Cartilage regeneration scaffold based on 3D printing of collagen Pickering emulsion and preparation method of cartilage regeneration scaffold

By collagen Pickering emulsion as a biomaterial ink, combined with 3D printing and freeze-drying technology, the problems of poor printability and poor pattern retention in 3D printing were solved, and a cartilage regeneration scaffold with high precision and porous structure were prepared. Improves the survival environment and repair efficiency of chondrocytes.

CN119075003AActive Publication Date: 2024-12-06FUJIAN UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410983082.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-12-06
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

The prior art is difficult to prepare cartilage regeneration scaffolds with high precision, porosity and biological activity. The collagen solution has poor printability during 3D printing and poor model retention after extrusion, which cannot meet the high-finement requirements of cartilage regeneration scaffolds. .

Method used

Collagen Pickering emulsion is used as biomaterial ink, and collagen molecules are wrapped on the surface of the droplets through emulsion to form emulsion microspheres, improving printability and post-extrusion model retention ability, combining 3D printing and freeze-drying technology to form a customized large Pore ​​structure and abundant microporous structure.

Benefits of technology

The cartilage regeneration scaffold is achieved with high precision, good thixotropy and type-retaining properties, providing an ideal living environment and nutritional supply efficiency, providing biological activity for chondrocytes, and enhancing tissue repair capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119075003A_ABST
    Figure CN119075003A_ABST
Patent Text Reader

Abstract

The invention discloses a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing and a preparation method of the cartilage regeneration scaffold. The method comprises the following steps: extracting collagen from a fresh collagen extraction raw material to obtain purified collagen sponge, dissolving the collagen sponge in acetic acid to obtain a high-concentration collagen solution, adding an oil phase into the collagen solution, carrying out high-speed emulsification by using a high-speed homogenizer to obtain a collagen-based Pickering emulsion, and finally carrying out computer digital modeling and low-temperature hydrogel forming equipment to obtain the collagen-based Pickering emulsion. The collagen-based Pickering emulsion is used as biological material ink for 3D printing of a cartilage regeneration hydrogel scaffold, the printed scaffold is rapidly frozen in liquid nitrogen and then subjected to vacuum drying, and the cartilage regeneration scaffold is obtained. The collagen Pickering emulsion biological material ink with excellent printability is developed, and the collagen-based cartilage regeneration scaffold which is excellent in formability, adjustable in pore structure and good in biological activity is rapidly customized through 3D printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of biomedical materials, and in particular relates to a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing and a preparation method thereof. Background Art

[0002] Cartilage is a special connective tissue that is mainly distributed in many parts of the human body, such as joints, nose, ears or trachea. The density of chondrocytes is low (consisting of about 1% chondrocytes and 99% extracellular matrix), and there are no other tissues such as blood vessels, nerves or lymphatic tissues, resulting in its weak self-repair ability. Various diseases after cartilage defects (arthritis, sinusitis or bronchitis, etc.) can easily have a significant impact on patients' daily life and personal health, severely limiting the function of damaged organs and personal motor ability. Therefore, tissue repair after cartilage defects is a long-standing clinical challenge and a world-class problem that troubles clinicians. At present, the commonly used methods for clinical treatment of cartilage defects mainly include microfracture, autologous cartilage or chondrocyte transplantation, and implantation of non-degradable prostheses. Although this type of treatment has achieved certain efficacy, there are still problems such as donor damage, long treatment cycle and implant infection. Tissue engineering technology provides a clinical option with great application prospects for cartilage repair. Implanting cell-loaded cartilage tissue engineering regeneration scaffolds into the defect site for wound repair is an ideal clinical treatment method.

[0003] The ideal cartilage tissue engineering regeneration scaffold must perfectly simulate the living environment of chondrocytes and have excellent bioactivity, biocompatibility and appropriate biodegradability. At the same time, the scaffold should have both high porosity and a multi-level pore structure that is interconnected; the larger pores provide an ideal environment for cells to proliferate, migrate and secrete extracellular matrix, while the smaller pores provide channels for the transport of nutrients and the discharge of metabolic waste. In addition, cartilage has an extremely rich and fine three-dimensional structure, with large individual differences in age and gender, and the degree of defect varies among patients. Therefore, it is extremely challenging to construct a highly porous, refined and customized cartilage regeneration tissue engineering scaffold with bioactivity.

[0004] In recent years, 3D bioprinting technology has been widely used in rapid prototyping of tissue engineering. It customizes high-precision scaffold contours and internal pore structures through digital modeling, and is particularly suitable for preparing cartilage regeneration scaffold materials with complex internal and external structures. The extracellular matrix of cartilage cells is mainly composed of a large amount of collagen and a small amount of glycosaminoglycans. Collagen has excellent biocompatibility and biodegradability, and has biological activity that promotes cell proliferation, differentiation and secretion of extracellular matrix. Therefore, collagen used in cartilage regeneration scaffolds can perfectly simulate the living environment of chondrocytes and is a very ideal tissue engineering material. The development of collagen-based biomaterial ink can not only make high-value use of biomass polymer materials, but also meet the major strategic needs of my country for the development of the big health industry and the transformation of economic development methods for biomedical materials.

[0005] The collagen solution has poor plasticity during the 3D printing process. The low-concentration collagen solution will immediately experience leveling after extrusion. The high-concentration collagen solution has many entanglement sites of collagen molecular chains, resulting in a high yield stress, which makes it difficult to extrude smoothly from the needle. After increasing the extrusion pressure, it is difficult to ensure the continuity and uniformity of the extrusion. In addition, the collagen solution has the extrusion swelling effect of polymer materials. After increasing the extrusion pressure, this effect is more obvious, thus affecting the shape retention of the scaffold. In order to solve the problem that low-concentration collagen is difficult to shape, the researchers directly extruded the collagen solution into a high-viscosity support bath (gelatin, carbomer, etc.) to assist in the extrusion of filaments. After the printing is completed, the viscosity of the support bath is reduced by changing the temperature, pH value or ionic strength to separate the printed materials. However, the lines extruded by a thinner needle with high printing accuracy are difficult to retain in a high-viscosity support bath. Therefore, this printing method usually sacrifices printing accuracy and uses a thicker needle for extrusion, which cannot meet the high-precision requirements of cartilage regeneration scaffolds. Summary of the invention

[0006] The purpose of the present invention is to provide a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing and a preparation method thereof. First, a collagen Pickering emulsion biomaterial ink with excellent printability is prepared, and then a collagen-based cartilage regeneration scaffold with good formability, adjustable pore structure and good biological activity is quickly customized through 3D printing.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: A method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing, comprising the following steps: 1) Extraction of collagen Wash and chop the fresh collagen extraction raw material, add sodium carbonate solution, shake at 4°C for 10-14h to remove impurities, add 0.1-0.7 mol / L acetic acid at a liquid-to-solid ratio of 30-50:1, then add pepsin at a mass of 1-3% of the raw material, stir at 4°C for 72-80h, collect the supernatant by centrifugation at 8000-9000 r / min, and continuously add sodium chloride to the supernatant to precipitate collagen solid precipitate, the final concentration of sodium chloride is 0.1-1 mol / L, use acetic acid to dissolve the collagen solid precipitate, after complete dissolution, dialyze the solution for more than 72h, collect the intercepted liquid, place it in a vacuum freeze-drying at -50°C to obtain a purified collagen sponge, and store the collagen sponge in a constant temperature, dry and dark place at 4°C; 2) Preparation of collagen-based Pickering emulsion The collagen sponge is dissolved in acetic acid to obtain a high-concentration collagen solution, and a high-speed homogenizer is used to stir the solution at a speed of 5000-10000 r / min for 1-3 min to assist in uniform dissolution. Then, the oil phase is added to the collagen solution, and the solution is emulsified at a high speed of 8000-20000 r / min for 2-5 min to obtain a collagen-based Pickering emulsion. 3) Preparation of collagen-based cartilage regeneration scaffold Using computer digital modeling and low-temperature hydrogel molding equipment, collagen-based Pickering emulsion was used as the biomaterial ink for 3D printing of cartilage regeneration hydrogel scaffolds. The printed scaffolds were quickly frozen in liquid nitrogen and then vacuum dried at -50~-150℃ to obtain cartilage regeneration scaffolds.

[0008] Furthermore, the collagen extraction raw material in step 1) is animal skin, tendon or bone.

[0009] Furthermore, the concentration of the sodium carbonate solution in step 1) is 1-5%.

[0010] Furthermore, the concentration of acetic acid in step 1) is 0.1-0.7 mol / L, and the concentration of pepsin is 1-3%.

[0011] Furthermore, the concentration of acetic acid in step 2) is 0.1-0.7 mol / L, and the concentration of the obtained collagen solution is 40-80 mg / mL.

[0012] Furthermore, the oil phase in step 2) is soybean oil, tea tree essential oil, cyclohexane, dichloromethane, toluene, etc.

[0013] Furthermore, the mass ratio of the collagen solution to the oil phase in step 2) is 3:7-9:1, such as 9:1, 8:2, 7:3, 6:4, 5:5, 4:6 or 3:7.

[0014] Furthermore, the cartilage regeneration hydrogel scaffold described in step 3) is a meniscus regeneration hydrogel, a nasal regeneration hydrogel, an auricle regeneration hydrogel, etc.

[0015] In recent years, the collagen molecular chains in the collagen solution have been proven to be stable at the water-oil interface to form a Pickering emulsion. The present invention uses collagen Pickering emulsion as a biomaterial ink to print cartilage regeneration scaffolds, which has the following beneficial effects: 1. Since the distance between high-concentration collagen molecular chains is relatively close, the internal friction between molecules is large. The present invention emulsifies the collagen solution into a collagen Pickering emulsion, and the collagen molecules are wrapped on the surface of the droplets through emulsification, thereby converting the sliding friction between the molecules into rolling friction of the emulsion microspheres, improving the poor printability of collagen and the weak shape retention after extrusion, and can break through the application limitations of the poor printability of collagen solutions. 2. The emulsion microspheres can be adaptively rearranged during the extrusion process to adapt to different shear stresses, resulting in good thixotropy, good shape retention after extrusion, and a high-precision scaffold can be obtained. Therefore, using collagen Pickering emulsion as ink, 3D printing and freeze drying (Pickering emulsion template method) can form a customized macroporous structure, and a rich and interconnected microporous structure can be formed inside the printed filaments. 3. After the collagen-based cartilage regeneration scaffold formed by this method is inoculated with chondrocytes, collagen can act as an artificial extracellular matrix to provide biological activity for chondrocytes; the rich and multi-level interconnected macro-microporous structure provides an ideal living environment for chondrocytes and improves the efficiency of nutrient supply and waste discharge. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The printed line effect diagram (above) and optical microscope image (below) of collagen Pickering emulsion and collagen solution; (a) is collagen Pickering emulsion; (b) is collagen solution with the same solid content.

[0017] Figure 2 The renderings of the meniscus, nose and auricle models printed with collagen Pickering emulsion and collagen solution; (a) is the collagen Pickering emulsion; (b) is the collagen solution with the same solid content. DETAILED DESCRIPTION Example 1

[0018] (1) Wash and chop fresh cowhide, add 1% sodium carbonate solution, shake at 4℃ for 12h to remove impurities, and add 0.1 mol / L acetic acid solution at a liquid-to-solid ratio of 30:1. Then add pepsin at a mass ratio of 3% of the raw material. After stirring at 4℃ for 72h, collect the supernatant by centrifugation at 8000 r / min, and continuously add sodium chloride to the supernatant to precipitate collagen. The final concentration of sodium chloride is 1 mol / L. Use 0.5 mol / L acetic acid to dissolve the collagen solid precipitate. After it is completely dissolved, dialyze the solution for more than 72h. Collect the intercepted liquid and freeze-dry it at -50℃ to obtain the purified collagen sponge, and store the extracted collagen sponge in a constant temperature, dry and dark place at 4℃.

[0019] (2) Dissolve the collagen sponge in 0.1 mol / L acetic acid to obtain a high-concentration collagen solution with a concentration of 60 mg / mL, and stir it at high speed for 1 min with a high-speed homogenizer at a speed of 5000 r / min to assist uniform dissolution. Add cyclohexane to the collagen solution at a water-oil ratio of 7:3, and emulsify it at high speed for 2 min with a high-speed homogenizer at a speed of 15000 r / min to obtain a collagen-based Pickering emulsion.

[0020] (3) Using computer digital modeling and low-temperature hydrogel molding equipment, collagen-based Pickering emulsion was used as biomaterial ink to 3D print cartilage regeneration hydrogel scaffolds (printing meniscus, nose and auricle respectively). The printed scaffolds were frozen in liquid nitrogen and then vacuum dried at -50°C to obtain cartilage regeneration scaffolds. Example 2

[0021] (1) Wash and chop the fresh fish skin, add a 5% sodium carbonate solution, shake at 4°C for 12 hours to remove impurities, and add 0.7 mol / L acetic acid solution at a liquid-to-solid mass ratio of 50:1. Subsequently, add pepsin at a mass ratio of 1% of the raw material. After stirring at 4°C for 72 hours, collect the supernatant by centrifugation at 8000 r / min, and continuously add sodium chloride to the supernatant to precipitate collagen, with a final sodium chloride concentration of 0.2 mol / L. Use 0.7 mol / L acetic acid to dissolve the collagen solid precipitate. After it is completely dissolved, dialyze the solution for more than 72 hours, collect the intercepted flow, and vacuum freeze-dry at -50°C to obtain a purified collagen sponge, and store the extracted collagen sponge in a constant temperature, dry and dark place at 4°C.

[0022] (2) Dissolve the collagen sponge in 0.3 mol / L acetic acid to obtain a high-concentration collagen solution with a concentration of 70 mg / mL, and stir it at high speed for 2 min with a high-speed homogenizer at a speed of 8000 r / min to assist uniform dissolution. Add tea tree essential oil to the collagen solution at a water-oil ratio of 6:4, and emulsify it at high speed for 4 min with a high-speed homogenizer at a speed of 18000 r / min to obtain a collagen-based Pickering emulsion.

[0023] (3) Using computer digital modeling and low-temperature hydrogel molding equipment, collagen-based Pickering emulsion was used as biomaterial ink to 3D print auricular cartilage regeneration hydrogel scaffolds. The printed scaffolds were frozen in liquid nitrogen and then vacuum dried at -150°C to obtain cartilage regeneration scaffolds. Example 3

[0024] (1) Wash and chop the fresh bovine Achilles tendon, add a 2% sodium carbonate solution, shake at 4°C for 12 hours to remove impurities, and add 0.4 mol / L acetic acid solution at a liquid-to-solid mass ratio of 50:1. Subsequently, add pepsin at a mass ratio of 2% of the raw material. After stirring at 4°C for 72 hours, collect the supernatant by centrifugation at 8000 r / min, and continuously add sodium chloride to the supernatant to precipitate collagen. The final concentration of sodium chloride is 0.4 mol / L. Use 0.3 mol / L acetic acid to dissolve the collagen solid precipitate. After it is completely dissolved, dialyze the solution for more than 72 hours, collect the intercepted liquid, and vacuum freeze-dry at -50°C to obtain a purified collagen sponge. The extracted collagen sponge is stored in a constant temperature, dry and dark place at 4°C.

[0025] (2) Dissolve the collagen sponge in 0.5 mol / L acetic acid to obtain a high-concentration collagen solution with a concentration of 80 mg / mL, and stir it at high speed for 3 min with a high-speed homogenizer at a speed of 10,000 r / min to assist uniform dissolution. Add dichloromethane to the collagen solution at a water-oil ratio of 3:7, and emulsify it at high speed for 2 min with a high-speed homogenizer at a speed of 20,000 r / min to obtain a collagen-based Pickering emulsion.

[0026] (3) Using computer digital modeling and low-temperature hydrogel molding equipment, collagen-based Pickering emulsion was used as biomaterial ink to 3D print tracheal cartilage regeneration hydrogel scaffolds. The printed scaffolds were frozen in liquid nitrogen and then vacuum dried at -50°C to obtain cartilage regeneration scaffolds. Comparative Example 1

[0027] Computer digital modeling and low-temperature hydrogel molding equipment were used to 3D print auricular cartilage regeneration hydrogel scaffolds (printing meniscus, nose and auricle respectively) using the collagen solution (i.e., not emulsified) in step (2) of Example 1 as biomaterial ink. The printed scaffolds were frozen in liquid nitrogen and then vacuum dried at -150°C to obtain cartilage regeneration scaffolds.

[0028] Printing effect: By comparing Example 1 and Comparative Example 1, it can be seen that compared with the unemulsified collagen solution, the print line uniformity of the collagen Pickering emulsion is significantly enhanced, and the line size fidelity is stronger, see Figure 1 Under the same printing conditions, the overall structure of the meniscus, nose and auricle was printed. The collagen Pickering emulsion has good self-supporting ability and can form an ideal stacking structure and a clear hollow structure. However, the collagen solution has poor shape retention due to factors such as extrusion swelling, leveling and gravity, and the printed structure eventually collapsed. Figure 2 .

Claims

1. A method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing, characterized in that: The following steps are involved: 1) Extraction of collagen The fresh collagen extraction raw material is washed and chopped, and a sodium carbonate solution is added. The solution is shaken to remove impurities, and an acetic acid solution is added at a liquid-to-solid mass ratio of 30-50:

1. Subsequently, pepsin is added, and the mixture is stirred at 4°C for 72-80 hours. The supernatant is collected by centrifugation, and sodium chloride is continuously added to the supernatant to precipitate a collagen solid precipitate. The final concentration of sodium chloride is 0.1-1 mol / L. Acetic acid is used to dissolve the collagen solid precipitate. After the collagen solid precipitate is completely dissolved, the solution is dialyzed for more than 72 hours, and the intercepted liquid is collected and vacuum freeze-dried to obtain a purified collagen sponge. 2) Preparation of collagen-based Pickering emulsion The collagen sponge is dissolved in acetic acid to obtain a high-concentration collagen solution, and a high-speed homogenizer is used to stir the solution to assist in uniform dissolution. An oil phase is then added to the collagen solution, and the solution is emulsified at high speed using a high-speed homogenizer to obtain a collagen-based Pickering emulsion. 3) Preparation of collagen-based cartilage regeneration scaffold Using computer digital modeling and low-temperature hydrogel molding equipment, collagen-based Pickering emulsion was used as the biomaterial ink for 3D printing of cartilage regeneration hydrogel scaffolds. The printed scaffolds were quickly frozen in liquid nitrogen and then vacuum dried at -50~-150℃ to obtain cartilage regeneration scaffolds.

2. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The raw material for collagen extraction in step 1) is animal skin, tendon or bone.

3. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The concentration of the sodium carbonate solution in step 1) is 1-5%.

4. A method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The concentration of acetic acid in step 1) is 0.1-0.7 mol / L, and the amount of pepsin added is 1-3% of the mass of the raw material.

5. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The shaking temperature of step 1) is 4°C, the shaking time is 10-14h, and the vacuum freeze-drying temperature is -50°C.

6. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The concentration of acetic acid in step 2) is 0.1-0.7 mol / L, and the concentration of the obtained collagen solution is 40-80 mg / mL.

7. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: Step 2) The oil phase is soybean oil, tea tree essential oil, cyclohexane, dichloromethane or toluene, and the mass ratio of the collagen solution to the oil phase is 3:7-9:

1.

8. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that In step 2), the rotation speed of the high-speed homogenizer for assisting uniform dissolution is 5000-10000 r / min, the stirring time is 1-3 min, and the rotation speed of the high-speed homogenizer for emulsification is 8000-20000 r / min, and the weakening time is 2-5 min.

9. The method for preparing a cartilage regeneration scaffold based on collagen Pickering emulsion 3D printing according to claim 1, characterized in that: The cartilage regeneration hydrogel scaffold described in step 3) is a meniscus regeneration hydrogel, a nasal regeneration hydrogel, an auricle regeneration hydrogel, etc.

10. A cartilage regeneration scaffold obtained according to the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method of bionics filling material for repairing knee joint cartilage defects

    CN110237306A

  • Mechanically self-enhanced collagen-based cornea repair material and preparation method thereof

    CN117126437A

  • 3D printing Pickering emulsion ink co-stabilized by double nano particles as well as preparation method and application of 3D printing Pickering emulsion ink

    CN117551353A

  • Bioink, molded body, article, and method for producing molded body

    US20240174976A1