Preparation method of multi-layer high-filtering combined fiber medical protective mask
Through the preparation method of multi-layer high-filtration combined fibers, the problem of low filtration efficiency and low breathability of medical protective masks is solved, and the effect of efficient filtration and adsorption of particles is achieved.
Patent Information
- Application Number
- CN202411213538.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing medical protective masks have low filtration efficiency and low breathability, making it difficult to effectively block tiny particles and pathogens in the air.
By using the preparation method of multi-layer high-filtration combined fiber, the solution is formed by mixing and heating the components such as polypropylene pellets, polylactic acid, polyphenylene sulfide, electret masterbatch and nanofiber, and then processed by a melt spinning machine. High-filter non-woven fabrics, combined with composite spinning technology and meltblown technology, prepare high-efficiency filter layers, and impart fiber charges through high-voltage electric field to improve adsorption force.
It significantly improves the filtration efficiency and breathability of medical protective masks, achieves efficient interception and adsorption of particles, and provides better air filtration performance.
Smart Images

Figure CN119073690A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical protective masks, in particular to a method for preparing a multi-layer high-filtration combined fiber medical protective mask. Background Art
[0002] As an important equipment in the medical field and personal protection, the design and manufacture of medical protective masks integrates many advanced technologies, aiming to effectively block harmful substances such as microorganisms and particulate matter in the air, and protect the health and safety of the wearer and the people around them. The core of medical protective masks lies in their high-efficiency filtration layer, which usually adopts a multi-layer composite structure, including meltblown cloth as the main filtration material. Meltblown cloth is made through a special process and has a fine fiber structure, which can effectively intercept tiny particles in the air, such as bacteria, viruses and PM2.5, etc. However, the existing medical protective masks have low filtration efficiency and low air permeability, which is not conducive to use.
[0003] The defects of existing medical protective masks are:
[0004] 1. Patent document CN112500670A discloses a method for preparing a protective mask breathing valve film. "The preparation process is simple and the raw material sources are wide. The protective mask breathing valve film disclosed in the present invention is blended with zinc oxide composite silver antibacterial agent and grafted antibacterial eucommia gum and polybutadiene rubber. Even if the protective mask is in a warm and humid environment, which is conducive to the growth of bacteria, the natural antibacterial components of eucommia and the grafted composition and the composite silver antibacterial components contained in the breathing valve film can penetrate the entire rubber component, providing a complete protection from the surface to the core for the breathing valve, with good safety, no pungent smell, non-toxic and harmless." However, the existing medical protective masks have low filtration efficiency and low air permeability, which is not conducive to use;
[0005] 2. Patent document CN113235296A discloses a method for preparing a nano silver material, "including the following steps: washing and drying a substrate; modifying the substrate, wherein the modified substrate contains a ligand for chelating with nano silver ions, washing and drying; mixing the modified substrate with a solution containing silver ions; and causing a substitution reaction to prepare a final product containing nano silver. The present invention provides a method for preparing a nano silver material. Compared with the prior art, the nano silver material prepared by the present method has both adsorption and antibacterial functions, and the nano silver in the material prepared by the method has strong adhesion, is not easy to fall off, has stronger antiviral and antibacterial effects, and has longer durability. At the same time, biological macromolecules are used as raw materials for preparation, the process is green and environmentally friendly, and has stronger biocompatibility. The present invention also provides a mask using the nano silver material and a protective member using the nano silver material", but the existing medical protective masks have low filtration efficiency and low air permeability, which is not conducive to use;
[0006] 3. Patent document CN112370867A discloses a method for preparing a high-efficiency antibacterial protective mask filter layer. "Specifically, the method is implemented as follows: first, polystyrene and porous polyvinylidene fluoride nanofiber membranes are prepared by electrospinning technology combined with solid phase separation, and then inorganic antibacterial oxides are synthesized at the contact interface of the two fiber membranes by interfacial chemical reaction method and thermal curing treatment, thereby obtaining an efficient antibacterial protective mask filter layer with hydrophobic outer layer, antibacterial interface and piezoelectric inner layer. The hydrophobic outer layer of polystyrene effectively isolates external moisture and protects the piezoelectric inner layer; polyvinylidene fluoride is used as the piezoelectric inner layer to improve the electrostatic adsorption efficiency, and the porous structure improves the adsorption capacity for viruses. The inorganic antibacterial agent is synthesized by chemical reaction method combined with thermal curing treatment at the contact interface of the two fiber membranes to improve the filtration efficiency of the mask filter layer. The present invention can be used to improve the filtration effect of the mask filter layer, and can also be used in industrial filter paper, anti-smog window screens, anti-bacterial and waterproof fabrics, etc., and has great application value", but the existing medical protective masks have low filtration efficiency and low air permeability, which is not conducive to use;
[0007] 4. Patent document CN111926568A discloses a method for preparing an antibacterial meltblown cloth layer for a protective mask. "The method includes step S10, pre-configuring customized sialic acid ligand functional molecules; step S20, pre-functionalizing the meltblown cloth to obtain a functionalized meltblown cloth; step S30, chemically grafting the customized sialic acid ligand functional molecules onto the surface fibers of the functionalized meltblown cloth to form an antibacterial meltblown cloth layer; without changing the key filter material performance, the filter material is endowed with a broad-spectrum, high-efficiency active antibacterial function, and the surface of the filter material is modified and grafted with high-affinity customized sialic acid ligand functional molecules. The modified filter material captures a variety of pathogen particles by high-affinity recognition and binding to viral surface proteins, which can effectively avoid secondary diffusion contamination of adsorbed pathogen particles; directly modifying and grafting the mask filter material to improve the capture and fixation ability of pathogen particles without affecting the key filtering performance." However, the existing medical protective masks have low filtration efficiency and low air permeability, which is not conducive to use. Summary of the invention
[0008] The object of the present invention is to provide a method for preparing a multi-layer high-filtration combined fiber medical protective mask to solve the technical problem that the existing medical protective masks proposed in the above background technology have low filtration efficiency and low air permeability and are not conducive to use.
[0009] To achieve the above object, the present invention provides the following technical solution: a method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0010] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0011] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0012] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0013] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0014] The non-woven fabric b is a high-filtration non-woven fabric, which comprises the following components a in parts by weight: 30-45 parts of polypropylene pellets, 10-20 parts of polylactic acid, 15-25 parts of polyphenylene sulfide, 5-20 parts of electret masterbatch, 2-10 parts of nanofibers, and 3-8 parts of vanillin, which are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring kettle, and the temperature of the components a when mixed and heated is 50-60° C.;
[0015] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 70-100MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers. The high-filterability combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be of different size, and each layer of non-woven fabric is cut.
[0016] Preferably, the electret masterbatch is a nitrogen-containing chemical fatty acid, and the composite spinning technology is one of parallel composite spinning and sheath-core composite spinning.
[0017] Preferably, the cover body is composed of three layers of non-woven fabrics, and the three layers of non-woven fabrics are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded together.
[0018] Preferably, the cover body is formed by sewing or welding the layers of non-woven fabric together along the edges by a sewing machine or an ultrasonic welding machine, and the thickness of the non-woven fabric b is 0.5 mm to 0.7 mm.
[0019] Preferably, the nose bridge strip and the ear straps are fixed by heat pressing.
[0020] Preferably, the high-filtration combined fibers are charged by a high-voltage electric field to increase the adsorption capacity for particles.
[0021] Preferably, the high-filtration composite fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with free radicals on the surface of the high-filtration composite fiber to form a graft copolymer.
[0022] Preferably, the temperature in the sterilizer is 80-120° C., one end of the sterilizing nozzle in the sterilizer has a Z-shaped path, ethylene oxide sterilization is performed in the sterilizer, and the packaging machine is an automatic continuous packaging machine.
[0023] Preferably, the non-woven fabric b is folded.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention is provided with a non-woven fabric b to form a high-filtration non-woven fabric. The high-filtration non-woven fabric comprises the following components a in parts by weight: 33 parts of polypropylene pellets, 12 parts of polylactic acid, 28 parts of polyphenylene sulfide, 8 parts of electret masterbatch, 4 parts of nanofibers, and 4 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle. The temperature of the components a when mixed and heated is 50-60° C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by the spinning machine. During the spinning process, the temperature, pressure, and filament output of the spinning machine are adjusted. The speed parameter is used to control the diameter and shape of the fiber. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form a high-filterability combined fiber. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fiber into a composite fiber. The high-filterability combined fiber is melt-blown to form a non-woven fabric b, realizing the function of significantly improving the filtration efficiency of the multi-layer high-filterability combined fiber medical protective mask;
[0026] 2. The present invention is provided with a non-woven fabric b to form a high-filtration non-woven fabric. The high-filtration non-woven fabric comprises the following components a in parts by weight: 33 parts of polypropylene pellets, 12 parts of polylactic acid, 28 parts of polyphenylene sulfide, 8 parts of electret masterbatch, 4 parts of nanofibers, and 4 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle. The temperature of the components a when mixed and heated is 50-60° C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by the spinning machine. During the spinning process, the temperature, pressure, and outlet of the spinning machine are adjusted. The diameter and morphology of the fiber are controlled by the spinning speed parameter, the melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form a high-filterability combined fiber. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are melt-blown to form non-woven fabric b, thereby realizing the function of significantly improving the air permeability of multi-layer high-filterability combined fiber medical protective masks. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The experimental data of the present invention are shown in FIG. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.
[0030] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, it can be understood according to the specific situation.
[0031] Embodiment 1: An embodiment provided by the present invention: A method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0032] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0033] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0034] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0035] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0036] The non-woven fabric b is a high-filtration non-woven fabric, which includes the following components a in parts by weight: 33 parts of polypropylene pellets, 12 parts of polylactic acid, 28 parts of polyphenylene sulfide, 8 parts of electret masterbatch, 4 parts of nanofibers, and 4 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring tank, and the temperature of the components a when mixed and heated is 50-60° C.;
[0037] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filtration combined fibers. The high-filtration combined fiber composite spinning technology spins the mixed high-filtration combined fibers into composite fibers. The high-filtration combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be sized, and each layer of the non-woven fabric is cut. The electret masterbatch is a nitrogen-containing chemical fatty acid. The composite spinning technology is one of parallel composite spinning and skin-core composite spinning. The mask body has The mask body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded to each other in sequence. The mask body is sewed or welded together along the edges of each layer of non-woven fabric by a sewing machine or an ultrasonic welding machine. The thickness of non-woven fabric b is 0.5mm-0.7mm. The nose bridge and ear straps are fixed by hot pressing. The high-filtration combined fiber is charged with a high-voltage electric field to improve the adsorption capacity of particles. The high-filtration combined fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with the free radicals on the surface of the high-filtration combined fiber to form a graft copolymer. The temperature in the sterilizer is 80-120°C, and the path of one end of the disinfection nozzle in the sterilizer is Z-shaped. Ethylene oxide sterilization is performed in the sterilizer. The packaging machine is an automatic continuous packaging machine, and non-woven fabric b is foldable.
[0038] Embodiment 2: An embodiment provided by the present invention: A method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0039] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0040] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0041] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0042] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0043] The non-woven fabric b is a high-filtration non-woven fabric, which includes the following components a in parts by weight: 36 parts of polypropylene pellets, 14 parts of polylactic acid, 18 parts of polyphenylene sulfide, 15 parts of electret masterbatch, 6 parts of nanofibers, and 5 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring tank, and the temperature of the components a when mixed and heated is 50-60° C.;
[0044] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 90MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filtration combined fibers. The high-filtration combined fiber composite spinning technology spins the mixed high-filtration combined fibers into composite fibers. The high-filtration combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be sized, and each layer of the non-woven fabric is cut. The electret masterbatch is a nitrogen-containing chemical fatty acid. The composite spinning technology is one of parallel composite spinning and skin-core composite spinning. The mask body has The mask body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded to each other in sequence. The mask body is sewed or welded together along the edges of each layer of non-woven fabric by a sewing machine or an ultrasonic welding machine. The thickness of non-woven fabric b is 0.5mm-0.7mm. The nose bridge and ear straps are fixed by hot pressing. The high-filtration combined fiber is charged with a high-voltage electric field to improve the adsorption capacity of particles. The high-filtration combined fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with the free radicals on the surface of the high-filtration combined fiber to form a graft copolymer. The temperature in the sterilizer is 80-120°C, and the path of one end of the disinfection nozzle in the sterilizer is Z-shaped. Ethylene oxide sterilization is performed in the sterilizer. The packaging machine is an automatic continuous packaging machine, and non-woven fabric b is foldable.
[0045] Embodiment 3: An embodiment provided by the present invention: A method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0046] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0047] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0048] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0049] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0050] The non-woven fabric b is a high-filtration non-woven fabric, which includes the following components a in parts by weight: 39 parts of polypropylene pellets, 18 parts of polylactic acid, 21 parts of polyphenylene sulfide, 16 parts of electret masterbatch, 8 parts of nanofibers, and 6 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring tank, and the temperature of the components a when mixed and heated is 50-60° C.;
[0051] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 85MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filtration combined fibers. The high-filtration combined fiber composite spinning technology spins the mixed high-filtration combined fibers into composite fibers. The high-filtration combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be sized, and each layer of the non-woven fabric is cut. The electret masterbatch is a nitrogen-containing chemical fatty acid. The composite spinning technology is one of parallel composite spinning and skin-core composite spinning. The mask body has The mask body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded to each other in sequence. The mask body is sewed or welded together along the edges of each layer of non-woven fabric by a sewing machine or an ultrasonic welding machine. The thickness of non-woven fabric b is 0.5mm-0.7mm. The nose bridge and ear straps are fixed by hot pressing. The high-filtration combined fiber is charged with a high-voltage electric field to improve the adsorption capacity of particles. The high-filtration combined fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with the free radicals on the surface of the high-filtration combined fiber to form a graft copolymer. The temperature in the sterilizer is 80-120°C, and the path of one end of the disinfection nozzle in the sterilizer is Z-shaped. Ethylene oxide sterilization is performed in the sterilizer. The packaging machine is an automatic continuous packaging machine, and non-woven fabric b is foldable.
[0052] Embodiment 4: An embodiment provided by the present invention: A method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0053] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0054] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0055] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0056] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0057] The non-woven fabric b is a high-filtration non-woven fabric, which includes the following components a in parts by weight: 42 parts of polypropylene pellets, 18 parts of polylactic acid, 22 parts of polyphenylene sulfide, 17 parts of electret masterbatch, 7 parts of nanofibers, and 6 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring tank, and the temperature of the components a when mixed and heated is 50-60° C.;
[0058] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filtration combined fibers. The high-filtration combined fiber composite spinning technology spins the mixed high-filtration combined fibers into composite fibers. The high-filtration combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be sized, and each layer of the non-woven fabric is cut. The electret masterbatch is a nitrogen-containing chemical fatty acid. The composite spinning technology is one of parallel composite spinning and skin-core composite spinning. The mask body has The mask body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded to each other in sequence. The mask body is sewed or welded together along the edges of each layer of non-woven fabric by a sewing machine or an ultrasonic welding machine. The thickness of non-woven fabric b is 0.5mm-0.7mm. The nose bridge and ear straps are fixed by hot pressing. The high-filtration combined fiber is charged with a high-voltage electric field to improve the adsorption capacity of particles. The high-filtration combined fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with the free radicals on the surface of the high-filtration combined fiber to form a graft copolymer. The temperature in the sterilizer is 80-120°C, and the path of one end of the disinfection nozzle in the sterilizer is Z-shaped. Ethylene oxide sterilization is performed in the sterilizer. The packaging machine is an automatic continuous packaging machine, and non-woven fabric b is foldable.
[0059] Embodiment 5: An embodiment provided by the present invention: A method for preparing a multi-layer high-filtration combined fiber medical protective mask, comprising the following steps:
[0060] Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body;
[0061] Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the layer of non-woven fabric b in step 1;
[0062] Step 3, bonding ear straps to the surface of the mask body according to step 2 to form a mask;
[0063] Step 4, sterilizing the mask in step 3 by a sterilizer and then packaging it by a packaging machine;
[0064] The non-woven fabric b is a high-filtration non-woven fabric, which includes the following components a in parts by weight: 44 parts of polypropylene pellets, 19 parts of polylactic acid, 24 parts of polyphenylene sulfide, 19 parts of electret masterbatch, 9 parts of nanofibers, and 8 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring tank, and the temperature of the components a when mixed and heated is 50-60° C.;
[0065] Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 95MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filtration combined fibers. The high-filtration combined fiber composite spinning technology spins the mixed high-filtration combined fibers into composite fibers. The high-filtration combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be sized, and each layer of the non-woven fabric is cut. The electret masterbatch is a nitrogen-containing chemical fatty acid. The composite spinning technology is one of parallel composite spinning and skin-core composite spinning. The mask body has The mask body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded to each other in sequence. The mask body is sewed or welded together along the edges of each layer of non-woven fabric by a sewing machine or an ultrasonic welding machine. The thickness of non-woven fabric b is 0.5mm-0.7mm. The nose bridge and ear straps are fixed by hot pressing. The high-filtration combined fiber is charged with a high-voltage electric field to improve the adsorption capacity of particles. The high-filtration combined fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with the free radicals on the surface of the high-filtration combined fiber to form a graft copolymer. The temperature in the sterilizer is 80-120°C, and the path of one end of the disinfection nozzle in the sterilizer is Z-shaped. Ethylene oxide sterilization is performed in the sterilizer. The packaging machine is an automatic continuous packaging machine, and non-woven fabric b is foldable.
[0066] Comparative experiment:
[0067] The difference between Comparative Example 1 and Example 1 is that the non-woven fabric b is a high-filtration non-woven fabric, and the high-filtration non-woven fabric comprises the following components a in parts by weight, 33 parts of polypropylene pellets, 12 parts of polylactic acid, 28 parts of polyphenylene sulfide, 8 parts of electret masterbatch, 4 parts of nanofibers, and 4 parts of vanillin, which are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle, and the temperature of the components a when mixed and heated is 50-60°C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by a spinning machine. The spinning process During the process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure and spinning speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are formed into non-woven fabric b by melt-blowing.
[0068] The difference between Comparative Example 1 and Example 2 is that the non-woven fabric b is a high-filtration non-woven fabric, which comprises the following components a in parts by weight: 36 parts of polypropylene pellets, 14 parts of polylactic acid, 18 parts of polyphenylene sulfide, 15 parts of electret masterbatch, 6 parts of nanofibers, and 5 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle. The temperature of the components a when mixed and heated is 50-60°C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by a spinning machine. The spinning process During the process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure and spinning speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 90MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are formed into non-woven fabric b by melt-blowing.
[0069] The difference between Comparative Example 1 and Example 3 is that the non-woven fabric b is a high-filtration non-woven fabric, which comprises the following components a in parts by weight: 39 parts of polypropylene pellets, 18 parts of polylactic acid, 21 parts of polyphenylene sulfide, 16 parts of electret masterbatch, 8 parts of nanofibers, and 6 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle. The temperature of the components a when mixed and heated is 50-60°C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by a spinning machine. The spinning process During the process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure and spinning speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 85MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are formed into non-woven fabric b by melt-blowing.
[0070] The difference between Comparative Example 1 and Example 4 is that the non-woven fabric b is a high-filtration non-woven fabric, and the high-filtration non-woven fabric comprises the following components a in parts by weight, 42 parts of polypropylene pellets, 18 parts of polylactic acid, 22 parts of polyphenylene sulfide, 17 parts of electret masterbatch, 7 parts of nanofibers, and 6 parts of vanillin, which are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle, and the temperature of the components a when mixed and heated is 50-60°C. The solution a is placed in a melt spinning machine, melt-extruded into filaments, and spun by a spinning machine. The spinning process During the process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure and spinning speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 75MPa, and the spinning speed of the spinning machine is 0.2-0.5mL / h. The solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are formed into non-woven fabric b by melt-blowing.
[0071] The difference between Comparative Example 1 and Example 5 is that the non-woven fabric b is a high-filtration non-woven fabric, which comprises the following components a in parts by weight: 44 parts of polypropylene pellets, 19 parts of polylactic acid, 24 parts of polyphenylene sulfide, 19 parts of electret masterbatch, 9 parts of nanofibers, and 8 parts of vanillin are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed by a stirring kettle. The temperature of the components a when mixed and heated is 50 ~ 60℃, solution a is put into a melt spinning machine, melted and extruded into filaments, and then spun by the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure and filament speed parameters of the spinning machine. The melting temperature is 230 ~ 360℃, the spinning machine temperature is 120~ 150℃, the internal pressure of the spinning machine is 95MPa, the spinning speed of the spinning machine is 0.2~0.5mL / h, the solution a is processed by the spinning machine to form high-filterability combined fibers, the high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers, and the high-filterability combined fibers are melt-blown to form non-woven fabric b.
[0072] The multi-layer high-filtration combined fiber medical protective masks of Examples 1, 2, 3, 4 and 5 of the present invention and the traditional mask (Comparative Example 1) were subjected to filtration efficiency and inhalation resistance tests under GB 19083-2010, and their filtration efficiency values were calculated and statistically analyzed. The results are as follows:
[0073] As shown in Table 1:
[0074] Air flow (L / min) Filtration efficiency (%) Example 1 82 98 Example 2 83 97 Example 3 83 98 Example 4 85 96 Example 5 86 98 Comparative Example 1 75 90
[0075] Table 1
[0076] From the data in Table 1, it can be seen that the filtration efficiencies of the multi-layer high-filtration combined fiber medical protective masks in Examples 1, 2, 3, 4 and 5 of the present invention are 98, 97, 98, 96 and 98, respectively, which are significantly higher than the filtration efficiency of the traditional mask in Comparative Example 1. Therefore, it is shown that the filtration efficiency of the multi-layer high-filtration combined fiber medical protective mask of the present invention is significantly improved.
[0077] From the data in Table 1, it can be seen that the airflow rates of the multi-layer high-filtration combined fiber medical protective masks in Examples 1, 2, 3, 4 and 5 of the present invention are 82, 83, 83, 85 and 86 respectively, which are significantly higher than the airflow rate of the traditional mask in Comparative Example 1. Therefore, it is shown that the air permeability of the multi-layer high-filtration combined fiber medical protective mask of the present invention is significantly improved.
[0078] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a multi-layer high-filtration combined fiber medical protective mask, characterized in that: The following steps are involved: Step 1, bonding two layers of non-woven fabric a and one layer of non-woven fabric b to form a cover body; Step 2, bonding the nose bridge strip between the two layers of non-woven fabric a and the one layer of non-woven fabric b in step 1; Step 3, bonding ear straps to the surface of the mask body in step 2 to form a mask; Step 4, sterilizing the mask in step 3 through a sterilizer and then packaging it through a packaging machine; The non-woven fabric b is a high-filtration non-woven fabric, which comprises the following components a in parts by weight: 30-45 parts of polypropylene pellets, 10-20 parts of polylactic acid, 15-25 parts of polyphenylene sulfide, 5-20 parts of electret masterbatch, 2-10 parts of nanofibers, and 3-8 parts of vanillin, which are mixed and heated to form a solution a. When the components a are mixed and heated, they are mixed in a stirring kettle, and the temperature of the components a when mixed and heated is 50-60° C.; Solution a is put into a melt spinning machine, melt-extruded into filaments, and spun through the spinning machine. During the spinning process, the diameter and shape of the fiber are controlled by adjusting the temperature, pressure, and filament output speed parameters of the spinning machine. The melting temperature is 230-360°C, the temperature of the spinning machine is 120-150°C, the internal pressure of the spinning machine is 70-100MPa, and the filament output speed of the spinning machine is 0.2-0.5mL / h. Solution a is processed by the spinning machine to form high-filterability combined fibers. The high-filterability combined fiber composite spinning technology spins the mixed high-filterability combined fibers into composite fibers. The high-filterability combined fibers are melt-blown to form non-woven fabric b. The mask is designed to be of different size, and each layer of non-woven fabric is cut.
2. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The electret masterbatch is a nitrogen-containing chemical fatty acid, and the composite spinning technology is one of parallel composite spinning and skin-core composite spinning.
3. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The cover body is composed of three layers of non-woven fabrics, which are non-woven fabric a, non-woven fabric b, and non-woven fabric a bonded together in sequence.
4. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The cover body is made by sewing or welding the layers of non-woven fabrics together along the edges by a sewing machine or an ultrasonic welding machine, and the thickness of the non-woven fabric b is 0.5 mm to 0.7 mm.
5. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The nose bridge strip and the ear straps are fixed by a heat pressing method.
6. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The high-filtration combined fibers are charged by a high-voltage electric field to improve the adsorption of particles.
7. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The high-filtration composite fiber is placed in a solution of acrylic acid or vinyl silane, and the acrylic acid or vinyl silane monomer reacts with free radicals on the surface of the high-filtration composite fiber to form a graft copolymer.
8. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 1, characterized in that: The temperature in the sterilizer is 80-120° C., one end of the sterilizing nozzle in the sterilizer has a Z-shaped path, ethylene oxide sterilization is performed in the sterilizer, and the packaging machine is an automatic continuous packaging machine.
9. The method for preparing a multi-layer high-filtration combined fiber medical protective mask according to claim 3, characterized in that: The nonwoven fabric b is folded.
Citation Information
Patent Citations
Cyclic regeneration medical protective mask, preparation method and cyclic regeneration method
CN112120317A
Low-resistance protective mask and preparation method thereof
CN113142712A
Multi-stage fiber multifunctional gradient filtering material and preparation method thereof
CN113426202A
Antimicrobial mask and preparation method thereof
CN117859979A
Method for producing extra fine fiber non-woven fabric, and apparatus for producing the same
JP2010185153A