Ceramic shell for precision casting of oriented nickel-based superalloy and application of ceramic shell

By using ceramic shells prepared with materials such as Ca2Mg2Al28O46, the problem of thickness of the interface reaction layer in nickel-based high-temperature alloy casting is solved, and a higher quality casting surface and a lower production cost are achieved.

CN119076889APending Publication Date: 2024-12-06UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205518.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

During the casting process of nickel-based high-temperature alloy, the reaction of high-active elements with the ceramic shell surface layer leads to thick interface reaction layer, increasing production costs and affecting casting quality.

Method used

The ceramic shell prepared with a surface layer of 4-10% Ca2Mg2Al28O46, 60-66% white corundum powder and 30% silica sol binder, and the ceramic shell is prepared by specific impregnation, rotational slurry control, sanding, dewaxing and roasting. The process is to form a dense surface layer to reduce interface reactions.

Benefits of technology

The reaction layer thickness of nickel-based high-temperature alloy blades is significantly reduced, the surface quality of the castings is improved, the production cost is reduced, and the pass rate of the blades is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119076889A_ABST
    Figure CN119076889A_ABST
Patent Text Reader

Abstract

The embodiment of the invention discloses a ceramic shell for directional nickel-based superalloy precision casting and application of the ceramic shell. The ceramic shell for directional nickel-based superalloy precision casting comprises a surface layer and a back layer, and the surface layer is prepared from, by mass, 4%-10% of Ca2Mg2Al28O46, 60%-66% of white corundum powder and 30% of silica sol binder. The thickness of a reaction layer on the surface of an alloy blade obtained through precision casting of the ceramic shell is 20 microns and is far smaller than that of an alloy blade obtained in the prior art, and the ceramic shell has good application prospects in the field of precision casting of directional nickel-based high-temperature alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of precision casting, and in particular relates to a ceramic shell for directional nickel-based high-temperature alloy precision casting and application thereof. Background Art

[0002] Due to its excellent performance, oriented nickel-based high-temperature alloys are used as manufacturing materials for aircraft engine blades. At present, DZ406 blades represented by the second-generation oriented high-temperature alloy DZ406 are usually prepared by precision casting. The ceramic shell is an important guarantee for the preparation of DZ406 blades and plays a key role in the surface quality and performance of the blades. The ceramic shell is usually composed of a surface layer and a back layer. The surface layer is the part that directly contacts the alloy melt during alloy pouring, which is crucial to controlling the quality of DZ406 blades.

[0003] For directional nickel-based high-temperature alloys, the alloy contains highly active elements such as Hf and Al. During the pouring process, these highly active elements are easy to react with the surface layer of the ceramic shell, resulting in the appearance of an alloy / ceramic interface reaction layer, which increases the subsequent production cost. The existing shell is generally a white corundum shell, and the surface layer materials are mostly Al2O3 powder and silica sol. The current method of using white corundum shell casting to prepare DZ406 blades cannot well meet the high-quality casting of DZ406 blades. The surface of the cast casting has a lot of sand adhesion and a thick interface reaction layer. In order to eliminate the influence of sand adhesion and interface reaction layer on the casting, the casting is often polished. An excessively thick reaction layer will not only increase the subsequent production cost, but also affect the dimensional accuracy and greatly reduce the qualified rate of the blade. Therefore, the development of a new shell is of great significance to improving the quality of the blade. Summary of the invention

[0004] In view of this, on the one hand, some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, the ceramic shell comprising a surface layer and a back layer, the surface layer comprising 4-10% Ca2Mg2Al 28 O 46 , 60-66% white corundum powder and 30% silica sol binder.

[0005] Further, some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a method for preparing the ceramic shell includes:

[0006] Immerse the module in the surface slurry for a set time, and apply the surface slurry on the surface of the module;

[0007] Take out the module coated with the surface slurry and rotate it to control the slurry;

[0008] Place the slurry-coated module at 45° in a sand spraying machine and spray 100# corundum sand. After blowing off the floating sand, place the module in a ventilated place to dry, forming a surface layer on the module surface.

[0009] Immerse the module forming the surface layer in the back layer slurry for a set time, and apply the back layer slurry on the surface of the module;

[0010] The module coated with the backing layer slurry is placed in a sand spraying machine at 45 degrees and sprayed with 24# corundum sand. After blowing away the floating sand, the module is dried in a ventilated place to form a backing layer on the module surface layer;

[0011] The module forming the surface layer and the back layer is placed in a dewaxing kettle for dewaxing treatment; after dewaxing, it is calcined to obtain a ceramic shell.

[0012] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a method for preparing a surface layer slurry, including:

[0013] Place the silica sol binder, defoamer and wetting agent in a mixing bucket and stir evenly;

[0014] Then add white corundum powder, Ca2Mg2Al 28 O 46 , stirring to obtain a surface slurry; wherein, the viscosity is measured using a flow cup, and the viscosity of the surface slurry is 10-35s; wherein, Ca2Mg2Al 28 O 46 The preparation method comprises:

[0015] Al2O3, CaCO3, and MgO are uniformly mixed in a mass ratio of 83-86:10-12:2-5, and water is added as a binder to perform granulation;

[0016] Subsequently, the Ca2Mg2Al2O3 was formed by pressing at a pressure of 130-170 MPa and finally fired at 1700 °C for 6 h in a box furnace to obtain Ca2Mg2Al2O3. 28 O 46 .

[0017] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a method for preparing a backing slurry, including:

[0018] Weigh silica sol binder, defoamer and wetting agent into a mixing bucket and stir evenly;

[0019] Silica powder and white corundum powder were added in sequence and stirred to obtain a back layer slurry; wherein, the viscosity was measured using a flow cup, and the viscosity of the back layer slurry was 10 to 20 seconds.

[0020] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a dewaxing treatment method for forming the ceramic shell includes:

[0021] The module is placed in a dewaxing kettle and dewaxed with water vapor at 150-200°C. The dewaxing time shall not exceed 30 minutes.

[0022] In the ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in some embodiments, the D50 particle size of the white corundum powder is 25.00±5 μm.

[0023] In the ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in some embodiments, the content of SiO2 in the silica sol binder is 20-30wt%.

[0024] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, wherein the surface layer is a single-layer structure and the back layer is a seven-layer structure.

[0025] On the other hand, some embodiments disclose the use of a ceramic shell for directional nickel-based high-temperature alloy precision casting, wherein the ceramic shell is used for a nickel-based high-temperature alloy blade.

[0026] Some embodiments disclose the application of a ceramic shell for directional nickel-based high-temperature alloy precision casting, and the thickness of the reaction layer of the nickel-based high-temperature alloy blade is 20 μm.

[0027] The ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in the embodiment of the present invention and its application, the ceramic shell comprises a surface layer and a back layer, the surface layer is composed of 4-10% Ca2Mg2Al 28 O 46 , 60-66% white corundum powder and 30% silica sol binder; the obtained CMA ceramic shell can be used for precision casting of nickel-based high-temperature alloy blades; the DZ406 blades precision cast by using the CMA ceramic shell have a reaction layer thickness of 20μm on the surface, which is much smaller than the DZ406 blades obtained by the prior art, and has good application prospects in the field of precision casting of directional nickel-based high-temperature alloys. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is a cross-sectional view of the DZ406 alloy blade casting disclosed in Example 1;

[0029] Figure 2 is a cross-sectional view of the DZ406 alloy blade casting disclosed in Comparative Example 1;

[0030] Figure 3 is a cross-sectional view of the DZ406 alloy blade casting disclosed in Example 2;

[0031] Figure 4 is a cross-sectional view of the DZ406 alloy blade casting disclosed in Example 3;

[0032] Figure 5 Test diagram of the wetting angle of the ceramic shell and DZ406 alloy disclosed in Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0033] The word "embodiment" used herein as an "exemplary" does not necessarily mean that any embodiment described is superior or better than other embodiments. Performance index tests in the embodiments of the present invention are performed using conventional test methods in the art unless otherwise specified. It should be understood that the terms described in the embodiments of the present invention are only used to describe specific implementation methods and are not intended to limit the contents disclosed in the embodiments of the present invention.

[0034] Unless otherwise specified, the technical and scientific terms used herein have the same meanings as commonly understood by ordinary technicians in the technical field to which the embodiments of the present invention belong; other experimental methods and technical means not specifically specified in the embodiments of the present invention refer to experimental methods and technical means commonly used by ordinary technicians in the field.

[0035] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values ​​clearly listed as the limits of the range, but also all independent values ​​or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values ​​of 1% to 5%, but also the independent values ​​and sub-ranges within the range shown. Therefore, independent values ​​such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.

[0036] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.

[0037] In order to better illustrate the present invention, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present invention can be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the gist of the present invention.

[0038] Under the premise of no conflict, the technical features disclosed in the embodiments of the present invention may be arbitrarily combined, and the resulting technical solutions belong to the contents disclosed in the embodiments of the present invention.

[0039] In some embodiments, the ceramic shell for precision casting of directional nickel-based high-temperature alloy includes a surface layer and a back layer, and the surface layer is prepared by 4-10% Ca2Mg2Al28O46, 60-66% white corundum powder and 30% silica sol binder in terms of mass percentage. Generally, the directional nickel-based high-temperature alloy includes DZ406, DZ125, etc.

[0040] Generally, the surface material of the existing white corundum shell is mostly Al2O3 powder and silica sol. The surface material of the white corundum shell is composed of mullite Al2O3·SiO2 and Al2O3 at a melting temperature of 1540°C. 28 O 46 Added into the white corundum surface material, during the melting and casting process, SiO2 in the silica sol binder and Ca2Mg2Al 28 O 46 The products generated by the reaction include mullite Al2O3·SiO2, Al2O3 and 2% liquid slag, which contains Al2O3, SiO2, CaO and MgO. The liquid slag generated in the surface layer can make the surface layer more compact, reduce the reaction between the alloy melt and the ceramic shell during pouring, greatly reduce the thickness of the reaction layer on the surface of the alloy melt, and improve the surface properties of precision castings. Therefore, it can be considered that the Ca2Mg2Al2O3 added to the surface layer material 28 O 46 It can inhibit interface reactions, improve the surface quality of precision castings, and reduce subsequent production costs.

[0041] Some embodiments disclose a method for preparing a ceramic shell for directional nickel-based high-temperature alloy precision casting, comprising:

[0042] Immerse the module in the surface slurry for a set time, and apply the surface slurry on the surface of the module;

[0043] Take out the module coated with the surface slurry and rotate it to control the slurry;

[0044] Place the slurry-coated module at 45° in a sand spraying machine and spray 100# corundum sand. After blowing off the floating sand, place the module in a ventilated place to dry, forming a surface layer on the module surface.

[0045] Immerse the module forming the surface layer in the back layer slurry for a set time, and apply the back layer slurry on the surface of the module;

[0046] The module coated with the backing layer slurry is placed in a sand spraying machine at 45 degrees and sprayed with 24# corundum sand. After blowing away the floating sand, the module is dried in a ventilated place to form a backing layer on the module surface layer;

[0047] The module forming the surface layer and the back layer is placed in a dewaxing kettle for dewaxing treatment; after dewaxing, it is calcined to obtain a ceramic shell.

[0048] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a method for preparing a surface layer slurry, including:

[0049] Place the silica sol binder, defoamer and wetting agent in a mixing bucket and stir evenly;

[0050] Then add white corundum powder, Ca2Mg2Al 28 O 46 , stirring to obtain a surface slurry; wherein the viscosity is measured using a flow cup, and the viscosity of the surface slurry is 10 to 35 seconds;

[0051] Among them, Ca2Mg2Al 28 O 46 The preparation method comprises:

[0052] Al2O3, CaCO3, and MgO are uniformly mixed in a mass ratio of 83-86:10-12:2-5, and water is added as a binder to perform granulation;

[0053] Subsequently, the Ca2Mg2Al2O3 was formed by pressing at a pressure of 130-170 MPa and finally fired at 1700 °C for 6 h in a box furnace to obtain Ca2Mg2Al2O3. 28 O 46 .

[0054] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a method for preparing a backing slurry, including:

[0055] Weigh silica sol binder, defoamer and wetting agent into a mixing bucket and stir evenly;

[0056] Silica powder and white corundum powder were added in sequence and stirred to obtain a back layer slurry; wherein, the viscosity was measured using a flow cup, and the viscosity of the back layer slurry was 10 to 20 seconds.

[0057] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, and a dewaxing treatment method for forming the ceramic shell includes:

[0058] The module is placed in a dewaxing kettle and dewaxed with water vapor at 150-200°C. The dewaxing time shall not exceed 30 minutes.

[0059] In the ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in some embodiments, the D50 particle size of the white corundum powder is 25.00±5 μm.

[0060] In the ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in some embodiments, the content of SiO2 in the silica sol binder is 20-30wt%.

[0061] Some embodiments disclose a ceramic shell for directional nickel-based high-temperature alloy precision casting, wherein the surface layer is a single-layer structure and the back layer is a seven-layer structure.

[0062] In some embodiments, the surface layer of the ceramic shell is a single layer, and the back layer is composed of seven back layers, wherein the seventh back layer is coated with slurry without being sanded.

[0063] Some embodiments disclose the application of a ceramic shell for directional nickel-based high-temperature alloy precision casting, and the ceramic shell is used to cast alloy blades. Generally, directional nickel-based high-temperature alloy precision casting requires the use of a ceramic shell. In the embodiment of the present invention, Ca2Mg2Al 28 O 46 The ceramic shell prepared by the powder can be called a CMA ceramic shell. The CMA ceramic shell is placed in a directional furnace to prepare a nickel-based high-temperature alloy blade according to a high-temperature alloy preparation process, for example, a DZ406 blade casting.

[0064] The technical details are further illustrated below in conjunction with embodiments.

[0065] Example 1

[0066] The method for preparing a ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in Example 1 includes preparing a surface layer slurry, preparing a back layer slurry and preparing a ceramic shell;

[0067] Wherein, the preparation method of the surface slurry comprises:

[0068] Place the silica sol binder, defoamer and wetting agent in a stirring bucket and stir for 20 minutes until uniform;

[0069] Then add white corundum powder, Ca2Mg2Al 28 O 46 , stirring for 3h to obtain the surface slurry; wherein, the viscosity of the surface slurry is measured by flow cup, and the viscosity of the surface slurry is 10s; the surface slurry is composed of 7% Ca2Mg2Al 28 O 46 , 63% white corundum powder and 30% silica sol binder;

[0070] Among them, the preparation materials of the surface slurry include Ca2Mg2Al 28 O 46, silica sol binder, silica powder, white corundum powder, defoaming agent, wetting agent; the mass ratio of silica powder to white corundum is 2:1; the D50 particle size of white corundum powder is 25.00±5μm, and the D50 particle size of silica powder is 0.3μm; the SiO2 content in the silica sol binder is 20wt%; the defoaming agent is a mixture of organic silane defoaming agent and n-octanol, and the wetting agents are all gemini siloxane wetting agents. Calculated by weight, 1 part of silica sol binder is equipped with 0.05 parts of defoaming agent and 0.03 parts of wetting agent.

[0071] Among them, Ca2Mg2Al 28 O 46 The preparation method comprises:

[0072] Al2O3, CaCO3, and MgO are uniformly mixed in a mass ratio of 83:12:5, and water is added as a binder for granulation;

[0073] Subsequently, the Ca2Mg2Al2O3 was formed by pressing at a pressure of 130-170 MPa and finally fired at 1700 °C for 6 h in a box furnace to obtain Ca2Mg2Al2O3. 28 O 46 .

[0074] The method for preparing the back layer slurry comprises:

[0075] Weigh silica sol binder, defoamer and wetting agent into a stirring bucket and stir for 20 minutes until uniform;

[0076] Silica powder and white corundum powder were added in sequence and stirred to obtain a back layer slurry; wherein, the viscosity was measured using a flow cup, and the viscosity of the back layer slurry was 10s.

[0077] Among them, the preparation materials of the back layer slurry include silica sol binder, silica powder, white corundum powder, defoamer, and wetting agent. The mass ratio of silica powder to white corundum is 2:1; the D50 particle size of white corundum powder is 25.00±5μm, and the D50 particle size of silica powder is 0.3μm; the SiO2 content in the silica sol binder is 20wt%; the defoamer is a mixture of organic silane defoamer and n-octanol, and the wetting agents are all geminisiloxane wetting agents. By weight, 1 part of silica sol binder is equipped with 0.05 parts of defoamer and 0.03 parts of wetting agent.

[0078] The method for preparing the ceramic shell includes:

[0079] Slowly immerse the wax model module into the surface slurry to ensure that the module is completely immersed in the surface slurry. Immerse for 1 minute and apply the surface slurry on the surface of the module.

[0080] Take out the module coated with the surface slurry, and rotate and control the slurry for 40 seconds;

[0081] Place the slurry-coated module at 45° in a sand spraying machine and spray 100# corundum sand. After blowing off the floating sand, place the module in a ventilated place to dry for 10 hours to form a surface layer on the module surface.

[0082] Slowly immerse the module forming the surface layer into the back layer slurry to ensure that the module is completely immersed in the back layer slurry. Immerse for 1 minute and apply the back layer slurry on the surface of the module.

[0083] The module coated with the backing layer slurry is placed in a sand spraying machine at 45 degrees and sprayed with 24# corundum sand. After blowing off the floating sand, the module is dried in a ventilated place for 10 hours to form a backing layer on the surface layer of the module;

[0084] The module forming the surface layer and the back layer is placed in a dewaxing kettle and subjected to steam dewaxing treatment at 150° C. for 30 minutes; after dewaxing, it is calcined at 800° C. to obtain a CMA ceramic shell.

[0085] Comparative Example 1

[0086] Comparative Example 1 discloses a method for preparing a white corundum ceramic shell. The specific preparation method is referred to Example 1, wherein the surface slurry is composed of 70% white corundum powder and 30% silica sol binder, and no Ca2Mg2Al2O3 is added. 28 O 46 .

[0087] Add 10% Ca2Mg2Al 28 O 46 The wetting experiment of the CMA ceramic shell with powder and the white corundum ceramic shell prepared in comparative example 1 with DZ406 alloy was carried out. The experiment was carried out in a visual high temperature contact angle tester, the experimental temperature was 1540℃, and the vacuum degree was controlled at 10 -4 Pa. Figure 5 As shown in the figure, after measurement, it was found that the contact angle between the white corundum ceramic shell and the DZ406 alloy was 92°. Figure 5 As shown in (a), the contact angle between the CMA ceramic shell and the DZ406 alloy is 120°. Figure 5 Generally speaking, the wetting angle has a greater impact on the interface reaction. The larger the wetting angle, the more difficult the interface reaction is. 28 O 46 The addition of powder makes the wettability of the alloy / ceramic shell system worse, which is beneficial to improving the surface quality of the alloy casting.

[0088] The CMA ceramic shell prepared in Example 1 and the white corundum ceramic shell prepared in Comparative Example 1 were precision casted respectively, and DZ406 blades were prepared by the same casting process;

[0089] The blades obtained by precision casting of the CAM ceramic shell and the white corundum ceramic shell obtained in Example 1 and Comparative Example 1 were randomly sampled and observed and counted by electron microscope. 50 samples of the blades cast by the CMA ceramic shell and the blades cast by the white corundum ceramic shell were taken at the same position for scanning electron microscope analysis, 20 pictures of each sample were taken by electron microscope, and the reaction layer presented in each picture was photographed and counted, and the average value was calculated. The reaction layer of the alloy blade casting cast by the CMA ceramic shell was about 20 μm, and the reaction layer of the casting cast by the white corundum ceramic shell was about 60 μm.

[0090] like Figure 1 The cross-sectional view of the DZ406 blade casting cast from the CMA ceramic shell obtained in Example 1 is shown. Figure 2 This is a cross-sectional view of a DZ406 alloy blade casting cast from a white corundum ceramic shell obtained in Comparative Example 1; Figure 1 and Figure 2 At the interface between the alloy blade casting cast by the CMA ceramic shell and the DZ406 blade casting cast by the white corundum ceramic shell, it was found that the reaction layer of the alloy blade casting cast by the CMA ceramic shell was about 20μm, and the reaction layer of the casting cast by the white corundum ceramic shell at the production site was about 60μm.

[0091] Example 2

[0092] The method for preparing a ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in Example 2 is based on Example 1, wherein the surface slurry is composed of 4% Ca2Mg2Al 28 O 46 , 66% white corundum powder and 30% silica sol binder.

[0093] The CMA ceramic shell obtained in Example 2 is used to precision cast the DZ406 blade. Figure 3 This is a cross-sectional view of the DZ406 blade obtained in Example 2; the blade interface reaction layer has an average thickness of about 20 μm.

[0094] Example 3

[0095] The method for preparing a ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in Example 3 is based on Example 1, wherein the surface slurry is composed of 10% Ca2Mg2Al 28 O 46 , 60% white corundum powder and 30% silica sol binder;

[0096] The CMA ceramic shell obtained in Example 3 is used to precision cast the DZ406 blade. Figure 4The cross-sectional view of the DZ406 blade obtained in Example 3; the average thickness of the blade interface reaction layer is about 18 μm. The ceramic shell for directional nickel-based high-temperature alloy precision casting disclosed in the embodiment of the present invention and its application, the ceramic shell includes a surface layer and a back layer, the surface layer is composed of 4-10% Ca2Mg2Al 28 O 46 , 60-66% white corundum powder and 30% silica sol binder. The obtained CMA ceramic shell can be used for precision casting of nickel-based high-temperature alloy blades; the DZ406 alloy blades precision cast by using the CMA ceramic shell have a reaction layer thickness of 20μm on the surface, which is much smaller than the DZ406 alloy blades obtained by the prior art. It can effectively improve the surface quality of the blades, improve the qualified rate of blade products, and reduce subsequent production costs. It has good application prospects in the field of precision casting of directional nickel-based high-temperature alloys.

[0097] The technical solutions disclosed in the embodiments of the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the embodiments of the present invention. Any conventional changes, replacements or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.

Claims

1. Ceramic shell for directional nickel-based high-temperature alloy precision casting, It is characterized in that The ceramic shell comprises a surface layer and a back layer. In terms of mass percentage, the surface layer is composed of 4 to 10% Ca 2 Mg 2 Al 28 O 46 , 60-66% white corundum powder and 30% silica sol binder.

2. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 1, It is characterized in that The method for preparing the ceramic shell comprises: Immerse the module in the surface slurry for a set time, and apply the surface slurry on the surface of the module; Take out the module coated with the surface slurry and rotate it to control the slurry; Place the module coated with slurry after slurry control in a sand spraying machine at 45 degrees to spray sand, blow off the floating sand and place the module in a ventilated place to dry, forming a surface layer on the surface of the module; Immerse the module forming the surface layer in the back layer slurry for a set time, and apply the back layer slurry on the surface of the module; The module coated with the backing layer slurry is placed in a sand spraying machine at 45 degrees to spray sand. After blowing away the floating sand, the module is dried in a ventilated place to form a backing layer on the module surface layer. The module forming the surface layer and the back layer is placed in a dewaxing kettle for dewaxing treatment; after dewaxing, it is calcined to obtain a ceramic shell.

3. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 2, wherein the preparation method of the surface layer slurry include: Place the silica sol binder, defoamer and wetting agent in a mixing bucket and stir evenly; Then add white corundum powder, Ca 2 Mg 2 Al 28 O 46 , stirring to obtain a surface slurry; wherein, the viscosity is measured using a flow cup, and the viscosity of the surface slurry is 10 to 35 seconds; wherein, the Ca 2 Mg 2 Al 28 O 46 The preparation method comprises: Al 2 O 3 、CaCO 3 , MgO are mixed evenly in a mass ratio of 83-86:10-12:2-5, and water is added as a binder to perform granulation; Subsequently, the CaO2 was formed by pressing at a pressure of 130-170 MPa and finally fired at 1700 °C for 6 h in a box furnace to obtain the CaO2 2 Mg 2 Al 28 O 46 .

4. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 2, It is characterized in that The preparation method of the back layer slurry comprises: Weigh silica sol binder, defoamer and wetting agent into a mixing bucket and stir evenly; Silica powder and white corundum powder were added in sequence and stirred to obtain a back layer slurry; wherein, the viscosity was measured using a flow cup, and the viscosity of the back layer slurry was 10 to 20 seconds.

5. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 2, It is characterized in that The dewaxing process for forming a ceramic shell includes: The module is placed in a dewaxing kettle and dewaxed with water vapor at 150-200°C. The dewaxing time shall not exceed 30 minutes.

6. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 1, It is characterized in that The D50 particle size of the white corundum powder is 25.00±5 μm.

7. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 1, It is characterized in that The silica sol binder contains SiO 2 The content is 20-30wt%.

8. The ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 1, It is characterized in that The surface layer is a single-layer structure, and the back layer is a seven-layer structure.

9. Application of the ceramic shell for directional nickel-based high-temperature alloy precision casting according to any one of claims 1 to 8, It is characterized in that The ceramic shell is used for casting nickel-based high-temperature alloy blades.

10. Application of the ceramic shell for directional nickel-based high-temperature alloy precision casting according to claim 9, It is characterized in that The thickness of the reaction layer of the nickel-based high-temperature alloy blade is 20 μm.