Zero-emission full-recovery method for waste electronic waste
Through wave cracking reactor technology, electromagnetic wave resonance breaks the C-C bond, the problems of environmental pollution and health hazards in traditional electronic waste treatment are solved, and carbon-free, zero-emission and fully recycled electronic waste treatment are achieved, and organic matter in electronic waste is achieved. and inorganic substances are effectively utilized.
Patent Information
- Application Number
- CN202411403841.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-10-10
- Filing Date
- 2024-10-09
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional electronic waste treatment methods have environmental pollution and health hazards, making it difficult to achieve carbon-free consumption, zero emissions and full recycling.
The wave cracking reactor technology is used to break the C-C bond through the electromagnetic wave resonance at fixed frequency, and the organic matter in electronic waste is decomposed into combustible gas and fuel oil, and the solid inorganic matter is separated, achieving large-scale industrial processing without classification and disassembly.
The zero-emission and full recycling of electronic waste has been achieved. The organic matter in the electronic waste has been turned into natural gas and fuel oil, and the inorganic matter has become metal minerals, achieving the effect of no carbon consumption and full recycling.
Smart Images

Figure CN119076588A_ABST
Abstract
Description
[0001] The present invention claims the priority of the Chinese patent application filed with the Chinese Patent Office on October 10, 2023, with application number 202311311025.9 and application name “Zero-emission full recycling method for discarded electronic waste”, the entire contents of which are incorporated by reference into the present invention. Technical Field
[0002] The present invention relates to the technical field of electronic waste treatment, and in particular to a method for completely recycling discarded electronic waste with zero emission. Background Art
[0003] Since March 2005, Greenpeace has collected 44 environmental samples. The published test results show that a large amount of toxic heavy metals and organic compounds are discharged during the dismantling of electronic waste, resulting in serious excessive heavy metal content in the air, water and soil. The barium content in the soil exceeds the standard by more than 10 times, tin by 152 times, lead by 212 times, and chromium by 1,338 times. Pollutants in the water exceed the drinking water standard by thousands of times. Medical examinations of the employed population show that 88% of the people surveyed suffer from skin diseases, nervous system, respiratory system or digestive system diseases, and their health is greatly damaged. According to a report released by the United Nations Environment Program in 2010, my country has become the world's second largest producer of electronic waste, producing more than 2.3 million tons of electronic waste each year, second only to the United States' 3 million tons. After 2010, my country has entered the peak period of electrical appliance elimination. In 2020, my country's waste computers will double or triple compared with 2007, and discarded mobile phones will increase by 7 times. As early as 2003, at least 6 million washing machines, 5 million televisions, and 4 million refrigerators were scrapped in my country every year. In addition, old cars and electric vehicles are also an important source of electronic waste. In the process of recycling and comprehensive utilization of electronic waste, there are different degrees of environmental pollution and damage to human health, which urgently needs to be paid attention to.
[0004] As a complex of resources, electronic waste contains many precious resources. The reuse and recycling of electronic waste is an important way to solve the problems of resource shortage and environmental pollution. By improving resource utilization, turning waste into treasure, and giving full play to the role of various waste resources including electronic waste, it has become one of the ways to support the rapid development of my country's economy and society. Research and analysis results show that 143kg of copper, 0.5kg of gold, 40.8kg of iron, 29.5kg of lead, 2.0kg of tin, 18.1kg of nickel, and 10.0kg of antimony can be separated from 1 ton of randomly collected electronic boards. In printed circuit boards, the most common metal is copper, in addition to gold, aluminum, nickel, lead and other metals, including rare metals. Statistics show that the gold content in each ton of waste circuit boards is about 1,000g. With the improvement of process level, 300g of gold can be extracted from each ton of waste circuit boards. Yokohama Metals of Japan analyzed the composition of discarded mobile phones and found that on average, every 100 grams of mobile phone body contained 14 grams of copper, 0.19 grams of silver, 0.03 grams of gold and 0.01 grams of palladium. In addition, metallic lithium can be recovered from mobile phone lithium batteries. The company has obtained considerable economic benefits by recycling a variety of precious metals from discarded mobile phones.
[0005] However, several traditional methods for treating electronic waste: chemical treatment, pyrolysis, mechanical treatment, and microbial treatment all have serious defects. Chemical treatment, also known as wet treatment, involves putting the crushed electronic waste particles into an acidic or alkaline liquid, and the leaching liquid undergoes a series of processes such as extraction, precipitation, replacement, ion exchange, filtration, and distillation to finally obtain high-grade metals. However, in the process of chemical treatment, strong acids and highly toxic fluorides are used, which will produce a large amount of waste liquid and emit toxic gases, and the amount of solid residue discharged is large, which has serious harm to the environment. Pyrolysis is a method of incinerating, smelting, sintering, melting, etc. electronic waste to remove plastics and other organic components to enrich metals. Pyrolysis is the complete incineration of organic matter, with large gas emissions and the risk of producing dioxins, which causes serious harm to the environment and will have a serious impact on the local environment and sustainable development. Mechanical treatment is a method of sorting by using the differences in physical properties between the components, including disassembly, crushing, sorting, etc. The materials after sorting can be processed through subsequent treatment to obtain recycled raw materials such as metals, plastics, and glass. This treatment method has the advantages of low cost, simple operation, not easy to cause secondary pollution, and easy to achieve scale. The disassembly of electronic waste is usually done manually to recover useful electronic components that have been tested. However, due to the large number of electronic components in electronic waste and the complex combination method, the efficiency of manual treatment is very low. More importantly, it is difficult to achieve complete separation of organic and inorganic substances by mechanical treatment, and the organic matter after disassembly still faces disposal problems. The microbial method uses the activity of microorganisms to oxidize other non-precious metals in precious metal alloys such as gold into soluble substances and enter the solution, exposing the precious metals for easy recovery. The microbial method has the advantages of simple process, low cost and simple operation to extract precious metals such as gold from electronic waste, but the leaching time is long and large-scale industrial production is difficult to achieve. The key is that the premise of using the microbial method must be mechanically separated first, the raw material requirements are harsh, and the economic and social benefits are obviously lower. Summary of the invention
[0006] The purpose of the present invention is to provide a method for the zero-emission and full recycling of discarded electronic waste, so as to realize large-scale industrialized treatment and disposal, carbon-free consumption, zero emission and full recycling. Both organic and inorganic substances in the electronic waste can be effectively utilized, the organic substances are converted into natural gas and fuel oil, and the inorganic substances are converted into metal minerals.
[0007] To achieve the above-mentioned purpose, the present invention provides a method for zero-emission and full recycling of discarded electronic waste, comprising the following steps:
[0008] Step S1, crushing the electronic waste to obtain electronic waste raw materials;
[0009] Step S2, after the electronic waste raw materials are fed into the wave cracking reactor, the wave cracking reactor is started, the reactor parameters of the wave cracking reactor and the electromagnetic parameters of the M wave source generators in the reactor are controlled, and the resonance fracture of the CC bond occurs under the irradiation of the electromagnetic wave of a fixed frequency, and the organic macromolecules are decomposed into small organic molecules to form oil and gas vapor and separate from the solid inorganic matter;
[0010] Step S3, collecting organic vapor at the top of the wave cracking reactor, and obtaining combustible gas and fuel oil through condensation treatment, and collecting solids at the bottom of the wave cracking reactor;
[0011] The M wave source generators have the same frequency and wavelength, the frequency range is 200-250kHz, the wavelength range is 1450-1850m, the phase angle difference between any two wave source generators is Δθ=nΔθ0, and the value range of Δθ0 is 54.3°-55.4°;
[0012] After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.
[0013] According to a technical solution of the present invention, it also includes:
[0014] Step S4: using a plasma emission spectrometer to determine the metal content at the bottom of the wave cracking reactor.
[0015] According to a technical solution of the present invention, in step S2, the M wave source generators are cyclically turned on, and the electromagnetic wave emitted by any of the wave source generators is expressed as:
[0016] E(t i )=A i ·sin(2πft+θ i )
[0017] Among them, t i represents the ith irradiation time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, f represents frequency, and the phase angle difference between any two wave source generators in adjacent irradiation time periods is represented by θ i+1 -θ i , then:
[0018] Δθ0=θ i+1 -θ i .
[0019] According to a technical solution of the present invention, any electromagnetic parameter of the wave source generator at least includes a single opening time length t of the wave source generator. 单, a phase angle difference between two wave source generators with adjacent irradiation time periods;
[0020] The single opening time t of any of the wave source generators 单 It is 30s to 200s.
[0021] According to a technical solution of the present invention, the reactor parameters at least include the pressure inside the reactor, the temperature inside the reactor and the wave cracking time;
[0022] The pressure in the kettle is 6000Pa-8000Pa, the temperature in the kettle is 370°C-425°C, and the wave cracking time is 30min-200min.
[0023] According to a technical solution of the present invention, a wave absorbing material is arranged in the wave cracking reactor, and the wave absorbing material is one or more of nickel oxide NiO, ferroferric oxide Fe3O4, cobalt oxide CoO, cadmium nitrate Cr(NO3)3, iron sulfide FeS2, cuprous sulfide Cu2S, carbon C, iron oxide Fe2O3, zinc oxide ZnO, manganese trioxide Mn2O3, carbonyl nickel Ni(CO)4, carbonyl iron Fe(CO)5, γ-Al2O3, cuprous oxide Cu2O, lead oxide PbO, calcium oxide CaO and molybdenum oxide MoO3.
[0024] According to a technical solution of the present invention, the amount of the wave absorbing material accounts for 0.1% to 10% of the total amount of the wave cracking raw materials in terms of mass percentage;
[0025] The wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor along with the raw materials after pretreatment.
[0026] According to a technical solution of the present invention, in step S3, the product at the top of the wave cracking reactor is recovered by a multi-stage recovery device, including four oil products, namely, combustion oil, diesel component, gasoline component and naphtha, and two combustible gas products, namely, liquefied gas and natural gas;
[0027] The product at the bottom of the wave cracking reactor includes one or more of gold, silver, copper, zinc and tin metals.
[0028] According to a technical solution of the present invention, the multi-stage recovery device is a first-stage condenser for recovering the combustion oil, a second-stage condenser for recovering the diesel component, a third-stage condenser for recovering the gasoline component, and a fourth-stage condenser for recovering the naphtha;
[0029] The non-condensable gas after passing through the fourth condenser enters the desulfurization device, the dechlorination device, the denitrification device, the dust removal device and the purification device in sequence. The non-condensable gas after purification is compressed by the compressor to obtain liquefied gas, and the incompressible oil and gas is natural gas.
[0030] According to a technical solution of the present invention, the value range of M is 3 to 20.
[0031] The beneficial effects of the present invention are:
[0032] According to one solution of the present invention, fixed frequency physical waves are used as the power source, and organic macromolecules are decomposed into organic small molecules by resonantly breaking CC chemical bonds, so that zero-emission and full recycling and disposal of electronic waste can be achieved. Moreover, electronic waste does not need to be classified and disassembled, but only needs to be simply crushed to make the raw materials reach a size that can enter the wave cracking reactor. When the electronic waste enters the wave cracking reactor, after the resonance of the wave cracking, all organic matter in the electronic waste will form gaseous substances and be separated from solid inorganic matter.
[0033] According to one solution of the present invention, all organic matter in electronic waste is decomposed into gaseous substances of C1-C4 and C5-C 20 The liquid substance and solid inorganic matter are discharged from the bottom of the wave cracking reactor, realizing large-scale industrial treatment and disposal, carbon-free consumption, zero emission and full recycling. Both the organic and inorganic matter in the electronic waste can be effectively utilized, the organic matter is turned into natural gas and fuel oil, and the inorganic matter is turned into metal minerals.
[0034] By reasonably controlling the electromagnetic parameters of the wave source generator and the reactor parameters in the wave cracking reactor, the wave cracking efficiency and cracking degree can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 A flowchart schematically showing a method for zero-emission and full recycling of discarded electronic waste according to an embodiment of the present invention;
[0036] Figure 2 A schematic diagram showing the change of the degree of cleavage over time in Example 1;
[0037] Figure 3 A schematic diagram showing the change of the gas product ratio over time in Example 1;
[0038] Figure 4 A schematic diagram showing the change of the degree of cleavage over time in Example 2;
[0039] Figure 5 A schematic diagram showing the change of the degree of cleavage over time in Example 3;
[0040] Figure 6 A schematic diagram showing the change of the degree of cleavage over time in Example 4;
[0041] Figure 7 A graph schematically showing the relationship between the degree of fragmentation and the relative value of the phase angle. DETAILED DESCRIPTION
[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0043] When describing the embodiments of the present invention, the orientation or positional relationship expressed by the terms "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or positional relationship shown in the relevant drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.
[0044] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The embodiments cannot be described one by one here, but the embodiments of the present invention are not therefore limited to the following embodiments.
[0045] like Figure 1 As shown, according to one embodiment of the present invention, a method for zero-emission and full recycling of discarded electronic waste of the present invention comprises the following steps:
[0046] Step S1, crushing the electronic waste to obtain electronic waste raw materials;
[0047] It can be understood that the main purpose of step S1 is to crush the raw materials. The shape of the crushed waste electronic waste can be any shape, such as powder, rubber, block and other crushed materials, as long as the maximum size of the appearance does not exceed 5 cm. If there are recycled materials with a size less than 5 cm, no further processing is required, and they can be directly regarded as raw materials entering the cracking reactor.
[0048] In step S1, whether there is a power source in the electronic waste has no effect on wave cracking, and no special treatment is required; it has been determined that engine parts must be removed from the electronic waste in advance; it has been determined that electronic waste consisting only of inorganic substances or metals, such as ceramic capacitors, thyristors, metal electrical appliance casings, etc., must be removed from the raw materials in advance.
[0049] Step S2, after the electronic waste raw materials are fed into the wave cracking reactor, the wave cracking reactor is started, the reactor parameters of the wave cracking reactor and the electromagnetic parameters of the M wave source generators in the reactor are controlled, and the resonance fracture of the CC bond occurs under the irradiation of the electromagnetic wave of a fixed frequency, and the organic macromolecules are decomposed into small organic molecules to form oil and gas vapor and separate from the solid inorganic matter;
[0050] The wave absorbing material is arranged in the wave cracking reactor, and the wave absorbing material is one or more of nickel oxide NiO, ferroferric oxide Fe3O4, cobalt oxide CoO, cadmium nitrate Cr(NO3)3, iron sulfide FeS2, cuprous sulfide Cu2S, carbon C, iron oxide Fe2O3, zinc oxide ZnO, manganese trioxide Mn2O3, carbonyl nickel Ni(CO)4, carbonyl iron Fe(CO)5, γ-Al2O3, cuprous oxide Cu2O, lead oxide PbO, calcium oxide CaO and molybdenum oxide MoO3. The amount of the wave absorbing material accounts for 0.1% to 10% of the total amount of the wave cracking raw materials in terms of mass percentage; the wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor with the pretreated raw materials.
[0051] The reaction kettle parameters at least include the pressure inside the kettle, the temperature inside the kettle and the wave cracking time; the pressure inside the kettle is 6000Pa-8000Pa, the temperature inside the kettle is 370℃-425℃, and the wave cracking time is 30min-200min.
[0052] The M wave source generators have the same frequency and wavelength, the frequency range is 200-250kHz, the wavelength range is 1450-1850m, the phase angle difference between any two wave source generators is Δθ=nΔθ0, and the value range of Δθ0 is 54.3°-55.4°;
[0053] After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.
[0054] In step S2, the M wave source generators are cyclically turned on, and the electromagnetic wave emitted by any of the wave source generators is expressed as:
[0055] E(t i )=A i ·sin(2πft+θ i )
[0056] Among them, t i represents the ith irradiation time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, f represents frequency, and the phase angle difference between any two wave source generators in adjacent irradiation time periods is represented by θi+1 -θ i , then:
[0057] Δθ0=θ i+1 -θ i .
[0058] Any electromagnetic parameter of the wave source generator at least includes a single opening time t of the wave source generator. 单 , a phase angle difference between two wave source generators with adjacent irradiation time periods;
[0059] The single opening time t of any of the wave source generators 单 It is 30s to 200s.
[0060] It is understandable that when the single opening time t 单 When the time is set to 100s and the phase angle difference Δθ0 is set to 55°, that is, Δθ0=55°, in the first time period (the first 100s), the electromagnetic wave emitted by the first wave source generator is expressed as: E(t1)=A1·sin(2πft+θ1). From the 101st second, the first wave source generator is turned off and the second wave source generator is turned on. The electromagnetic wave emitted by the second wave source generator is expressed as: E(t2)=A2·sin(2πft+θ2). Under normal circumstances, A1=A2, and Δθ=θ2-θ1=55°; and from the 201st second, the second wave source generator is turned off and the third wave source generator is turned on, then Δθ=θ3-θ2=55°. At this time, 2Δθ0=θ3-θ1=110°, and so on. When the Mth wave source generator is turned off and the set wave splitting time has not been reached, the first wave source generator is turned on again for the next cycle.
[0061] Typically, the value range of M is 3 to 20, preferably, the value range is 4 to 10.
[0062] In addition, the first wave source generator, the second wave source generator, the third wave source generator...the Mth wave source generator can be regarded as the first type of wave source generator, the second type of wave source generator, the third type of wave source generator...the Mth type of wave source generator. Multiple wave source generators of each type can be set and turned on or off at the same time to improve the wave splitting efficiency.
[0063] Step S3, collecting organic vapor at the top of the wave cracking reactor, and obtaining combustible gas and fuel oil through condensation treatment, and collecting solids at the bottom of the wave cracking reactor;
[0064] In the step S3, the product at the top of the wave cracking reactor is recovered by a multi-stage recovery device, including four oil products, namely, combustion oil, diesel component, gasoline component and naphtha, and two combustible gas products, namely, liquefied gas and natural gas;
[0065] The product at the bottom of the wave cracking reactor includes one or more of gold, silver, copper, zinc and tin metals.
[0066] The multi-stage recovery device is a first-stage condenser for recovering the combustion oil, a second-stage condenser for recovering the diesel component, a third-stage condenser for recovering the gasoline component, and a fourth-stage condenser for recovering the naphtha;
[0067] The non-condensable gas after passing through the fourth condenser enters the desulfurization device, the dechlorination device, the denitrification device, the dust removal device and the purification device in sequence. The non-condensable gas after purification is compressed by the compressor to obtain liquefied gas, and the incompressible oil and gas is natural gas.
[0068] Step S4: using a plasma emission spectrometer to determine the metal content at the bottom of the wave cracking reactor.
[0069] In this embodiment, the waste electronic waste is crushed so that the raw materials can be irradiated more evenly and sufficiently by the wave during wave cracking, thereby improving the efficiency of wave cracking. The fixed frequency physical wave is used as the power source, and the organic matter in the electronic waste is completely decomposed into C1-C4 gaseous substances and C5-C 20 The liquid substances are recovered in gaseous form through the top of the reactor in the wave cracking reactor, and the uncracked metals are recovered at the bottom of the wave cracking reactor, thereby achieving carbon-free consumption, zero emissions and full recycling. The organic and inorganic substances in the mixed electronic waste can be effectively utilized, the organic substances are converted into natural gas and fuel oil, and the inorganic substances are converted into metal minerals.
[0070] Four groups of specific implementation methods are given below based on the above-mentioned waste electronic waste zero-emission full recycling method to specifically illustrate the waste electronic waste zero-emission full recycling method of the present invention. In the following four embodiments, Motorola V3 mobile phones without batteries are used as the main raw materials, and their main components are polycarbonate (PC) and acrylonitrile-butadiene-styrene copolymer (ABS).
[0071] It should also be noted that the degree of cracking in the present invention is expressed as: degree of cracking = (mass of gas product + mass of liquid product + mass of inorganic matter) / mass of raw material × 100%, the mass of inorganic matter includes the mass of solid carbon and the mass of metal; and for the recovery rate involved in the present invention, the recovery rate = (mass of gas product + mass of liquid product + mass of inorganic matter) / (mass of raw material - mass of uncrashed solid) × 100%. The mass of recovered solid includes the mass of inorganic matter and uncrashed solid.
[0072] Example 1
[0073] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the M wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 150s, Δθ0=55°, and the number of wave source generators M=5.
[0074] The wavelength is set to 1500m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 200kHz, the wave cracking temperature is 400℃, the wave cracking pressure is 7000Pa, the energy density is 150Wh / L, the wave cracking time is 45min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.
[0075] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 43 kg of four fuel oils (including 13 kg of combustion oil component, 19 kg of diesel component, 10 kg of gasoline component, and 1 kg of naphtha component), 10 kg of liquefied gas, about 10 kg of natural gas, 37 kg of inorganic matter (almost no un-cracked solids), the product recovery rate was close to 100%, and the cracking degree was close to 100%. When the wave cracking time was 43 min, almost no gas product was produced.
[0076] The solid at the bottom of the wave cracking reactor was detected by plasma emission spectrometer ICP, and the metal content in the solid at the bottom of the wave cracking reactor was about 9.8 kg.
[0077] Example 2
[0078] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the M wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 180s, Δθ0=58°, and the number of wave source generators M=7.
[0079] The wavelength is set to 1600m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 210kHz, the wave cracking temperature is 380℃, the wave cracking pressure is 8000Pa, the energy density is 160Wh / L, the wave cracking time is 100min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.
[0080] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 25.69 kg of four fuel oils (8.37 kg of combustion oil component, 10.75 kg of diesel component, 5.97 kg of gasoline component, 0.6 kg of naphtha component), 6.5 kg of liquefied gas, about 7.5 kg of natural gas, 23.3 kg of inorganic matter, 37.01 kg of un-cracked solids, the product recovery rate was close to 100%, and the cracking degree was 62.99%. When the wave cracking time was 90 min, almost no gas product was produced.
[0081] The solid at the bottom of the wave cracking reactor was detected by plasma emission spectrometer ICP, and the metal content in the solid at the bottom of the wave cracking reactor was about 6.16 kg.
[0082] Example 3
[0083] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the M wave source generators in the wave cracking reactor are adjusted, and the single opening time t 单 Set to 170s, Δθ0=62°, and the number of wave source generators M=4.
[0084] The wavelength is set to 1750m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 215kHz, the wave cracking temperature is 410℃, the wave cracking pressure is 6000Pa, the energy density is 180Wh / L, the wave cracking time is 180min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.
[0085] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 13 kg of four fuel oils (including 3.9 kg of combustion oil component, 5.3 kg of diesel component, 3.4 kg of gasoline component, and 0.4 kg of naphtha component), 3 kg of liquefied gas, about 2.9 kg of natural gas, 18.4 kg of inorganic matter, 62.7 kg of un-cracked solids, the product recovery rate was close to 100%, and the cracking degree was 37.3%. When the wave cracking time was 150 min, almost no gas product was produced.
[0086] The solid at the bottom of the wave cracking reactor was detected by plasma emission spectrometer ICP, and the metal content in the solid at the bottom of the wave cracking reactor was about 4.88 kg.
[0087] Example 4
[0088] In this embodiment, after the pretreatment in step S1, 100 kg of crushed raw materials are obtained. Before the wave cracking treatment, the electromagnetic parameters of the M wave source generators in the wave cracking reactor are adjusted, and the single opening time t单 Set to 190s, Δθ0=52°, and the number of wave source generators M=8.
[0089] The wavelength is set to 1800m, the raw material size is set to 5cm, the type of wave used for wave cracking is electromagnetic wave, the wave frequency is 230kHz, the wave cracking temperature is 420℃, the wave cracking pressure is 7500Pa, the energy density is 155Wh / L, the wave cracking time is 80min, and at the same time, 5% of the total amount of crushed raw materials is added to the raw materials.
[0090] Using the above reactor parameters and electromagnetic parameters, the wave cracking reactor was started, and the product data were as follows: 31.94 kg of four fuel oils (including 8.57 kg of combustion oil component, 8.73 kg of diesel component, 7.1 kg of gasoline component, and 0.74 kg of naphtha component), 8.57 kg of liquefied gas, about 8.73 kg of natural gas, 27.3 kg of inorganic matter, 23.46 kg of un-cracked solids, the product recovery rate was close to 100%, and the cracking degree was 76.54%. When the wave cracking time was 70 min, almost no gas product was produced.
[0091] The solid at the bottom of the wave cracking reactor was detected by plasma emission spectrometer ICP, and the metal content in the solid at the bottom of the wave cracking reactor was about 7.23 kg.
[0092] The above contents are merely examples of specific solutions of the present invention. For devices and structures not described in detail therein, it should be understood that they can be implemented by adopting general devices and general methods available in the art.
[0093] The above is only one solution of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for zero-emission recycling of discarded electronic waste. It is characterized in that The following steps are involved: Step S1, crushing the electronic waste to obtain electronic waste raw materials; Step S2, after the electronic waste raw materials are fed into the wave cracking reactor, the wave cracking reactor is started, the reactor parameters of the wave cracking reactor and the electromagnetic parameters of the M wave source generators in the reactor are controlled, and the resonance fracture of the CC bond occurs under the irradiation of the electromagnetic wave of a fixed frequency, and the organic macromolecules are decomposed into small organic molecules to form oil and gas vapor and separate from the solid inorganic matter; Step S3, collecting organic vapor at the top of the wave cracking reactor, and obtaining combustible gas and fuel oil through condensation treatment, and collecting solids at the bottom of the wave cracking reactor; The M wave source generators have the same frequency and wavelength, the frequency range is 200-250kHz, the wavelength range is 1450-1850m, and the phase angle difference between any two wave source generators is Δθ=nΔθ. 0 , Δθ 0 The value range of is 54.3°~55.4°; After the wave cracking reactor is started, the energy density in the wave cracking reactor is 130-220Wh / L.
2. The recycling method according to claim 1, It is characterized in that Also includes: Step S4: using a plasma emission spectrometer to determine the metal content at the bottom of the wave cracking reactor.
3. The recycling method according to claim 1, It is characterized in that In step S2, the M wave source generators are cyclically turned on, and the electromagnetic wave emitted by any of the wave source generators is expressed as: E(t i )=A i ·sin(2πft+θ i ) Among them, t i represents the ith irradiation time period, θ i Represents the phase angle of the corresponding electromagnetic wave, A i represents the amplitude of the corresponding electromagnetic wave, t represents time, f represents frequency, and the phase angle difference between any two adjacent wave source generators in the irradiation time period is represented by θ i+1 -θ i , then: Dth 0 =θ i+1 -θ i 。 4. The recovery method according to claim 3, It is characterized in that Any electromagnetic parameter of the wave source generator at least includes a single opening time t of the wave source generator. 单 , a phase angle difference between two wave source generators with adjacent irradiation time periods; The single opening time t of any of the wave source generators 单 It is 30s to 200s.
5. The recycling method according to claim 1, It is characterized in that The reactor parameters include at least the pressure inside the reactor, the temperature inside the reactor and the wave cracking time; The pressure in the kettle is 6000Pa-8000Pa, the temperature in the kettle is 370°C-425°C, and the wave cracking time is 30min-200min.
6. The recycling method according to claim 1, It is characterized in that The wave absorbing material is arranged in the wave cracking reactor, and the wave absorbing material is nickel oxide NiO, ferroferric oxide Fe 3 O 4 , cobalt oxide CoO, cadmium nitrate Cr(NO 3 ) 3 , iron sulfide FeS 2 , Cuprous sulfide Cu 2 S, carbon C, iron oxide Fe 2 O 3 , zinc oxide ZnO, manganese trioxide Mn 2 O 3 ,Nickel Carbonyl Ni(CO) 4 , Carbonyl iron Fe(CO) 5 ,γ-Al 2 O 3 , cuprous oxide Cu 2 O, lead oxide PbO, calcium oxide CaO and molybdenum oxide MoO 3 One or more of .
7. The recovery method according to claim 6, It is characterized in that The amount of the wave absorbing material is 0.1% to 10% of the total amount of the wave cracking raw material in terms of mass percentage; The wave absorbing material is added to the wave cracking reactor before adding the raw materials, and / or is added to the wave cracking reactor along with the raw materials after pretreatment.
8. The recycling method according to claim 1, It is characterized in that In the step S3, the product at the top of the wave cracking reactor is recovered by a multi-stage recovery device, including four oil products, namely, combustion oil, diesel component, gasoline component and naphtha, and two combustible gas products, namely, liquefied gas and natural gas; The product at the bottom of the wave cracking reactor includes one or more of gold, silver, copper, zinc and tin metals.
9. The recovery method according to claim 8, It is characterized in that The multi-stage recovery device is a first-stage condenser for recovering the combustion oil, a second-stage condenser for recovering the diesel component, a third-stage condenser for recovering the gasoline component, and a fourth-stage condenser for recovering the naphtha; The non-condensable gas after passing through the fourth condenser enters the desulfurization device, the dechlorination device, the denitrification device, the dust removal device and the purification device in sequence. The non-condensable gas after purification is compressed by the compressor to obtain liquefied gas, and the incompressible oil and gas is natural gas.
10. The recycling method according to claim 1, It is characterized in that The value range of M is 3 to 20.
Citation Information
Patent Citations
Waste circuit board microwave anaerobic splitting treatment method
CN106345794A
Method for wave polarization catalytic cracking of biomass
CN110157456A
Household garbage oversize product total recovery treatment method
CN113102449A
Microwave delivery system with multiple magnetrons for a cooking appliance
US6680467B1