Method for improving cold rolling edge quality of high-grade non-oriented silicon steel rough edge coil
By adopting the large-side wave rolling mode in cold rolling of high-grade non-oriented silicon steel, the rolling speed and emulsion flow rate are adjusted, and the roughness of the working roller is controlled, the problems of side cracking and side wave are solved, and the yield rate is improved Production efficiency achieves efficient quality of cold rolled finished products.
Patent Information
- Application Number
- CN202411304380.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-19
AI Technical Summary
The prior art is difficult to simultaneously control the cracks and waves of the cold rolled edges of the burrs of the unoriented silicon steel with high grades, resulting in low material yield and high production costs.
Adopt the large side wave rolling mode to adjust the rolling speed, emulsion flow rate and the original roughness of the working roller, and control the plate straightness, rolling speed, emulsion flow rate and Working roller roughness to reduce the occurrence of side cracks and waves.
It effectively reduces the occurrence of cold rolling edge cracks and waves, improves the yield and production efficiency, and ensures the quality of the finished product and the production cost.
Smart Images

Figure CN119076612A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of non-oriented silicon steel production, and in particular relates to a method for improving the quality of cold-rolled edges of high-grade non-oriented silicon steel burr coils. Background Art
[0002] Cold rolling process is one of the main production processes of high-grade non-oriented silicon steel. Whether the cold rolling production is smooth or not has an extremely important impact on the quality and production cost of high-grade non-oriented silicon steel. Due to the high silicon content, high-grade non-oriented silicon steel is more brittle and is prone to edge cracking during cold rolling production, which reduces the yield rate and causes waste of resources. In severe cases, it can also cause belt breakage accidents, resulting in inestimable economic losses.
[0003] The edge crack phenomenon is more likely to occur in the rolling of rough edge coils. The rolling of rough edge coils refers to a process technology in which the hot-rolled raw materials are directly cold-rolled without trimming. Due to the inherent disadvantages of the edge quality of the rough edge coils, the edges are very likely to crack during the rolling process, which brings a higher risk of strip breakage to the rolling process. However, since the rough edge coils save the trimming operation in the normal pickling unit, the rough edge coils have great advantages in cutting loss for the same hot-rolled incoming materials. From the actual production data, it can be clearly seen that compared with trimmed coils, the rough edge coils have reduced cutting losses and improved the yield rate. At the same time, due to the reduction of trimming operations, the loss of the shear blade of the disc shear of the previous process unit is greatly reduced, which greatly reduces the production cost. Therefore, the research on the rolling of rough edge coils is very practical.
[0004] Regarding improving the quality of cold-rolled edges of high-grade non-oriented silicon steel rough edge coils, the relevant research results are as follows:
[0005] Patent CN105396879A discloses a method for controlling edge cracks in cold rolling of high-grade non-oriented silicon steel. In order to effectively reduce the edge stress of the strip and avoid edge cracks in high-grade non-oriented silicon steel during cold rolling, the load distribution of the first stand is reduced from 33-36% when the system automatically distributes to 25-30%; the UCMW rolling mill working roll shifting value is set to -40-20mm. Although this patent improves the edge cracking problem of the exit steel plate by reducing the load distribution of the first stand, it will inevitably increase the rolling load distribution of the rear stand, and with the increase of deformation resistance, the rolling load of the rear stand will increase sharply, which is extremely unfavorable for edge cracks and plate shape control.
[0006] Patent CN111687210A discloses a method for producing 0.35mm non-oriented silicon steel by using a cold rolling mill. The cold-rolled raw material coil is subjected to continuous five-stand cold rolling by a one-time rolling method. By controlling the reduction rate, rolling force, inter-stand and inlet and outlet tensions of each pass, and using emulsion spraying for process lubrication and cooling, and partitioning cooling of the working rolls, the thermal convexity of the working rolls is controlled to adjust the steel strip shape, and an intermediate product of non-oriented silicon steel with a thickness of 0.35mm can be obtained. Its main purpose is to obtain a 0.35mm product with a good plate shape, and there is no improvement on the edge crack problem.
[0007] The above patent documents all optimize the edge quality of silicon steel cold rolling, but all have certain problems or limitations. At present, there is no perfect means to simultaneously control edge cracks and edge waves to obtain good edge quality for cold rolling of rough edge coils of high-grade non-oriented silicon steel. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a method for improving the quality of the cold-rolled edge of a high-grade non-oriented silicon steel rough edge coil in view of the shortcomings of the prior art. By adopting a large edge wave rolling mode and adjusting the rolling speed, emulsion flow rate, original roughness of the working roll, etc., the purpose of controlling the rolling edge cracks and reducing the edge waves is achieved, thereby obtaining the best quality of the cold-rolled edge of the rough edge coil and improving production efficiency and product yield.
[0009] In order to solve the technical problem proposed by the present invention, the present invention provides a method for improving the quality of the cold-rolled edge of a high-grade non-oriented silicon steel burr coil, comprising: cold rolling using a multi-stand continuous rolling mill or a single-stand reversible rolling mill for 5 to 7 passes, and controlling the flatness of the plate shape after the first, second and last passes to meet the following formula:
[0010] 0.8×H 40 ≤F1≤0.8×H 40 +20
[0011] 0.6×H 40 ≤F2≤0.6×H 40 +20
[0012] 0.3×H 40 ≤F m ≤0.3×H 40 +20
[0013] In the formula, F1, F2, F m They are the straightness after the first, second and last rolling passes, in I; H 40 It is the thickness difference between the hot-rolled rough edge coil material 40mm away from the edge and the outermost edge. The average value of the whole coil is taken in μm.
[0014] Furthermore, the H40 ≤120μm.
[0015] In the above scheme, the rolling speed of the first pass of the cold rolling process satisfies the following formula:
[0016] 1200-2.4×10 4 ×(Si+Al)≤V≤1200-1.8×10 4 ×(Si+Al)
[0017] Wherein, V is the rolling speed, unit is m / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in the steel.
[0018] In the above scheme, the emulsion flow rate of the first and second passes of the cold rolling process satisfies the following formula:
[0019] 10000-1.4×10 5 ×(Si+Al)≤L≤10000-10 5 ×(Si+Al)
[0020] Wherein, L is the emulsion flow rate of the first and second passes, unit is L / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in steel.
[0021] In the above scheme, the original roughness of the working roll of the cold rolling control mill satisfies the following formula:
[0022] 50×(Si+Al)≤R≤100×(Si+Al)
[0023] Where R is the original roughness of the working roll, in μm; (Si+Al) is the sum of the mass percentages of Si and Al in the steel.
[0024] In the above scheme, the sum of the mass percentage contents of Si and Al in the high-grade non-oriented silicon steel is 2-4.5%, that is, (Si+Al) in the above formula is 2-4.5%.
[0025] Furthermore, the chemical composition of the high-grade non-oriented silicon steel includes, by mass percentage, C≤0.004%, S≤0.003%, N≤0.003%, Ti≤0.003%, P≤0.05%, Nb≤0.003%, Si≤4.0%, Al≤2.0%, (Si+Al)2~4.5%, Mn≤2.0%, and the balance is Fe and unavoidable impurities.
[0026] In the above scheme, the thickness of the high-grade non-oriented silicon steel burr roll is 1.6-2.4 mm.
[0027] In the above scheme, the thickness of the finished product of the high-grade non-oriented silicon steel burr coil after cold rolling is 0.20-0.50 mm.
[0028] In the above scheme, the edge crack depth of the finished product of the high-grade non-oriented silicon steel rough edge coil after cold rolling is ≤2mm, and the edge wave height is ≤4mm.
[0029] The technical concept of the present invention is as follows:
[0030] 1) For high-grade non-oriented silicon steel, especially silicon steel with high alloy content, its plasticity is slightly poor. At this time, the edge wave control mode (flatness control is released) is adopted for rolling, which can effectively reduce the occurrence of strip edge cracks during rolling. By rationally controlling the edge wave shape and speed during rolling, the strip breakage caused by strip deviation can be greatly reduced, and the occurrence of strip edge cracks can be reduced. Since the first pass has the largest reduction rate, the risk of edge cracks is the highest, and the greater the corresponding plate flatness. Since the edge of the hot-rolled coil is not trimmed, there is an obvious edge drop phenomenon, and the greater the edge drop, the more serious the uneven deformation of the edge, so the flatness control is looser, but the upper limit of the plate flatness control is too high, which will lead to excessively high edge waves of the subsequent finished product, increased cutting loss, and reduced yield rate. Therefore, the flatness control of the last pass is tightened to try to eliminate or reduce the edge waves generated in the previous pass. In summary, the first pass flatness control: 0.8×H 40 ≤F1≤0.8×H 40 +20, second pass straightness control: 0.6×H 40 ≤F2≤0.6×H 40 +20, final straightness control: 0.3×H 40 ≤F m ≤0.3×H 40 +20.
[0031] 2) Due to the large reduction rate in the first pass, the rollers heat up rapidly, increasing the risk of deformation and loss of rolls. On the other hand, the fluctuation of raw material thickness will cause uneven deformation. At the same time, the rolling speed directly affects the stability and deformation temperature of the rolling process. The appropriate rolling speed range can effectively control the deformation behavior of the material during the rolling process to avoid excessive strain rate and rolling force fluctuations. In the present invention, if the first rolling speed is too high and the strain rate is too large, the plate shape will not be adjusted in time and the strip will break. If the first rolling speed is too low, it will lead to too low deformation temperature and excessive cold deformation stress, which will affect the dimensional accuracy and surface quality of the product and reduce production efficiency. In addition, the higher the (Si+Al), the lower the first rolling speed range V is, which prevents the risk of edge cracking caused by high strain rate. Therefore, the present invention controls the first rolling speed V to: 1200-2.4×10 4 ×(Si+Al)≤V≤1200-1.8×10 4×(Si+Al).
[0032] 3) Due to the high alloy content, high brittleness and poor toughness of high-grade non-oriented silicon steel, increasing the plate temperature can effectively reduce deformation resistance and improve rollability. By increasing the strip temperature at a low flow rate, this method can be used to further increase the strip temperature, so that the resistance of the strip along the rolling direction is reduced and the cracks are reduced. On the other hand, due to the large rolling deformation during the first and second cold rolling processes, the rollers will experience thermal expansion. By maintaining an appropriate emulsion flow rate, the thermal expansion of the rollers can be eliminated, thereby effectively controlling the strip shape. During the rolling process, the emulsion can lubricate the friction interface between the roller and the strip and the roller support interface, thereby increasing the reduction, reducing the rolling pressure, and reducing the risk of edge cracks. Considering that the higher the (Si+Al), the higher the plate temperature requirement, the lower the emulsion flow rate, so the first and second emulsion flow rate L is controlled to be: 10000-1.4×10 5 ×(Si+Al)≤L≤10000-10 5 ×(Si+Al).
[0033] 4) The friction coefficient has a certain influence on the edge cracking. The larger the friction coefficient, the lighter the edge cracking of cold-rolled silicon steel. Therefore, increasing the friction coefficient can improve the edge cracking. The original roughness of the working roll will affect the rolling force and the thickness of the lubricating oil film, especially the first and second passes with the largest reduction. For high-grade non-oriented silicon steel, the higher the (Si+Al), the higher the required rolling force. Increasing the original roughness of the working roll can reduce the thickness of the lubricating oil film, increase the friction coefficient, and thus increase the rolling force, thereby reducing the incidence of edge cracking. However, the original roughness of the working roll will affect the working life of the roll. Excessive original roughness of the working roll will accelerate the wear of the working roll, produce meat defects, affect the plate surface quality and the life of the roll. Therefore, the original roughness R of the working roll is controlled to be: 50×(Si+Al)≤R≤100×(Si+Al).
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] The present invention adopts a large edge wave rolling mode and adjusts the rolling speed, emulsion flow rate, original roughness of the working roll, etc., to reduce the occurrence of cold-rolled edge cracks and edge waves of high-grade non-oriented silicon steel under the condition of no edge trimming of the hot-rolled raw materials. After rolling, no long continuous cracks occur, the edge crack depth is ≤2mm, and the edge wave height is ≤4mm, thereby achieving continuous and efficient production, reducing the amount of edge cutting loss after cold rolling, and improving the yield rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a comparison chart of the edge quality of the cold-rolled products 1-3 in Example 1 (left) and 1-5 in Comparative Example 1 (right). DETAILED DESCRIPTION
[0037] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with the embodiments, but the content of the present invention is not limited to the following embodiments.
[0038] In the following examples, the chemical composition and weight percentage content of high-grade non-oriented silicon steel are shown in Table 1, and the balance is Fe and unavoidable impurities.
[0039] Table 1 Chemical composition of steel and its weight percentage content
[0040] serial number C(%) S(%) N(%) Ti(%) P(%) Nb(%) Si(%) Al(%) Mn(%) Example 1 0.0025 0.0022 0.0024 0.0017 0.02 0.0021 2.2 0.8 0.52 Example 2 0.0031 0.0017 0.0018 0.0023 0.03 0.0013 3.5 0.5 0.24 Example 3 0.0018 0.0009 0.0012 0.0015 0.04 0.0018 2.7 1.1 0.65
[0041] In the following embodiments, the method for improving the quality of the cold-rolled edge of a high-grade non-oriented silicon steel rough edge coil comprises:
[0042] 1) Cold rolling adopts multi-stand continuous rolling mill or single-stand reversible rolling mill for 5 to 7 passes, and the flatness of the plate after the first, second and last passes is controlled to meet the following formula:
[0043] 0.8×H 40 ≤F1≤0.8×H 40 +20
[0044] 0.6×H 40 ≤F2≤0.6×H 40 +20
[0045] 0.3×H 40 ≤F m ≤0.3×H 40 +20
[0046] In the formula, F1, F2, F m They are the straightness after the first, second and last rolling passes, in I; H 40 It is the thickness difference between the hot rolled rough edge coil material 40mm away from the edge and the outermost edge, the average value of the whole coil is taken, in μm;
[0047] 2) The rolling speed of the first cold rolling pass satisfies the following formula:
[0048] 1200-2.4×10 4 ×(Si+Al)≤V≤1200-1.8×10 4 ×(Si+Al)
[0049] Wherein, V is the rolling speed, unit is m / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in the steel;
[0050] 3) The emulsion flow rate of the first and second cold rolling passes satisfies the following formula:
[0051] 10000-1.4×10 5×(Si+Al)≤L≤10000-10 5 ×(Si+Al)
[0052] Where, L is the emulsion flow rate of the first and second passes, unit L / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in steel;
[0053] 4) The original roughness of the cold rolling mill working roll satisfies the following formula:
[0054] 50×(Si+Al)≤R≤100×(Si+Al)
[0055] Where R is the original roughness of the working roll, in μm; (Si+Al) is the sum of the mass percentages of Si and Al in the steel.
[0056] Example 1 and Comparative Example 1
[0057] The high grade non-oriented silicon steel burrs used have (Si+Al)=3%, H 40 =50μm, thickness is 2.3mm, cold rolling is carried out by multi-stand continuous rolling mill for 5 passes, and the finished product thickness is 0.50mm. After calculation:
[0058] 1) The flatness of the plate after the first, second and last rolling passes must meet 40≤F1≤60, 30≤F2≤50, 15≤F m ≤35, unit I;
[0059] 2) The rolling speed of the first pass must meet 480≤V≤660, unit: m / min;
[0060] 3) The emulsion flow rate of the first and second passes must meet 5800≤L≤7000, unit L / min;
[0061] 4) The original roughness of the working roll must meet 1.5≤R≤3, unit: μm.
[0062] The actual process parameter control conditions and the edge quality conditions of the finished products after rolling in the embodiments and comparative examples are shown in Table 2.
[0063] Table 2
[0064]
[0065] As shown in Table 2, the edge quality of the finished product obtained in the embodiment is good. In Comparative Example 1-1, the rolling speed of the first pass is too high, and the flatness control of the first and second passes is too strict, resulting in strip breakage in the second pass of cold rolling. In Comparative Example 1-2, the emulsion flow rate of the first and second passes is too large, the original roughness of the working roll is too small, and the edge cracks of the rolled product are too large. In Comparative Example 1-3, the flatness control of the first, second and last passes is too loose, and the edge waves of the finished product are too large. In Comparative Example 1-4, the emulsion flow rate is too large, the original roughness of the working roll is too small, and the edge cracks of the finished product are too large. In Comparative Example 1-5, the emulsion flow rate is too small, the thermal expansion of the roller is not sufficiently eliminated, the lubrication of the roller and the steel plate surface is insufficient, and the flatness control of the first pass is too strict, resulting in excessive edge cracks of the finished product. Figure 1 This is a comparison chart of the edge quality of the cold-rolled finished products 1-3 (left) in Example 1 and 1-5 (right) in Comparative Example 1. The difference in effect can be intuitively felt from the figure. In Comparative Example 1-6, the second pass of plate flatness control is too strict, and the original roughness of the working roll is too large, resulting in large edge cracks in the finished product and pitting defects on the plate surface. In Comparative Example 1-7, the first pass rolling speed is too low, resulting in too low deformation temperature, large cold deformation stress, and large edge waves in the finished product.
[0066] Example 2 and Comparative Example 2
[0067] The high grade non-oriented silicon steel burrs used have (Si+Al) = 4%, H 40 =80μm, thickness is 2.1mm, cold rolling uses 20-roller single-stand reversible rolling mill for 5 passes, and the finished product thickness is 0.25mm. After calculation:
[0068] 1) The flatness of the plate after the first, second and last rolling passes must meet 64≤F1≤84, 48≤F2≤68, 24≤F m ≤44, unit I;
[0069] 2) The rolling speed of the first pass must meet 240≤V≤480, unit: m / min;
[0070] 3) The emulsion flow rate of the first and second passes must meet 4400≤L≤6000, unit L / min;
[0071] 4) The original roughness of the working roll must satisfy 2≤R≤4, unit: μm.
[0072] The actual process parameter control conditions and the edge quality conditions of the finished products after rolling in the embodiments and comparative examples are shown in Table 3.
[0073] Table 3
[0074]
[0075]
[0076] As shown in Table 3, the edge quality of the finished product obtained in the embodiment is good. In Comparative Example 2-1, the rolling speed of the first pass is too high, and the flatness control of the first pass is too strict, resulting in strip breakage in the first pass of cold rolling. In Comparative Example 2-2, the flatness control of the first pass is too strict, the emulsion flow rate of the first and second passes is too large, and the edge cracks of the rolled product are too large. In Comparative Example 2-3, the flatness control of the first, second and last passes is too loose, and the edge waves of the finished product are too large. In Comparative Example 2-4, the emulsion flow rate is too large, the original roughness of the working roll is too small, and the edge cracks of the finished product are too large. In Comparative Example 2-5, the emulsion flow rate is too small, and the flatness control of the first pass is too strict, resulting in excessive edge cracks of the finished product. In Comparative Example 2-6, the flatness control of the second pass is too strict, and the original roughness of the working roll is too large, resulting in large edge cracks of the finished product and pitting defects on the plate surface. In Comparative Example 2-7, the first rolling speed is too low, resulting in too low deformation temperature, large cold deformation stress, and large edge waves of the finished product.
[0077] Example 3 and Comparative Example 3
[0078] The high grade non-oriented silicon steel burrs used have (Si+Al) = 3.8%, H 40 =60μm, thickness is 1.6mm, cold rolling uses 20-roller single-stand reversible rolling mill for 6 passes, and the finished product thickness is 0.20mm. Calculation:
[0079] 1) The flatness of the plate after the first, second and last rolling passes must meet 48≤F1≤68, 36≤F2≤56, 18≤F m ≤38, unit I;
[0080] 2) The rolling speed of the first pass must meet 288≤V≤516, unit: m / min;
[0081] 3) The emulsion flow rate of the first and second passes must meet 4680≤L≤6200, unit L / min;
[0082] 4) The original roughness of the working roll must meet 1.9≤R≤3.8, unit: μm.
[0083] The actual process parameter control conditions and the edge quality conditions of the finished products after rolling in the embodiments and comparative examples are shown in Table 4.
[0084] Table 4
[0085]
[0086] As shown in Table 4, the edge quality of the finished product obtained in the embodiment is good. In Comparative Example 3-1, the rolling speed of the first pass is too high, and the flatness control of the first pass is too strict, resulting in strip breakage in the first pass of cold rolling. In Comparative Example 3-2, the flatness control of the first pass is too strict, the emulsion flow rate of the first and second passes is too large, and the edge cracks of the rolled product are too large. In Comparative Example 3-3, the flatness control of the first, second and last passes is too loose, and the edge waves of the finished product are too large. In Comparative Example 3-4, the emulsion flow rate is too large, the original roughness of the working roll is too small, and the edge cracks of the finished product are too large. In Comparative Example 3-5, the emulsion flow rate is too small, and the flatness control of the first pass is too strict, resulting in excessive edge cracks of the finished product. In Comparative Example 3-6, the flatness control of the second pass is too strict, and the original roughness of the working roll is too large, resulting in large edge cracks of the finished product and pitting defects on the plate surface. In Comparative Example 3-7, the first rolling speed is too low, resulting in too low deformation temperature, large cold deformation stress, and large edge waves of the finished product.
[0087] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.
Claims
1. A method for improving the quality of cold-rolled edges of high-grade non-oriented silicon steel rough edge coils. It is characterized in that Cold rolling adopts multi-stand continuous rolling mill or single-stand reversible rolling mill for 5 to 7 passes, and the flatness of the plate after the first, second and last passes is controlled to meet the following formula: 0.8×H 40 ≤F 1 ≤0.8×H 40 +20 0.6×H 40 ≤F 2 ≤0.6×H 40 +20 0.3×H 40 ≤F m ≤0.3×H 40 +20 In the formula, F 1 、F 2 、F m They are the straightness after the first, second and final rolling passes, in I; H 40 It is the thickness difference between the hot-rolled rough edge coil material 40mm away from the edge and the outermost edge. The average value of the whole coil is taken in μm.
2. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The H 40 ≤120μm.
3. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The rolling speed of the first pass of the cold rolling process satisfies the following formula: 1200-2.4×10 4 ×(Si+Al)≤V≤1200-1.8×10 4 ×(If+Al) Wherein, V is the rolling speed, unit is m / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in the steel.
4. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel burr coil according to claim 1, It is characterized in that The emulsion flow rate of the first and second cold rolling passes satisfies the following formula: 10000-1.4×10 5 ×(Si+Al)≤L≤10000-10 5 ×(If+Al) Wherein, L is the emulsion flow rate of the first and second passes, unit is L / min; (Si+Al) is the sum of the mass percentage contents of Si and Al in steel.
5. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The original roughness of the working roll of the cold rolling control mill satisfies the following formula: 50×(Si+Al)≤R≤100×(Si+Al) Where R is the original roughness of the working roll, in μm; (Si+Al) is the sum of the mass percentages of Si and Al in the steel.
6. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The sum of the mass percentage contents of Si and Al (Si+Al) in the high-grade non-oriented silicon steel is 2-4.5%.
7. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The chemical composition of the high-grade non-oriented silicon steel includes, by mass percentage, C≤0.004%, S≤0.003%, N≤0.003%, Ti≤0.003%, P≤0.05%, Nb≤0.003%, Si≤4.0%, Al≤2.0%, (Si+Al)2~4.5%, Mn≤2.0%, and the balance is Fe and unavoidable impurities.
8. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The thickness of the high-grade non-oriented silicon steel burr roll is 1.6-2.4 mm.
9. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel rough edge coil according to claim 1, It is characterized in that The thickness of the finished product of the high-grade non-oriented silicon steel burr coil after cold rolling is 0.20-0.50 mm.
10. The method for improving the cold-rolled edge quality of high-grade non-oriented silicon steel burr coil according to claim 1, It is characterized in that The edge crack depth of the finished product of the high-grade non-oriented silicon steel rough edge coil after cold rolling is ≤2mm, and the edge wave height is ≤4mm.
Citation Information
Patent Citations
Control method for high-mark non-oriented silicon steel cold continuous rolling edge crack
CN105396879A
Method for producing 0.35 mm non-oriented silicon steel through cold continuous rolling machine
CN111687210A
Diversified cross-connection control method for plate shape of hot rolling band steel
CN101372018A
Cold rolling method for high grade non-oriented silicon steel through hot rolling, acid pickling and non-edge-cutting
CN107962075A
Cold roller and cold rolling method