Drying agent as well as preparation method and application thereof
A desiccant composition with magnesium chloride, magnesium oxide, and additives addresses the issues of liquefaction and corrosion in LED headlights by maintaining neutral pH and preventing agglomeration, ensuring effective and long-lasting moisture absorption.
Patent Information
- Application Number
- CN202411193303.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Current car lamp desiccants fail to meet the requirements of high hygroscopicity, corrosion resistance, anti-agglomeration, and fast demisting, leading to liquefaction, corrosion, and volume expansion issues, which affect the performance and longevity of LED headlights.
A desiccant composition comprising magnesium chloride, magnesium oxide, a pH adjuster, dispersant, and moisture absorption control agent, which maintains neutral pH, prevents agglomeration, and regulates moisture absorption, ensuring long-term moisture absorption and anti-corrosion.
The desiccant maintains a neutral pH, prevents liquefaction and agglomeration, and extends moisture absorption life, enhancing the performance and longevity of LED headlights by maintaining efficient moisture removal and preventing corrosion.
Smart Images

Figure BDA0005015672150000021 
Figure BDA0005015672150000061 
Figure BDA0005015672150000062
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additives, and in particular to a desiccant and a preparation method and application thereof. Background Art
[0002] With the popularity of new energy vehicles, more and more car headlights are switching from original xenon headlights and halogen headlights to LED headlights. The temperature generated by LED headlights is relatively low, so the fog generated by the headlights is relatively difficult to dissipate, and it is necessary to place desiccant and matching CMD condensation devices in the headlights to absorb moisture.
[0003] However, compared with the traditional desiccants used in daily life, the desiccants used in car lights have six special performance requirements, mainly as follows: high hygroscopicity (under the conditions of temperature 40°C and humidity 90%, water absorption rate >30% in 3 days, total water absorption rate >150-180%), corrosion resistance (pH neutrality), no agglomeration, no liquefaction (anti-leakage), fast demisting time, reversible cycle and other requirements.
[0004] As it is an emerging industry demand, the performance of the car lamp desiccant patents and commercial car lamp desiccant products currently on the market cannot fully meet customer requirements and are still in the development stage. The vast majority of car lamp desiccants at home and abroad can achieve "no liquefaction" and "fast mist dissipation". However, the effects in terms of corrosion resistance (neutral pH value), anti-caking, and reversible circulation are not ideal and are still in the research stage.
[0005] For example, since car lights need to demist quickly, in order to prevent liquefaction caused by excessive moisture absorption, desiccants used in car lights generally contain a large amount of magnesium chloride and magnesium oxide, which makes them exhibit obvious strong alkalinity (pH value above 11) after moisture absorption, which poses a risk of corrosion to plastic parts around car lights (such as PC materials, etc.).
[0006] More importantly, the current common desiccant for car lights will aggregate into "hard lumps" after absorbing moisture, and the continuous moisture absorption capacity of the desiccant that forms "hard lumps" decreases exponentially. In addition, almost all car light desiccants must be used in conjunction with a breathable membrane (or a CMD device containing a breathable membrane), and the volume of the desiccant that forms a "hard lump" will expand by about 2 times. If the filling volume is insufficient, the moisture absorption effect will be insufficient. If the filling volume is sufficient, there is a risk of causing the breathable membrane to deform or even break.
[0007] Therefore, providing a desiccant that is particularly suitable for use in vehicle lamps, which can ensure that the fog of the vehicle lamps dissipates quickly and does not liquefy during normal use, while increasing the anti-chemical corrosion and anti-caking functions of the desiccant, has good application prospects. Summary of the invention
[0008] In order to solve the above technical problems, the present invention provides a desiccant and a preparation method and application thereof. The various functional components in the desiccant provided by the present invention are reasonably compounded, and the obtained desiccant is not only not easy to liquefy and has excellent long-term moisture absorption performance, but also has excellent anti-caking and anti-chemical corrosion technical effects, and has good application prospects.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a desiccant, wherein the desiccant comprises the following components in parts by weight:
[0011]
[0012] Wherein, the magnesium chloride can be 42 parts, 45 parts, 48 parts, 50 parts, 52 parts, 55 parts, 58 parts, 60 parts, 62 parts, etc.
[0013] The magnesium oxide can be 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, etc.
[0014] The pH adjuster can be 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, etc.
[0015] The dispersant can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, etc.
[0016] The moisture absorption control agent can be 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, etc.
[0017] In the present invention, magnesium chloride is the main hygroscopic material in the desiccant and has an excellent hygroscopic effect. Meanwhile, magnesium oxide can be used as an auxiliary absorbing material to prevent the desiccant from accumulating liquid. The addition of an inorganic pH regulator can effectively improve the phenomenon that magnesium chloride and magnesium oxide present strong alkalinity during the hygroscopic process, so that the desiccant remains neutral after absorbing water vapor, thereby reducing the risk of corrosion. The dispersant has a relatively small particle size and can be effectively distributed in the magnesium chloride to form an independent phase structure, thereby isolating the magnesium chloride and preventing it from agglomerating. The hygroscopic control agent can adjust the hygroscopic speed of the desiccant to a certain extent, thereby extending the service life of the product.
[0018] The various functional components in the desiccant provided by the present invention are reasonably compounded, and the obtained desiccant is not only not easy to liquefy and has excellent long-term moisture absorption performance, but also has excellent technical effects of anti-caking and anti-chemical corrosion.
[0019] Preferably, the pH adjuster includes any one of copper sulfate, ferric chloride, ammonium chloride, aluminum chloride or ferric sulfate, or a combination of at least two thereof.
[0020] Preferably, the dispersant includes any one of nano-silicon dioxide, bentonite, kaolin, alumina, diatomaceous earth, calcium sulfate, barium carbonate, magnesium carbonate, calcium phosphate or magnesium sulfate, or a combination of at least two thereof.
[0021] Preferably, the dispersant comprises a combination of nano-silicon dioxide, bentonite and magnesium carbonate.
[0022] In the present invention, since nano silicon dioxide, bentonite and magnesium carbonate have different crystal forms, three different phase structures are formed, thereby effectively destroying the percolation structure formed after the magnesium chloride absorbs moisture and agglomerates. At the same time, the covalent bonds of the three additives interfere with each other, making it more difficult to form a single phase structure, thereby improving the dispersion of the three additives in magnesium chloride. The three substances are compounded, and the three substances synergize to exert a dispersing effect from many aspects, and can have a more excellent anti-caking effect.
[0023] Preferably, the mass ratio of nano-silicon dioxide, bentonite and magnesium carbonate in the dispersant is 1:(0.5-1.5):(0.5-1.5).
[0024] The above-mentioned value (0.5-1.5) can be 0.6, 0.8, 1, 1.2, 1.4, etc.
[0025] In the present invention, when the proportion of the components in the dispersant is within the above-defined range, the anti-caking performance of the obtained desiccant is more prominent.
[0026] Preferably, the particle size of the nano-silicon dioxide in the dispersant is 1-30 μm, for example, the intermediate value in the Gaussian distribution of the particle size may be 2 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, etc.
[0027] Preferably, the moisture absorption control agent includes any one of polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinyl phthalate (PVAP) or polyvinyl butyral, or a combination of at least two thereof.
[0028] Preferably, the moisture absorption control agent comprises a combination of polyvinyl alcohol and ethylene-vinyl alcohol copolymer.
[0029] In the present invention, the two components of the moisture control agent are compounded, which can increase the moisture absorption performance and at the same time enhance the molding effect of the product, making it present a more uniform powder state.
[0030] Preferably, the mass ratio of polyvinyl alcohol to ethylene-vinyl alcohol copolymer in the moisture absorption control agent is 1:(0.5-1.5).
[0031] The above-mentioned value (0.5-1.5) can be 0.6, 0.8, 1, 1.2, 1.4, etc.
[0032] In the present invention, when the proportion of the components in the moisture absorption control agent is within the above-defined range, the moisture absorption effect of the obtained desiccant is better and the service life is extended.
[0033] Preferably, the desiccant further comprises porous carbon black.
[0034] In the present invention, porous carbon black as an auxiliary absorption material can cooperate with magnesium oxide to prevent the occurrence of liquid accumulation in the desiccant.
[0035] Preferably, the desiccant further comprises 0.1-5 parts of porous carbon black by weight, for example, 0.2 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts, etc.
[0036] Preferably, the pore size of the porous carbon black is 0.02-2 μm, for example, the intermediate value in the Gaussian distribution of the pore size may be 0.05 μm, 0.1 μm, 0.2 μm, 0.5 μm, 1 μm, 1.5 μm, 1.8 μm, etc.
[0037] In a second aspect, the present invention provides a method for preparing the desiccant according to the first aspect, the preparation method comprising the following steps: crushing, grinding and mixing magnesium chloride, magnesium oxide, a pH adjuster, a dispersant, a moisture absorption control agent and optionally porous carbon black to obtain the desiccant.
[0038] In a third aspect, the present invention provides a use of the desiccant according to the first aspect in a vehicle lamp.
[0039] In a fourth aspect, the present invention provides a vehicle lamp condensation control device, wherein the vehicle lamp condensation control device comprises the desiccant described in the first aspect.
[0040] The desiccant provided by the present invention is suitable for new energy vehicles, especially for meeting the need for drying the inside of LED headlights. The desiccant eliminates the phenomenon that the condensed mist on the lampshade cannot be dissipated in time due to insufficient heat generated when the LED headlights are turned on, thereby greatly improving the aesthetics of the headlights.
[0041] Compared with the prior art, the present invention has at least the following beneficial effects:
[0042] (1) The desiccant provided by the present invention contains a variety of functional components, wherein the pH regulator can achieve the purpose of reducing corrosiveness while ensuring the solid form and desiccant function; the dispersant prevents the desiccant from forming a whole hard block after absorbing moisture, thereby maintaining the moisture absorption efficiency for a long time, and at the same time avoids the risk of deformation of the breathable membrane caused by volume expansion of the desiccant after absorbing moisture; the moisture absorption control agent has the function of regulating the moisture absorption speed and extending the service life; the various components in the desiccant provided by the present invention cooperate with each other, and have excellent moisture absorption, non-liquefaction, anti-caking and anti-corrosion properties;
[0043] (2) The additive raw materials provided by the present invention are simple and easy to obtain, low in price, and the preparation method is simple, which is suitable for commercial production needs. DETAILED DESCRIPTION
[0044] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0045] The sources of materials used in the following examples are as follows:
[0046] The particle size of nano-silicon dioxide is 1-30 μm;
[0047] The bentonite particle size is 100-200 mesh;
[0048] The particle size of polyvinyl alcohol is 10-200 mesh;
[0049] The particle size of ethylene-vinyl alcohol copolymer is 10-200 mesh;
[0050] The pore size of porous carbon black is 0.02-2μm.
[0051] Example 1
[0052] This embodiment provides a desiccant, which includes the following components in parts by weight:
[0053]
[0054] The pH regulator is ammonium chloride;
[0055] The dispersant is a combination of nano silicon dioxide, bentonite and magnesium carbonate in a mass ratio of 1:1:1;
[0056] The moisture absorption control agent is a 1:1 combination of polyvinyl alcohol and ethylene-vinyl alcohol copolymer.
[0057] The preparation method of the desiccant comprises: crushing, grinding and uniformly mixing the above raw materials to obtain the desiccant.
[0058] Example 2
[0059] This embodiment provides a desiccant, which includes the following components in parts by weight:
[0060]
[0061] The pH regulator is a combination of ammonium chloride and aluminum chloride in a mass ratio of 1:1;
[0062] The dispersant is a combination of nano silicon dioxide, bentonite and magnesium carbonate in a mass ratio of 1:0.5:1.5;
[0063] The moisture absorption control agent is a combination of polyvinyl alcohol and ethylene-vinyl alcohol copolymer in a ratio of 1:0.5.
[0064] The preparation method of the desiccant comprises: crushing, grinding and uniformly mixing the above raw materials to obtain the desiccant.
[0065] Example 3
[0066] This embodiment provides a desiccant, which includes the following components in parts by weight:
[0067]
[0068] The pH regulator is ammonium chloride;
[0069] The dispersant is a combination of nano silicon dioxide, bentonite and magnesium carbonate in a mass ratio of 1:1.5:0.5;
[0070] The moisture absorption control agent is a combination of polyvinyl alcohol and ethylene-vinyl alcohol copolymer in a ratio of 1:1.5.
[0071] The preparation method of the desiccant comprises: crushing, grinding and uniformly mixing the above raw materials to obtain the desiccant.
[0072] Example 4
[0073] This embodiment provides a desiccant, which is different from the embodiment 1 only in that porous carbon black is not added, and its weight portion is distributed to magnesium oxide. The rest is as in the embodiment 1.
[0074] Example 5
[0075] This embodiment provides a desiccant, which is different from the embodiment 1 only in that nano silicon dioxide is not added to the dispersant, and its weight proportions are distributed according to the ratio of bentonite and magnesium carbonate. The rest is as in the embodiment 1.
[0076] Example 6
[0077] This embodiment provides a desiccant, which is different from the embodiment 1 only in that bentonite is not added to the dispersant, and its weight proportions are distributed according to the ratio of nano-silicon dioxide and magnesium carbonate. The rest is as in the embodiment 1.
[0078] Example 7
[0079] This embodiment provides a desiccant, which is different from the embodiment 1 only in that magnesium carbonate is not added to the dispersant, and its weight proportion is distributed according to the ratio of nano-silicon dioxide and bentonite. The rest is referred to the embodiment 1.
[0080] Example 8
[0081] This embodiment provides a desiccant, which is different from the embodiment 1 only in that polyvinyl alcohol is not added to the moisture absorption control agent, and its weight proportion is distributed to the ethylene-vinyl alcohol copolymer. The rest is as in the embodiment 1.
[0082] Example 9
[0083] This embodiment provides a desiccant, which is different from the embodiment 1 only in that ethylene-vinyl alcohol copolymer is not added to the moisture absorption control agent, and its weight proportion is allocated to polyvinyl alcohol. The rest is as in the embodiment 1.
[0084] Comparative Example 1
[0085] This comparative example provides a desiccant, which is different from Example 1 only in that no pH adjuster is added, and the rest is referred to Example 1.
[0086] Comparative Example 2
[0087] This comparative example provides a desiccant, which differs from Example 1 only in that no dispersant is added, and its weight portion is allocated to the moisture absorption control agent. The rest is as in Example 1.
[0088] Comparative Example 3
[0089] This comparative example provides a desiccant, which is different from Example 1 only in that no moisture absorption control agent is added, and its weight portion is distributed to the dispersant. The rest is referred to Example 1.
[0090] Test Case
[0091] Take 5g of the desiccant provided in Examples 1-9 and Comparative Examples 1-3 respectively and place them in an inner cavity with a diameter of 10m 3 In the headlight condensation device, the headlight condensation device or desiccant is tested as follows:
[0092] (1) Water absorption test: The test was conducted in accordance with the industry standard provided by BBT 0049-2008. The headlights were tested using a condensation device at 40°C and 90% RH to obtain the water absorption of the desiccant after 3, 8 and 16 days.
[0093] (2) Liquefaction test: The test was conducted in accordance with the industry standard provided by BBT 0049-2008. The headlights were tested using a condensation device at 40°C and 90% RH. After 16 days, the desiccant was taken out and centrifuged. The mass ratio of the centrifuged liquid and the desiccant after the test was calculated to obtain the mass percentage of the accumulated liquid.
[0094] (3) Anti-caking test: The test was conducted in accordance with the industry standard provided by BBT 0049-2008. The headlights were tested using a condensation device at 40°C and 90% RH. After 16 days, the desiccant was removed and the diameter of the largest hard lump was measured.
[0095] (4) Expansion test: The test is conducted in accordance with the industry standard provided by BBT 0049-2008. The condensation device for vehicle lamps is tested at 40°C and 90% RH. The height of the desiccant in the condensation device for vehicle lamps is measured at the initial stage and after 16 days. The ratio of the height of the desiccant after the test to the height of the desiccant in the initial stage is calculated.
[0096] (5) pH test: Test according to the industry standard provided by ISO16750-5. Mix the desiccant and water in a mass ratio of 1:1 and test the pH.
[0097] The test results of the desiccants provided in Examples 1-9 and Comparative Examples 1-3 are shown in Table 1.
[0098] Table 1
[0099]
[0100]
[0101]
[0102] The test results show that:
[0103] (1) It can be seen from Examples 1 to 9 that the various functional components in the desiccant provided by the present invention are reasonably compounded, and the obtained desiccant is not only not easy to liquefy and has excellent long-term moisture absorption performance, but also has excellent anti-caking and anti-chemical corrosion technical effects; within the preferred range, the desiccant has a water absorption rate of >30% in 3 days and >100% in 8 days under the conditions of a temperature of 40°C and a relative humidity of 90%, and continues to absorb moisture after 16 days, with a total moisture absorption of about 150-200%. After 16 days, the desiccant does not form a hard lump as a whole, and there is no liquid water penetration. After the desiccant is soaked in water, its aqueous solution is neutral (pH value between 6.5-8), and there is no corrosion risk.
[0104] (2) By comparing Example 1 with Examples 5-7, it can be seen that the present invention further compounded the nano-silicon dioxide, bentonite and magnesium carbonate in the dispersant, and the three components synergistically enhanced the effect, thereby achieving a better anti-caking technical effect.
[0105] By comparing Example 1 with Examples 8-9, it can be seen that the present invention further compounded the polyvinyl alcohol and ethylene-vinyl alcohol copolymer in the moisture absorption control agent, and the two components synergistically enhanced the effect, thereby achieving a better moisture absorption effect.
[0106] (3) By comparing Example 1 with Comparative Examples 1-3, it can be seen that when the desiccant lacks any one of the pH regulator, dispersant and moisture absorption control agent, the corresponding anti-corrosion, anti-caking and moisture absorption functions of the obtained desiccant are reduced.
[0107] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A desiccant, characterized in that: The desiccant comprises the following components by weight:
2. The desiccant according to claim 1, characterized in that The pH adjuster includes any one of copper sulfate, ferric chloride, ammonium chloride, aluminum chloride or ferric sulfate, or a combination of at least two thereof.
3. The desiccant according to claim 1 or 2, characterized in that: The dispersant includes any one of nano silicon dioxide, bentonite, kaolin, alumina, diatomaceous earth, calcium sulfate, barium carbonate, magnesium carbonate, calcium phosphate or magnesium sulfate, or a combination of at least two thereof.
4. The desiccant according to any one of claims 1 to 3, characterized in that: The dispersant includes a combination of nano silicon dioxide, bentonite and magnesium carbonate; Preferably, the mass ratio of nano-silicon dioxide, bentonite and magnesium carbonate in the dispersant is 1:(0.5-1.5):(0.5-1.5); Preferably, the particle size of the nano-silicon dioxide in the dispersant is 1-30 μm.
5. The desiccant according to any one of claims 1 to 4, characterized in that: The moisture absorption control agent includes any one of polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyvinyl phthalate or polyvinyl butyral, or a combination of at least two of them.
6. The desiccant according to any one of claims 1 to 5, characterized in that: The moisture absorption control agent includes a combination of polyvinyl alcohol and ethylene-vinyl alcohol copolymer; Preferably, the mass ratio of polyvinyl alcohol to ethylene-vinyl alcohol copolymer in the moisture absorption control agent is 1:(0.5-1.5).
7. The desiccant according to any one of claims 1 to 6, characterized in that: The desiccant also includes porous carbon black; Preferably, the desiccant further comprises 0.1-5 parts by weight of porous carbon black; Preferably, the pore size of the porous carbon black is 0.02-2 μm.
8. A method for preparing a desiccant according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: crushing, grinding and mixing magnesium chloride, magnesium oxide, a pH regulator, a dispersant, a moisture absorption control agent and optionally porous carbon black to obtain the desiccant.
9. Use of the desiccant according to any one of claims 1 to 7 in a vehicle lamp.
10. A vehicle lamp condensation control device, characterized in that: The vehicle lamp condensation control device comprises the desiccant according to any one of claims 1-7.