Plasma processing method and plasma processing apparatus

By using plasma treatment methods of hydrogen and water vapor, the problems of copper layer oxidation, photoresist residue removal and surface hydrophilization in electronic devices such as semiconductor substrates and lead frames are solved, and convenient access to the plating solution is achieved. Improves processing efficiency.

CN119072771APending Publication Date: 2024-12-03SAMCO INC
3 Cites 0 Cited by

Patent Information

Application Number
CN202380035911.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the plasma treatment of electronic devices such as semiconductor substrates and lead frames, it is impossible to effectively prevent the oxidation of the copper layer, remove the photoresist residue, and make the surface of the through-hole hydrophilization, affecting the entry of the plating solution.

Method used

The raw material gas composed of hydrogen and water vapor is used for plasma treatment, hydrogen and water vapor are generated through an electrolytic device of water, and plasma treatment is performed in the treatment room to ensure that the water vapor is above saturation, usually between 10 and 40%. water vapor ratio.

Benefits of technology

The copper layer is prevented from oxidation, rapid removal of photoresist residues and surface hydrophilization are achieved, making the plating solution easy to enter the narrow space, and the treatment efficiency is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119072771A_ABST
    Figure CN119072771A_ABST
Patent Text Reader

Abstract

The present invention provides a plasma treatment method capable of obtaining the effects of (1) reduction of a copper layer, (2) high-speed ashing of a photoresist, and (3) hydrophilization of the inner surface of a through hole when performing plasma treatment on a substrate for an electronic device in which a semiconductor substrate having a copper layer on the surface is etched using the photoresist and plated. A plasma processing method for plating a substrate for an electronic device according to the present invention is characterized by comprising the steps of: a) disposing a substrate for an electronic device, such as a semiconductor substrate or a lead frame, in a processing chamber; b) supplying a raw material gas comprising hydrogen and water vapor obtained from a device for electrolyzing water to the processing chamber; and c) plasma processing is performed on the substrate for the electronic device by converting the raw material gas in the processing chamber into plasma.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a plasma processing method for cleaning the surface of a substrate for electronic devices such as a semiconductor substrate and a lead frame, and an apparatus therefor. Background Art

[0002] With the development of information society, semiconductor packaging is becoming more and more high-performance, high-functional and miniaturized. By using flip chip mounting technology, semiconductor chips can be connected at a high density, but due to the requirements of electrical characteristics, the increase in the number of I / Os, and in order to cope with the rise in gold prices, micro bumps using copper (Cu) pillars are widely used.

[0003] In more cases, such as Figure 1 First, on the substrate 11 ( Figure 1 (a)) is coated with a photoresist 13, and a through hole (opening) 14 is formed in the wiring portion ( Figure 1 (b)). At this point, in order to clean the inside and the periphery of the through hole 14, a pre-treatment is performed using plasma 15 ( Figure 1 (c)). Then, copper 16 is filled in the through hole 14 by plating ( Figure 1 (d)). Then, the photoresist 13 is removed ( Figure 1 (e)), removing the copper layer 12 on the substrate 11 ( Figure 1 (f)).

[0004] [Prior art literature]

[0005] [Patent Document]

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 06-029254

[0007] [Patent Document 2] Japanese Patent Application Publication No. 2018-098353

[0008] [Patent Document 3] Japanese Patent Application Publication No. 2015-160192

[0009] [Non-patent literature]

[0010] [Non-patent document 1] “Application of Aqua Plasma(R) to microbumps”, samco NOW, Vol. 111, October 2020, Samco Co., Ltd. Summary of the invention

[0011] [Problems to be Solved by the Invention]

[0012] When forming copper microbumps, the cleaning of the through hole must achieve the following effects: (1) preventing or reducing oxidation of the copper layer at the bottom (on the substrate); (2) ashing of photoresist residues; and (3) making the inner surface of the through hole hydrophilic so that the plating solution can easily enter. In the previous treatment of semiconductor substrates using plasma (for example, Patent Document 1), by performing hydrogen plasma treatment in a specific chamber, the effect of (1) preventing or reducing oxidation of the copper layer is achieved, but sufficient effects cannot be achieved for (2) ashing of photoresist residues and (3) hydrophilization of the inner surface of the through hole.

[0013] Such effects (1) to (3) (regarding (2) obtaining a sufficient ashing speed) are not only required for the process of forming micro bumps, but are also commonly required for the pre-processing when etching a semiconductor substrate having a copper layer on its surface using a photoresist and performing a plating process. In addition, in the conventional mounting technology in which a lead portion (lead frame) and an electrode portion (hereinafter referred to as a metal portion) of a semiconductor substrate are connected by a metal wire, it is also necessary to prevent or reduce oxidation of the lead portion and the electrode portion.

[0014] The present invention is completed to solve the problems of the prior art, and its purpose is to provide a plasma processing method that can obtain the above-mentioned effects (1) to (3) when processing a substrate for an electronic device including such a semiconductor substrate, a metal part, a lead part, etc.

[0015] [Methods to solve the problem]

[0016] The plasma processing method for an electronic device substrate of the present invention, which has been accomplished to solve the above-mentioned problems, is characterized by comprising the following steps:

[0017] a) placing an electronic device substrate in a processing chamber;

[0018] b) supplying a raw material gas consisting of hydrogen and water vapor obtained from a device for electrolyzing water to the above-mentioned treatment chamber; and

[0019] c) performing plasma processing on the electronic device substrate by converting the source gas in the processing chamber into plasma.

[0020] Here, the electronic device substrate includes not only the semiconductor substrate, but also the metal parts such as the electrodes thereof and the lead parts such as the peripheral lead frame. In addition, with respect to the raw material gas, it is desirable that the water vapor in the raw material gas as a whole is an amount above the saturation state of the water in the raw material gas. For example, it is about 3.3% by pressure or more at 27°C. Furthermore, it is more desirable to be 10 to 40% by pressure.

[0021] Furthermore, the plasma processing apparatus for plating a substrate for an electronic device of the present invention, which has been completed in order to solve the above-mentioned problems, is characterized by comprising:

[0022] a) a plasma processing chamber provided with a stage for mounting a substrate for an electronic device to be processed;

[0023] b) a water electrolysis device, which is a supply source of a raw material gas consisting of hydrogen and water vapor connected to the above-mentioned treatment chamber; and

[0024] c) A plasma generating unit that converts the source gas introduced into the processing chamber into plasma.

[0025] [Effects of the Invention]

[0026] According to the method of the present invention, in the plasma treatment of substrates for electronic devices, the following effects can be reliably obtained: (1) prevention or reduction of oxidation of the copper layer on the substrate; (2) high-speed ashing of photoresist residues; and (3) making the surface hydrophilic and making it easy for the plating solution to enter narrow spaces. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] [ Figure 1 ] is an explanatory diagram showing the sequence of forming microbumps.

[0028] [ Figure 2 ] is a diagram showing a sample group in which a copper oxide chip and a silicon chip are placed on a dummy substrate.

[0029] [ Figure 3 ] is a schematic diagram of the structure of a plasma processing device used in an experiment conducted to confirm the effect of the present invention.

[0030] [ Figure 4 ] is a luminescence intensity curve graph showing the results of emission spectrum analysis of plasma performed during plasma processing.

[0031] [ Figure 5 ] is a table showing the contents of each test performed to confirm the effects of the present invention.

[0032] [ Figure 6 ] is a table showing the results of Test 1 and Test 2.

[0033] [ Figure 7 ] is a table showing the results of Experiment 3. DETAILED DESCRIPTION

[0034] Hereinafter, the method and results of the test conducted to confirm the effects of the present invention will be described with reference to the drawings.

[0035] [sample]

[0036] The samples tested were the following two types.

[0037] (1) Copper oxide chip

[0038] The surface of a copper plate of 10×20×0.3 mm was oxidized. The thickness of the oxide layer was 40 nm.

[0039] (2) Silicon chip

[0040] The photoresist (PR) was applied on the surface of a silicon (Si) plate of 15×15×0.5±0.025 mm. The PR was THMR-IP3250 manufactured by Tokyo Ohka, baked at 110°C for 5 minutes, and the coating thickness was 1 μm.

[0041] In the following Test 3, these chips were mounted on the following dummy substrate.

[0042] (3) Dummy substrate

[0043] 200×150×0.3mm pure copper plate. It is the substrate for 300mm (φ8) wafer.

[0044] A sample set 20 in which a copper oxide chip 22 and a silicon chip 23 are placed on a dummy substrate 21 is shown in FIG. Figure 2 middle.

[0045] A parallel plate type plasma processing apparatus (PD-220) 30 manufactured by Samco Co., Ltd. was used as a plasma processing apparatus. Figure 3 As shown in (a) to (c), in the plasma processing device 30, the lower electrode 32 is grounded, and the upper electrode 33 (area 452m 2 ) is connected to a high frequency power supply 34 and used (PE mode). Then, the processing chamber 31 is connected to a vacuum pump (DRP) 35 and to a plasma gas source via a flow meter (FM) 36. The plasma gas source is set differently depending on the experiment. The contents are shown in Figure 5 The processing chamber 31 is made of metal (stainless steel).

[0046] The methods and results of each test are as follows. Figure 5 The results are summarized in Figure 6 and Figure 7 middle.

[0047] <Test 1>

[0048] In Experiment 1, if Figure 3As shown in (a), an electrolysis device 37 is used as a plasma gas source. If a high-pressure hydrogen cylinder is used as a plasma gas source, it is necessary to install and maintain it according to the provisions of the High-Pressure Gas Safety Act, so an electrolysis device 37 is used in the present invention. In the electrolysis device 37, hydrogen is generated and output by electrolyzing water, but water (water vapor) is also output at the same time. Water is output in a state of approximately saturated water vapor pressure, so about 3.3 pressure % is contained in the output gas at room temperature (27°C).

[0049] Furthermore, when hydrogen is generated by the electrolysis device 37, in addition to pure water, water containing a small amount of sodium hydroxide (NaOH) can also be used as a raw material. Thus, the electrolysis of water is performed more efficiently. However, when water containing a small amount of sodium hydroxide is used, there is a possibility that a raw material gas mixed with a trace amount of Na is supplied to the processing chamber and the processing chamber and the surface of the substrate are contaminated by Na. Therefore, it is more desirable to use pure water as a raw material, and in this respect, it is more desirable to have an electrolysis device with a solid electrolyte battery.

[0050] The copper oxide chip 22 and the silicon chip 23 were placed on the lower electrode 32, and after the processing chamber 31 was evacuated by the vacuum pump 35, hydrogen containing water vapor was transported into the processing chamber 31 from the electrolysis device 37 to a pressure of 5 Pa, and the plasma raw material gas (hydrogen + water vapor) was circulated at a flow rate of 20 SCCM, and high-frequency power was input from the high-frequency power supply 34. The input high-frequency power was 100 W, and the processing time was 3 minutes.

[0051] The results of the emission spectrum analysis of the plasma during the treatment are shown in FIG. Figure 4 (a) (solid line). In addition to the higher peak of H (hydrogen) at 656nm, the peak of OH (hydroxyl radical) at 309nm caused by water vapor is observed at twice the height of the following experiment 2, and the peak of O (oxygen) at 777nm is observed at 1.5 times the height of experiment 2 ( Figure 4 (b), (c)). OH (hydroxyl) helps to improve the hydrophilicity of the surface, and O (oxygen) helps to increase the ashing speed of PR.

[0052] After the plasma treatment, if the surface of the copper oxide chip 22 is observed, the copper oxide is completely reduced, exposing the pure copper surface ( Figure 6 middle column).

[0053] Next, if the ashing rate is calculated by dividing the thickness (1 μm) of the photoresist (PR) on the surface of the silicon chip 23 by the processing time, it becomes 19 nm / min ( Figure 6 middle column).

[0054] Furthermore, the water contact angle of the surface (photoresist layer) of the silicon chip 23 after the plasma treatment was measured. A water contact angle of 90° or less was defined as hydrophilicity, and a water contact angle of 10° or 5° or less was defined as super hydrophilicity. The results of the measurement showed that the water contact angle was 3°, which was super hydrophilicity ( Figure 6 below the middle column).

[0055] <Test 2>

[0056] In Test 2, instead of using an electrolytic device, such as Figure 3 As shown in (b), a high-pressure hydrogen gas cylinder 38 containing high-purity hydrogen is used as a plasma gas source. The purity of hydrogen supplied from the high-pressure hydrogen gas cylinder 38 is 99.9999% or more.

[0057] As in Experiment 1, the copper oxide chip 22 and the silicon chip 23 were placed on the lower electrode 32, and after the processing chamber 31 was evacuated by the vacuum pump 35, high-purity hydrogen was transported into the processing chamber 31 from the high-pressure hydrogen cylinder 38. As in Experiment 1, the plasma raw material gas (hydrogen) was circulated at a pressure of 5 Pa and a flow rate of 20 SCCM, and high-frequency power was input from the high-frequency power supply 34. As in Experiment 1, the high-frequency power input was 100 W, and the processing time was 3 min.

[0058] The results of the emission spectrum analysis of the plasma during the treatment are as follows Figure 4 (a) is shown by the dotted line. No clear peaks were observed in OH at 309 nm or O at 777 nm due to water vapor ( Figure 4 (b), (c)).

[0059] After the plasma treatment, if the surface of the copper oxide chip 22 is observed, the copper oxide is completely reduced, exposing the pure copper surface ( Figure 6 on the right column).

[0060] In this test 2, the ashing rate was 6 nm / min ( Figure 6 in the right column).

[0061] Moreover, the water contact angle is 20° ( Figure 6 right column).

[0062] <Test 3>

[0063] In Experiment 3, if Figure 3As shown in (c), a hydrogen source and a water vapor source are used together as plasma gas sources, and an electrolysis device 37 with a water vapor capture device (H2O-TRAP) (electrolysis device with H2O-TRAP 39) is used as a hydrogen source, and a heating vaporization type water vapor generator 40 is used as a water vapor source. The flow rates of these hydrogen and water vapor are adjusted by respective flow meters 36a and 36b, and the mixing ratio of the two is changed from 0% water vapor to 100% by 10% each time to perform plasma treatment.

[0064] In Experiment 3, in order to be close to the actual processing environment of the wafer, the copper oxide chip 22 and the silicon chip 23 are placed as shown in FIG. Figure 2 The sample group 20 placed on the pure copper dummy substrate 21 was placed on the lower electrode 32. The plasma treatment conditions were the same as those in the experiments 1 and 2.

[0065] When the surface of the copper oxide chip 22 was observed after plasma treatment at various mixing ratios of hydrogen / water vapor = 100 / 0 to 0 / 100, Figure 7 As shown in the second paragraph, under the condition of hydrogen / water vapor = 100 / 0 to 60 / 40, the copper oxide on the surface is completely reduced and the pure copper surface is exposed, but under the condition of hydrogen / water vapor = 50 / 50 to 0 / 100, the surface is not completely reduced (in Figure 7 The results of hydrogen / water vapor = 40 / 60, 20 / 80, and 30 / 90 are omitted).

[0066] The ashing rate of the photoresist layer under various conditions is as follows Figure 7 As shown in the third paragraph of , the ashing rate value is slightly lower in hydrogen / water vapor = 100 / 0, but the photoresist layer is removed at a sufficiently high speed in hydrogen / water vapor = 90 / 10 to 0 / 100.

[0067] The water contact angle of the photoresist layer after treatment under various conditions is as follows: Figure 7 As shown in the fourth paragraph of , here, too, the water contact angle value is slightly larger, 20°, in hydrogen / water vapor = 100 / 0, but is 5 to 3° in hydrogen / water vapor = 90 / 10 to 0 / 100, showing superhydrophilicity.

[0068] <Conclusion>

[0069] If we compare the experiment 1 in which the plasma raw gas is hydrogen + water vapor with the experiment 2 in which the plasma raw gas is only hydrogen ( Figure 3 (a), (b) and Figure 5 ), there is no difference in the effect of reducing copper oxide ( Figure 6 However, in the speed of photoresist layer removal (ashing rate), the experiment 1 using hydrogen + water vapor as raw material gas obtained a higher value than the experiment 2 using only hydrogen as raw material gas ( Figure 6Paragraph 3). In addition, regarding the hydrophilization of the photoresist layer surface, the experiment 1 using hydrogen + water vapor as the raw material gas obtained a high degree of hydrophilization effect ( Figure 6 Paragraph 4). Thus, a semiconductor substrate having a copper layer on its surface is etched using a photoresist, and in the pre-treatment when a plating treatment is performed, a plasma treatment is performed using a raw material gas composed of hydrogen and water, and the following effects can be significantly obtained: (1) preventing or reducing oxidation of the copper layer; (2) ashing of photoresist residues; (3) making the surface of the photoresist layer such as the inside of the through hole hydrophilic and allowing easy entry of the plating liquid. This plasma treatment is also effective in the case where it is necessary to prevent or reduce oxidation of metal parts such as the lead part (lead frame) and the electrode part of the semiconductor substrate in the mounting technology of connecting the lead part and the electrode part of the semiconductor substrate using a metal wire.

[0070] When hydrogen + water vapor is used as the raw material gas in the plasma treatment of the substrate, water vapor that is inevitably mixed into the hydrogen generated by the electrolysis device can be used directly by using an electrolysis device as performed in Experiment 1. When a high-pressure hydrogen cylinder is used as the hydrogen source, it is necessary to adjust specific equipment and deploy qualified personnel in accordance with laws such as the High-Pressure Gas Safety Act, so there are high practical obstacles, but this problem can also be avoided by using an electrolysis device.

[0071] When the raw material gas is hydrogen + water vapor, the ratio of water vapor therein is preferably 10 to 40% according to the results of Experiment 3. In this way, when the ratio of water vapor in the raw material gas is set to 10% or more (more precisely, when the pressure is set to be about 3.3% or more of the saturated vapor pressure of water), the hydrogen generated by the electrolysis device as described above (including water vapor at saturated vapor pressure) is not sufficient, so it is necessary to prepare a water vapor generator separately from the hydrogen source and add water vapor generated by it.

[0072] The inventors have proposed a plasma treatment method for reducing copper oxide and silver oxide by converting a mixed gas of water vapor and oxygen or a mixed gas of oxygen and hydrogen into plasma (Patent Document 2, Patent Document 3). However, an electrolysis device may also be used as a source for generating these mixed gases.

[0073] Explanation of symbols

[0074] 11: Substrate

[0075] 12: Copper layer

[0076] 13: Photoresist

[0077] 14: Through hole

[0078] 15: Plasma

[0079] 16: Copper

[0080] 20: Sample group

[0081] 21: Dummy substrate

[0082] 22: Copper oxide chip

[0083] 23: Silicon chip

[0084] 30: Plasma treatment device

[0085] 31: Processing Room

[0086] 32: Lower electrode

[0087] 33: Upper electrode

[0088] 34: High frequency power supply

[0089] 35: Vacuum pump

[0090] 36, 36a, 36b: Flow meter

[0091] 37: Electrolysis device

[0092] 38: High-pressure hydrogen cylinder

[0093] 39: Electrolysis device with water vapor capture device

[0094] 40: Steam generator

Claims

1. A plasma treatment method for a substrate for an electronic device, It is characterized in that It has the following steps: a) placing an electronic device substrate in a processing chamber; b) supplying a raw material gas consisting of hydrogen and water vapor obtained from a device for electrolyzing water to the above-mentioned treatment chamber; and c) performing plasma processing on the electronic device substrate by converting the source gas in the processing chamber into plasma.

2. The method for processing an electronic device substrate according to claim 1, in, Water vapor is further supplied into the processing chamber, and the mixing ratio of the source gas is set to hydrogen / water vapor=90 / 10 to 60 / 40.

3. The plasma treatment method for an electronic device substrate according to claim 1 or 2, in, The above-mentioned device for electrolyzing water does not include a water vapor capturing device.

4. The plasma treatment method for an electronic device substrate according to claim 1 or 2, in, The electronic device substrate has a photoresist layer and a copper layer on the surface.

5. A plasma processing device, It is characterized in that It has: a) a plasma processing chamber provided with a stage for mounting a substrate for an electronic device to be processed; b) a water electrolysis device, which is a supply source of a raw material gas consisting of hydrogen and water vapor connected to the above-mentioned treatment chamber; and c) A plasma generating unit that converts the source gas introduced into the processing chamber into plasma.

6. The plasma processing apparatus according to claim 5, in, The water electrolysis device described above does not include a water vapor capture device.

Citation Information

Patent Citations

  • Hydrogen plasma processing apparatus

    JP1994029254A

  • Plasma cleaning device

    JP2015160192A

  • Plasma processing method

    JP2018098353A