may be particularly unrelated to some embodiments of methods according to the present technology. It will also be understood that any electroplating system operated according to method 300 may also include one or more additional elements or features discussed in the present disclosure. Method 300 can be performed in an external electroplating system 400 without interrupting production to use an existing electroplating chamber in production. It is noteworthy that method 300 can also alternatively be performed using an existing electroplating chamber that is a two-compartment mode, such as electroplating system 200. However, using an existing electroplating chamber requires interrupting production.

[0042] The method 300 may include providing an electrolyte material to the first compartment 98 of the electrochemical cell 74 at operation 305. The electrolyte material may include the electrolyte material described above. Figure 1-2 Any characteristic or feature of the electrolyte raw material discussed. For example, the electrolyte raw material can include a metal such as copper, and can be characterized by a metal ion concentration. In an embodiment, the electrolyte raw material can be characterized by a copper ion concentration of less than or about 60.0 g / L. In addition, the electrolyte raw material can be characterized by an acid concentration of less than or about 120.0 g / L.

[0043] The first compartment 98 of the electrochemical cell can be separated from the second compartment 106 of the electrochemical cell 74 by a membrane 104, such as an ion-selective membrane. The membrane 104 can selectively allow cations to pass between the first compartment 98 and the second compartment 106 of the electrochemical cell 74, and block other components from migrating between the first compartment 98 and the second compartment 106 of the electrochemical cell 74. Similar to the system 200, a burn-in plate 114 can be positioned in the electrochemical cell 74. In addition, a bulk plating material 92 can be provided in the electrochemical cell 74, such as metal particles. The bulk plating material 92 can be simply referred to as an anode. The bulk plating material 92 can be positioned in the first compartment 98 or disposed near the first compartment 98. In an embodiment with two compartments, the burn-in plate 114 can be positioned in the second compartment 106 or disposed near the second compartment 106. In embodiments having a third compartment 112 , a burn-in plate 114 may be positioned in or disposed adjacent to the third compartment 112 .

[0044] At operation 310, in an embodiment having two compartments, the method 300 may include providing an electrolyte raw material or an acidic solution to the second compartment 106 of the electrochemical cell 74. In an embodiment having three compartments, the method 300 may include providing an acidic solution to the second compartment 106 of the electrochemical cell 74. In an embodiment, the acidic solution may include sulfuric acid diluted with water, such as deionized water, but it is contemplated that other acids may be used in addition to or in place of sulfuric acid. The acidic solution can be characterized by an acid concentration of less than or about 120.0 g / L, for example, less than or about 118.0 g / L, less than or about 116.0 g / L, less than or about 114.0 g / L, less than or about 112.0 g / L, less than or about 110.0 g / L, less than or about 108.0 g / L, less than or about 106.0 g / L, less than or about 104.0 g / L, less than or about 102.0 g / L, less than or about 100.0 g / L, or less.

[0045] During the method 300, the electrolyte raw material may be continuously circulated between the first compartment 98 of the electrochemical cell 74, for example, via the electrolyte raw material loop 90. The electrolyte raw material may be provided to the electrolyte raw material tank 96 via the conduit 124. During the method 300, the electrolyte raw material in the first compartment 98 may be continuously circulated through the bulk electroplating material 92 and through the electrolyte raw material tank 96. The solution in the second compartment 106 (or the third compartment 112 when present) may be continuously circulated through the burn-in plate 114. Figure 4 As shown in , during the method 300, the material in the third compartment 112 can be provided via the conduit 122 and can be circulated through the tank 118. During the method 300, the material in the second compartment 106 can be provided via the conduit 72 and can be circulated through the tank (not shown). More specifically, the conduit 72 can be connected to one side of the second compartment 106, and the conduit 78 can be connected to the other side of the second compartment 106, which can allow the circulation of the material in the second compartment 106.

[0046] As previously described, in embodiments, the electrochemical cell 74 may include a third compartment 112. The third compartment 112 may be separated from the second compartment 106 by a membrane 108, such as a second ion-selective membrane. At optional operation 315, the method 300 may include providing additional electrolyte raw material or additional acidic solution to the third compartment 112. The electrolyte raw material or acidic solution provided to the third compartment 112 may be the same or similar to the electrolyte raw material provided to the first compartment 98 or the acidic solution provided to the second compartment 106.

[0047] The method 300 may include applying a current to the anode at operation 320. The negative electrode or cathode of the power source 55 may be electrically connected to the burn-in plate 114, and the power source 55 may be, for example, a direct current (DC) power source. The positive electrode or anode of the power source 55 may be electrically connected to the bulk electroplating material 92 or metal in the supplementary assembly anode electrolyte compartment 98, and a voltage difference is applied or generated across the electrochemical cell 74. The current applied to the anode of the electrochemical cell may be greater than 800 amperes. Higher currents may increase the amount of metal ions produced by the anode. Thus, the current applied to the anode of the existing electrochemical cell 74 may be greater than or about 900 amperes, greater than or about 1000 amperes, greater than or about 1100 amperes, greater than or about 1200 amperes, greater than or about 1300 amperes, greater than or about 1400 amperes, greater than or about 1500 amperes, greater than or about 1600 amperes, or greater. During operation 110, metal ions from the anode may be concentrated into the electrolyte material in the first compartment 98. Additionally, during operation 110, the acid concentration may be reduced compared to the initial concentration in the electrolyte material.

[0048] During operation, the acid concentration in the acidic solution in the second compartment 106 or the third compartment 112 may increase or decrease. In embodiments, the method 300 may include removing, or bleeding, a portion of the acidic solution in one or both of the second compartment 106 or the third compartment 112 at operation 325. This portion of the acidic solution may be removed, for example, by Figure 4 86 is removed from the three-compartment system shown in FIG. Similarly, method 300 may include providing or feeding a new acidic solution to one or both of the second compartment 106 or the third compartment 112 at operation 325. By draining and feeding the acidic solution, the acidity in the second compartment 106 and / or the third compartment 112 may be maintained, and the formation of the anolyte and cathode electrolyte precursors may be promoted.

[0049] At operation 330, method 300 may include forming an anolyte and a cathode electrolyte precursor in first compartment 98. The anolyte and cathode electrolyte precursors may be used to form a separate anolyte and a separate cathode electrolyte. Operations 320 and 325 may continue until the anolyte and cathode electrolyte precursors meet the desired metal ion concentration and the desired acid concentration. In an embodiment, the anolyte and cathode electrolyte precursors are characterized by a copper ion concentration greater than or about 70.0 g / L, such as greater than or about 72.0 g / L, greater than or about 74.0 g / L, greater than or about 75.0 g / L, greater than or about 76.0 g / L, greater than or about 78.0 g / L, greater than or about 80.0 g / L, greater than or about 82.0 g / L, greater than or about 84.0 g / L, greater than or about 86.0 g / L, greater than or about 88.0 g / L, greater than or about 90.0 g / L, or greater.

[0050] In optional operations 335 and 340, method 300 may include forming an anolyte and forming a cathode electrolyte, respectively. In operation 335, the anolyte may be formed by mixing the anolyte and cathode electrolyte precursors with a diluent. In an embodiment, the diluent may be or include water, such as deionized water. The anolyte may be characterized by a metal ion concentration greater than or about 60.0 g / L, such as greater than or about 62.0 g / L, greater than or about 64.0 g / L, greater than or about 66.0 g / L, greater than or about 68.0 g / L, greater than or about 70.0 g / L, greater than or about 72.0 g / L, greater than or about 74.0 g / L, greater than or about 76.0 g / L, greater than or about 78.0 g / L, greater than or about 80.0 g / L, or greater. The anolyte may also be characterized by an acid concentration of less than or about 20.0 g / L, such as less than or about 15.0 g / L, less than or about 12.5 g / L, less than or about 10.0 g / L, less than or about 7.5 g / L, less than or about 5.0 g / L, less than or about 4.0 g / L, less than or about 3.0 g / L, less than or about 2.0 g / L, less than or about 1.0 g / L, or less. At operation 340, a cathode electrolyte may be formed by mixing the anolyte and cathode electrolyte precursors with additional electrolyte raw materials and evaporating water. In embodiments, a portion of the cathode electrolyte may be evaporated, which may increase the metal ion concentration and / or acid concentration. The cathode electrolyte can be characterized by a metal ion concentration of greater than or about 60.0 g / L, such as greater than or about 62.0 g / L, greater than or about 64.0 g / L, greater than or about 66.0 g / L, greater than or about 68.0 g / L, greater than or about 70.0 g / L, greater than or about 72.0 g / L, greater than or about 74.0 g / L, greater than or about 76.0 g / L, greater than or about 78.0 g / L, greater than or about 80.0 g / L, or greater. The cathode electrolyte can also be characterized by an acid ion concentration of greater than or about 85.0 g / L, such as greater than or about 87.5 g / L, greater than or about 90.0 g / L, greater than or about 92.5 g / L, greater than or about 95.0 g / L, greater than or about 97.5 g / L, greater than or about 100.0 g / L, or greater.

[0051] Embodiments of the present technology allow electroplating operations to be performed with increased metal ion concentrations in the cathode electrolyte over long periods of time. The increased metal ion concentration increases the deposition rate of metal on the substrate during the electroplating operation, thereby increasing the throughput of the substrate through the electroplating system. In embodiments, the increased metal ion concentration can be maintained for long periods of time by increasing the preparation rate of the cathode electrolyte and the anolyte. Efficient preparation of the cathode electrolyte and the anolyte precursors and / or the cathode electrolyte and the anolyte can reduce system downtime and can further increase throughput.

[0052] In the foregoing description, for the purpose of explanation, many details have been set forth in order to understand several embodiments of the present technology. However, it will be apparent to those skilled in the art that certain embodiments may be implemented without some of these details or with additional details.

[0053] Having disclosed several embodiments, those skilled in the art will recognize that several modifications, alternative configurations, and equivalents may be used without departing from the spirit of the embodiments. In addition, some well-known processes and components are not described to avoid unnecessary confusion of the present technology. Therefore, the above description should not be used as a limitation on the scope of the present technology.

[0054] It will be understood that, unless the context clearly dictates otherwise, where a numerical range is provided, each intermediate value between the upper and lower limits of the range to the minimum fraction of the lower limit unit is also explicitly disclosed. Any narrower range between any stated value or unstated intermediate value in the stated range, and any other stated value or intermediate value in the stated range are included. The upper and lower limits of these smaller ranges may be independently included or excluded in the range, and each range that includes either one, neither, or both limits in the smaller range is also included in this technology, but is still subject to any explicitly excluded limits in the stated range. Where the stated range includes one or two limits, the range that does not include either or both of these limits is also included. Where multiple values ​​are provided in a list, any range that includes or is based on any of these values ​​is similarly specifically disclosed.

[0055] As used herein and in the appended claims, the singular forms "a," "an," and "the" include plural forms unless the context clearly dictates otherwise. Thus, for example, reference to "a feedstock" includes a plurality of such feedstocks and reference to "the electrochemical cell" includes one or more electrochemical cells and equivalents thereof known to those skilled in the art, and so forth.

[0056] Furthermore, when used in this specification and the claims that follow, the words “comprise(s),” “comprising,” “contain(s),” “containing,” “include(s),” and “including” are intended to mean the presence of stated features, integers, elements, or operations, but they do not preclude the presence or addition of one or more other features, integers, elements, operations, actions, or groups.

Claims

1. An electroplating method, comprising: providing a first portion of an electrolyte raw material to a first compartment of an electrochemical cell, the electrolyte raw material comprising copper; providing a second portion of the electrolyte raw material or the acidic solution to a second compartment of the electrochemical cell, wherein the first compartment and the second compartment are separated by a separator; applying an electric current to an anode of the electrochemical cell, wherein the anode of the electrochemical cell is disposed adjacent to the first compartment and opposite to the separator; as well as Anolyte and catholyte precursors are formed.

2. The electroplating method of claim 1, wherein the electrolyte feedstock is characterized by a copper ion concentration of less than or about 50.0 g / L.

3. The electroplating method of claim 1, wherein the acidic solution is characterized by an acid concentration of less than or about 110.0 g / L.

4. The electroplating method of claim 1, wherein the anolyte and catholyte precursors are characterized by a copper ion concentration greater than or about 70.0 g / L.

5. The electroplating method according to claim 1, further comprising: The anolyte is formed by mixing the anolyte and catholyte precursors with a diluent, and wherein the diluent comprises deionized water.

6. The electroplating method of claim 5, wherein: The anolyte is characterized by a copper ion concentration of greater than or about 60.0 g / L; and The anode electrolyte is characterized by an acid concentration of less than or about 20.0 g / L.

7. The electroplating method according to claim 1, further comprising: The cathode electrolyte is formed by mixing the anode electrolyte and cathode electrolyte precursors with additional electrolyte raw materials and evaporating water.

8. The electroplating method of claim 7, wherein: The cathode electrolyte is characterized by a copper ion concentration greater than or about 60.0 g / L; and The cathode electrolyte is characterized by an acid ion concentration greater than or about 90.0 g / L.

9. The electroplating method of claim 1, wherein a temperature is maintained at greater than or about 40°C when forming the anolyte and catholyte precursors.

10. The electroplating method according to claim 1, further comprising: A portion of the acidic solution is removed from the second compartment and replaced with a new acidic solution, wherein the new acidic solution maintains the acid concentration in the second compartment.

11. The electroplating method according to claim 1, further comprising: Additional electrolyte raw material or additional acidic solution is provided to a third compartment of the electrochemical cell, wherein the second compartment and the third compartment are separated by a second separator.

12. The electroplating method of claim 1, wherein the first compartment and the second compartment of the electrochemical cell are existing electroplating chamber compartments.

13. An electroplating method, comprising: providing electrolyte raw materials to a first compartment and a second compartment of an existing electroplating chamber, wherein the first compartment and the second compartment are separated by a diaphragm; applying an electric current to an anode located in the existing electroplating chamber, wherein the anode is disposed adjacent to the first compartment and opposite to the diaphragm; increasing the concentration of copper ions in the electrolyte feedstock in the first compartment to form a cathode electrolyte; directing the cathode electrolyte to a storage tank, the storage tank being in fluid communication with the existing electroplating chamber; providing a diluted electrolyte feedstock to the first compartment; as well as The copper ion concentration in the electrolyte feedstock in the first compartment is increased to form an anode electrolyte.

14. The electroplating method according to claim 13, further comprising: After forming the anode electrolyte, the cathode electrolyte is directed from the storage tank to a cathode electrolyte tank.

15. The electroplating method according to claim 13, further comprising: After forming the anolyte, the existing electroplating chamber is converted to production mode.

16. The electroplating method of claim 13, wherein: The cathode electrolyte and the anode electrolyte are each characterized by a copper ion concentration greater than or about 65.0 g / L.

17. The electroplating method of claim 13, wherein the current applied to the anode of the existing electroplating chamber is greater than or approximately 10 amps.

18. The electroplating method of claim 13, wherein a temperature is maintained at greater than or about 40°C when forming the cathode electrolyte and the anode electrolyte.

19. The electroplating method of claim 13, wherein the existing electroplating chamber is operable to electroplate copper material from the cathode electrolyte onto a substrate.

20. An electroplating method, comprising: Converting existing electroplating chambers from production mode to concentration mode; providing electrolyte raw materials to a first compartment and a second compartment of the existing electroplating chamber, wherein the first compartment and the second compartment are separated by a diaphragm; applying an electric current to an anode located in the existing electroplating chamber, wherein the anode is disposed adjacent to the first compartment and opposite to the diaphragm; increasing the concentration of copper ions in the electrolyte feedstock in the first compartment to form a cathode electrolyte; directing the cathode electrolyte to a storage tank, the storage tank being in fluid communication with the existing electroplating chamber; providing a diluted electrolyte feedstock to the first compartment; increasing the copper ion concentration in the electrolyte raw material in the second compartment to form an anode electrolyte; as well as The existing electroplating chamber is converted from a concentration mode to a production mode.

21. The electroplating method of claim 20, wherein the cathode electrolyte and the anode electrolyte are each characterized by a copper ion concentration greater than or about 65.0 g / L.