Building ceramic tile with cloisonne enamel effect and preparation method thereof

Through the combination of digital inkjet and glue drying machine, combined with metal and sunken ink and dry particles, the diversified metal texture and enamel color effects of ceramic tiles are achieved, solving the problem of single effect of existing ceramic tiles and enhancing the art of products Ornamental and competitive.

CN119077912APending Publication Date: 2024-12-06GUANGXI MONALISA NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128445.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing ceramic tile pattern and metal effects are single, and it is impossible to achieve more other effects types that customers want, and it is difficult to achieve the richness of patterns and metal effects.

Method used

The digital inkjet machine and glue dry granulator are combined to achieve regional metallic and glitter effects by printing metal ink and sunken ink, paired with gold or colored dry granulates, and enhance the enamel color effect through transparent hair color glaze formula.

Benefits of technology

It realizes the diversified metal texture and enamel color effects of the surface of the ceramic tile, enriches the pattern and metal effects, and enhances the artistic ornamentality and core competitiveness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119077912A_ABST
    Figure CN119077912A_ABST
Patent Text Reader

Abstract

The invention discloses a building ceramic tile with a cloisonne enamel effect and a preparation method of the building ceramic tile, and relates to the technical field of building ceramic tiles. The ceramic tile sequentially comprises a green body layer, a cover glaze layer, a pattern layer, a glue layer, a dry particle layer and a transparent color-emitting glaze layer from bottom to top, the pattern layer is formed by printing a cloisonne enamel pattern file on the cover glaze layer by using a digital ink jet machine; according to the glue layer, digital glue is printed on the surface of the blank body layer after the patterns are printed in an ink-jet mode through a glue dry particle machine, and a file for printing the glue is a file which is manufactured by printing a cloisonne enamel pattern file through a digital ink-jet machine and has the metal flashing and sinking effects. It is ensured that the digital glue printing position and the cloisonne enamel pattern printed by the digital ink jet machine are completely matched and overlapped; the dry particle layer is coated with golden dry particles and / or colored dry particles. The problem that an existing ceramic tile is single in pattern and metal effect is solved, the regional metal and glittering effect can be achieved according to pattern requirement positioning, and the cloisonne enamel effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building ceramic tiles, and in particular to a building ceramic tile with cloisonné enamel effect and a preparation method thereof, involving the use of gold-plated dry particles, golden flashing dry particles with metal ink and sunken ink to achieve a unique metal texture effect on the brick surface, and at the same time matching enamel effect patterns to achieve a thick and gorgeous enamel color effect. Background Art

[0002] Cloisonné is one of China's famous special metal crafts and a national intangible cultural heritage. It is an artifact made by pinching soft flat copper wire into various patterns on a copper mold, welding them on the copper mold, and then filling the patterns with enamel glaze and firing them. Cloisonné is deeply loved by people for its brilliant gold, complete glaze colors, fine and smooth porcelain, and bright and bright colors. Incorporating the characteristics of cloisonné enamel into architectural ceramic products can enrich the types and decorative effects of ceramic tiles and enhance the artistic appreciation and core competitiveness of products.

[0003] The patterns and metal effects of tiles on the market are currently single, and cannot achieve more other types of effects that customers want. For example, in the patent "Porcelain tiles with glittering effects and preparation methods thereof" application number: 202110860650.3, the metal glitter particles and the matte glaze are evenly mixed and then poured on the tile surface through a bell jar glaze. The metal effect of the tiles produced by this solution is relatively single, and cannot achieve more other types of effects that customers want.

[0004] Patent "Glare Antique Tiles and Preparation Methods Thereof" application number: 202011580498.5 is to apply a base glaze first, mix and stir the glittering particles and suspended glue evenly to obtain glittering particle glaze, spray the glittering particle glaze on the base glaze layer, and then mix and stir the glaring particles, metal particles, suspended glue and transparent glaze to obtain a mixed particle glaze, and finally pour the mixed particle glaze on the brick surface by pouring glaze. The tile pattern and metal effect produced by this solution are single, and cannot achieve more other effect types that customers want.

[0005] Patent application number: 201020610978.7 of "A Glazed Tile with Metallic Effect" first applies the surface glaze, and then prints metal particles or prints full glaze on the tile surface. The metal effect of the tiles produced by this solution is relatively simple and cannot achieve more other effects that customers want.

[0006] The public technical solution "A method for producing metallic glare and glitter tiles" was published in Foshan Ceramics, Issue 11 (Issue 304) in 2021. The solution is to mix metal dry particles, crystal dry particles, transparent dry particles and suspending agents evenly, and then pour them on the tile surface through a bell jar glaze. The tile pattern and metal effect produced by this solution are single, and cannot achieve more other effect types that customers want.

[0007] In summary, how to obtain tiles with rich patterns and metallic effects is an urgent problem to be solved in the current tile field. Summary of the invention

[0008] In view of the above shortcomings, the present invention provides a building ceramic tile with cloisonné effect and a preparation method thereof, which solves the problem of single pattern and metal effect of existing ceramic tiles, and can realize regional metal and glitter effects according to the requirements of the pattern, and realize the cloisonné effect. The specific technical scheme is as follows:

[0009] A building ceramic tile with cloisonné enamel effect, the building ceramic tile with cloisonné enamel effect comprising, from bottom to top, a body layer, a surface glaze layer, a pattern layer, a glue layer, a dry particle layer, and a transparent color-generating glaze layer;

[0010] The pattern layer is a cloisonné enamel pattern file printed on the glaze layer using a digital inkjet machine using metallic ink and a new type of sinking functional ink;

[0011] The glue layer is made by printing digital glue on the surface of the blank layer after the inkjet printing pattern with a glue dryer. The file for printing the glue is a file with metallic glitter and sinking effect produced by printing the cloisonné pattern file with a digital inkjet machine. Through precise alignment, it is ensured that the position of the digital glue printing is completely consistent with the cloisonné pattern printed by the digital inkjet machine.

[0012] The dry particle layer is coated with golden dry particles and / or colored dry particles.

[0013] Furthermore, the chemical composition of the green body powder on the green body layer includes, by mass percentage, loss on ignition: 3.8-4.6%, SiO2: 65-70%, Al2O3: 18-22%, Fe2O3: 0.3-0.8%, TiO2: 0.1-0.2%, CaO: 0.3-0.8%, MgO: 0.5-1.0%, K2O: 3.0-4.0% and Na2O: 2.0-3.0%; the particle grading of the green body powder includes, by mass percentage, 20 mesh: ≦1%, above 30 mesh: 10-20%, 30-60 mesh: 65-75%, 60-80 mesh: ≦12%, below 80 mesh: ≦6%.

[0014] Furthermore, the chemical composition of the top glaze on the top glaze layer includes, in mass percentage, loss on ignition: 2.0-5.0%, SiO2: 55-65%, Al2O3: 18-21%, Fe2O3: 0.1-0.2%, TiO2: 0.03-0.05%, CaO: 0.5-1.0%, MgO: 1.0-2.0%, K2O: 0.8-1.2%, Na2O: 4.0-5.0%, BaO: 5.0-6.0%, ZrO2: 4.0-5.0%, and the sum of the mass percentages of the chemical compositions is 100%; the fineness requirement of the top glaze is that the residue on the 325 mesh sieve reaches 0.5-0.8wt%.

[0015] Furthermore, the particle gradation of the dry particle layer includes: in terms of mass percentage, 85%-90% for 100-200 mesh, 5%-10% for above 100 mesh, and less than 5% for below 200 mesh.

[0016] Furthermore, the formula of the transparent color glaze is: a part of albite (0≤a≤43), b parts of potassium feldspar (a+b=43), 8 parts of kaolin, 3 parts of calcined kaolin, c parts of strontium carbonate (6≤c≤12), d parts of quartz (6≤d≤20), e parts of dolomite (8≤e≤12), f parts of calcite (3≤f≤10), g parts of talc (4≤g≤12), h parts of zinc oxide (2≤h≤6), and 1 part of zirconium silicate, wherein c+d+e+f+g+h=45.

[0017] The present invention also provides a method for preparing a building ceramic tile with cloisonné effect, comprising the following steps:

[0018] (1) making a green body, which is polished and dried to obtain a green body with a certain strength;

[0019] (2) spraying water to moisten the surface of the blank and applying a glaze layer;

[0020] (3) Using a digital inkjet printer to print the cloisonné enamel pattern file on the surface of the blank after the top glaze layer is applied, the color and texture of the design pattern can be appropriately adjusted according to the requirements of the metal flash and sinking effect;

[0021] (4) using a glue dryer to print digital glue on the surface of the brick blank after the cloisonné enamel pattern is printed by inkjet printing;

[0022] (5) golden dry particles and / or colored dry particles are placed on the surface of the brick blank printed with digital glue, the fan speed is controlled to be 1500-2000r / min, and the dry particles not on the digital glue layer are sucked away by the fan to obtain a dry particle layer with a thickness of 1-3mm; the golden dry particles are made of iron chrome brown and titanium yellow as seeds, the golden dry particles are gold-plated dry particles or golden flash dry particles; the colored dry particles are made of cobalt oxide, copper oxide, titanium dioxide, etc. as main raw materials;

[0023] (6) spraying transparent coloring glaze on the surface of the brick with Bugan particles;

[0024] (7) Dry and fire the bricks sprayed with transparent colored glaze. The kiln firing cycle is 40-50 minutes. The highest temperature in the high temperature zone is 1200-1215°C (kiln surface temperature). Then, you can get tiles with cloisonné enamel effect on the surface.

[0025] Furthermore, in step (1), the drying is carried out in a drying kiln, the drying kiln is a four-layer drying kiln, 100M long, the drying time is 40-60min, and the moisture content of the green body after drying is controlled to be 0.2-0.4wt%.

[0026] Furthermore, in step (2), the water spraying is performed using two spray guns with nozzle sizes of 0.52-0.62 mm, and the water spraying amount is 60-100 g / m 2 The process parameters of the glaze layer are: the glaze amount is 480-580g / m 2 , specific gravity is 1.82-1.92g / ml, and flow rate is 26-32 seconds.

[0027] Furthermore, in step (4), the grayscale value of the digital glue printing is 10-100%, and the thermal decomposition temperature of the digital glue is 600-800°C.

[0028] Furthermore, in step (6), the process parameters for spraying the transparent color glaze are: glaze spraying amount: 350-450g / m 2 , specific gravity is 1.40-1.50g / ml; two caliber spray guns are used to spray transparent color glaze: 0.52mm spray gun A and 0.62mm spray gun B; there are two groups of spray gun A and four groups of spray gun B; the installation order of the six groups of spray guns is: spray gun A→spray gun B→spray gun B→spray gun B→spray gun A; in order to avoid uneven local glaze spraying and large deviation of glaze spraying amount on both sides and the middle position, the distance between spray gun A and spray gun B is 30cm, and the distance between spray gun B and spray gun B is 20 cm; and with the middle of the brick as the reference line, six groups of spray guns are 5 cm away from the reference line, and are arranged in sequence one left and one right of the reference line, which can effectively ensure that the glaze sprayed on both sides of the brick is close to that in the middle; the height between the nozzle and the brick surface is 80-90 cm, the spray gun is at an angle of 45 degrees to the brick surface, the gun nozzle is tilted backwards, and if the spray gun is vertical to the brick surface, the transparent colored glaze will easily blow away the dry particles; when spraying transparent colored glaze, the pressure of the high-pressure glaze sprayer is set to 4-4.5 MPa.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The present invention uses a digital glue dry granulator to position dry granules with different effects, and uses metal ink and sinking ink to achieve the purpose of enriching patterns and metal effects through inkjet printing. Among them, gold dry granules, colored dry granules and metal inks are used in combination to achieve a unique metal texture effect on the brick surface; a new type of sinking functional ink is developed and colored dry granules are used to match the enamel effect pattern to achieve a thick and gorgeous enamel color effect; a digital glue dry granulator is used to position dry granules with different effects, combined with unique effect dry granule crystallization technology and new sinking functional ink technology, to achieve a cloisonné enamel effect on the surface of building ceramic tiles.

[0031] 2. The present invention adopts golden dry particles with iron chrome brown and titanium yellow as crystal seeds and digital glue dry particle machine positioning process technology combined with digital inkjet printing technology, so that the digital glue printing and the design pattern file are accurately overlapped, and the golden dry particles are applied and bonded with the digital glue to achieve accurate overlap with the design pattern texture.

[0032] 3. The present invention adopts colored dry particles with cobalt oxide, copper oxide, titanium dioxide, etc. as main raw materials and digital glue dry particle machine positioning process technology combined with digital inkjet printing technology, so that the digital glue printing and the design pattern file are accurately overlapped, and the colored dry particles are applied and bonded with the digital glue to achieve accurate overlap with the design pattern texture.

[0033] 4. The present invention has developed a transparent color glaze formula that can achieve a cloisonné enamel effect on the surface of ceramic tiles. Increasing the quartz content in the formula helps the color to turn blue, and adjusting the ratio of strontium carbonate, dolomite, calcite, talc and zinc oxide at the same time, thereby achieving the purpose of ensuring stable glaze color and excellent anti-fouling performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below.

[0035] Figure 1 is a process flow chart of the present invention; DETAILED DESCRIPTION

[0036] The specific embodiments of the present invention are described in detail below, but it should be understood that the protection scope of the present invention is not limited by the specific embodiments.

[0037] Example 1

[0038] The present embodiment of a building ceramic tile with cloisonné enamel effect comprises, from bottom to top, a body layer, a glaze layer, a pattern layer, a glue layer, a dry particle layer, and a transparent coloring glaze layer. The specific preparation method is:

[0039] (1) The green body is obtained by pressing. The chemical composition of the green body powder includes: by mass percentage, ignition loss: 3.8%, SiO2: 68%, Al2O3: 21%, Fe2O3: 0.3%, TiO2: 0.1%, CaO: 0.3%, MgO: 0.5%, K2O: 3.0, Na2O: 3.0%. The particle size distribution of the powder includes: by mass percentage, 20 mesh: 0.5%, above 30 mesh: 10%, 30-60 mesh: 75%, 60-80 mesh: 12%, below 80 mesh: 2.5%.

[0040] (2) After the formed green body is polished by a green body grinding machine, it is dried in a drying kiln to obtain a green body with a certain strength. The drying kiln is a four-layer drying kiln with a length of 100M. The drying time can be 40min, and the moisture content of the green body after drying is controlled at 0.4wt%.

[0041] (3) Spray water to moisten the surface of the blank. Water spraying amount: 60g / m 2 , using two spray guns, nozzle size: 0.52mm.

[0042] (4) Apply the top glaze layer by bell jar glazing method. The process parameters of the top glaze are: glaze amount 480g / m 2 , specific gravity is 1.82g / ml, flow rate is 26 seconds. The chemical composition of the glaze includes, by mass percentage, loss on ignition: 2.0%, SiO2: 63%, Al2O3: 19.57%, Fe2O3: 0.1%, TiO2: 0.03%, CaO: 0.5%, MgO: 1.0%, K2O: 0.8%, Na2O: 4.0%, BaO: 5.0%, ZrO2: 4.0%, the sum of the mass percentages of the chemical composition is 100%. The fineness requirement of the glaze is that the residue on the 325 mesh screen reaches 0.5wt%.

[0043] (5) After applying the top glaze layer, the surface of the blank is printed with a digital inkjet machine using metallic ink and a new type of sinking function ink to print the cloisonné enamel pattern file. The color and texture of the design pattern can be appropriately adjusted according to the requirements of the metal flash and sinking effect.

[0044] (6) After the inkjet printing pattern, the surface of the brick blank is printed with digital glue using a glue dryer. The file for printing glue is a file with metallic glitter and sinking effect produced by printing the cloisonné pattern file using a digital inkjet machine. Through precise alignment, ensure that the position of the digital glue printing is completely consistent with the cloisonné pattern printed by the digital inkjet machine. The gray value of the digital glue printing is 10%, and the thermal decomposition temperature of the digital glue is 600°C.

[0045] (7) Gold-plated dry particles and golden flash dry particles are placed on the surface of the brick blank printed with digital glue, and the fan speed is controlled to 1500r / min. The dry particles not on the digital glue layer are sucked away by the fan to obtain a dry particle layer with a thickness of 1mm. The particle grading is 100-200 mesh: 88%, above 100 mesh: 8%, below 200 mesh: 4%.

[0046] The parameters involved in steps (5) to (7) are:

[0047]

[0048] (8) Spray transparent color glaze on the surface of the brick with Bugan particles:

[0049] Transparent color glaze formula: 3 parts of sodium feldspar, 40 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 10 parts of strontium carbonate, 8 parts of quartz, 10 parts of dolomite, 5 parts of calcite, 8 parts of burnt talc, 4 parts of zinc oxide, and 1 part of zirconium silicate.

[0050] The process parameters for spraying transparent color glaze are: spraying glaze amount: 350g / m 2 , specific gravity is 1.40g / ml.

[0051] The specific spraying method is: mix the required raw materials evenly in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.4% (325 mesh sieve), age for 18 hours, control the specific gravity to 1.40, and use the glaze spraying process to apply the glaze to the surface of the brick with dry particles.

[0052] Two caliber spray guns are used to spray transparent colored glaze: 0.52mm spray gun A and 0.62mm spray gun B; among them, spray gun A is divided into two groups, and spray gun B is divided into four groups; the installation order of the six groups of spray guns is: spray gun A→spray gun B→spray gun B→spray gun B→spray gun A; in order to avoid uneven local glaze spraying and large deviation of glaze spraying amount between the two sides and the middle position, the distance between spray gun A and spray gun B is 30cm, and the distance between spray gun B and spray gun B is 20cm; and taking the middle position of the brick as the reference line, the six groups of spray guns are 5cm away from the reference line respectively, and are arranged in sequence one left and one right according to the reference line, which can effectively ensure that the glaze spraying amount between the two sides and the middle position of the brick is close; the height of the nozzle and the surface of the brick is 80cm, the spray gun is inclined at a 45-degree angle to the surface of the brick, the nozzle is tilted backward, and the spray gun is perpendicular to the brick surface, and the transparent colored glaze is easy to blow away the dry particles; when spraying transparent colored glaze, the pressure of the high-pressure glaze sprayer is set to 4mpa.

[0053] (9) After spraying transparent color glaze, the brick blank is dried in the pre-kiln drying kiln and then fired in the kiln. The firing temperature is 1140℃ and the firing time is 40min. After firing, the tile with cloisonné effect on the surface is obtained. The glossiness and dirt absorption are measured, and the glaze surface and the cloisonné effect are observed visually.

[0054] Example 2

[0055] The present embodiment of a building ceramic tile with cloisonné enamel effect comprises, from bottom to top, a body layer, a glaze layer, a pattern layer, a glue layer, a dry particle layer, and a transparent coloring glaze layer. The specific preparation method is:

[0056] (1) The green body is obtained by pressing. The chemical composition of the green body powder includes: by mass percentage, ignition loss: 4.2%, SiO2: 68%, Al2O3: 18%, Fe2O3: 0.8%, TiO2: 0.2%, CaO: 0.8%, MgO: 1.0%, K2O: 4.0, Na2O: 3.0%. The particle size distribution of the powder includes: by mass percentage, 20 mesh: 1%, above 30 mesh: 20%, 30-60 mesh: 68%, 60-80 mesh: 8%, below 80 mesh: 3%.

[0057] (2) The formed green body is polished by a grinding machine and then dried in a drying kiln to obtain a green body with a certain strength. The drying kiln is a four-layer drying kiln with a length of 100M. The drying time can be 60min, and the moisture content of the green body after drying is controlled at 0.2wt%.

[0058] (3) Spray water to moisten the surface of the blank. Water spraying amount: 100g / m 2 , using two spray guns, nozzle size: 0.62mm.

[0059] (4) Apply the top glaze layer by bell jar glazing method. The process parameters of the top glaze are: glaze amount 580g / m 2 , specific gravity is 1.92g / ml, flow rate is 32 seconds. The chemical composition of the glaze includes, by mass percentage, loss on ignition: 5.0%, SiO2: 59%, Al2O3: 18%, Fe2O3: 0.1%, TiO2: 0.05%, CaO: 1.0%, MgO: 2.0%, K2O: 1.2%, Na2O: 4.65%, BaO: 5.0%, ZrO2: 4.0%, and the sum of the mass percentages of the chemical composition is 100%. The fineness requirement of the glaze is that the residue on the 325 mesh screen reaches 0.8wt%.

[0060] (5) After applying the top glaze layer, the surface of the blank is printed with a digital inkjet machine using metallic ink and new sinking function ink to print the cloisonné enamel pattern file. The color and texture of the design pattern can be appropriately adjusted according to the requirements of the metal flash and sinking effect.

[0061] (6) After the inkjet printing pattern, the surface of the brick blank is printed with digital glue using a glue dryer. The file for printing glue is a file with metallic glitter and sinking effect produced by printing the cloisonné pattern file using a digital inkjet machine. Through precise alignment, ensure that the position of the digital glue printing is completely consistent with the cloisonné pattern printed by the digital inkjet machine. The grayscale value of the digital glue printing is 100%, and the thermal decomposition temperature of the digital glue is 800°C.

[0062] (7) Gold-plated dry particles and golden flash dry particles are placed on the surface of the brick blank printed with digital glue, and the fan speed is controlled to 2000r / min. The dry particles not on the digital glue layer are sucked away by the fan to obtain a dry particle layer with a thickness of 3mm. The particle grading is 100-200 mesh: 89%, above 100 mesh: 7%, and below 200 mesh: 4%.

[0063] (The parameters for steps (5) to (7) are:

[0064]

[0065] (8) Spray transparent color glaze on the surface of the brick with Bugan particles:

[0066] Transparent color glaze formula: 3 parts of sodium feldspar, 40 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 10 parts of strontium carbonate, 6 parts of quartz, 11 parts of dolomite, 6 parts of calcite, 9 parts of burned talc, 3 parts of zinc oxide, and 1 part of zirconium silicate.

[0067] The process parameters for spraying transparent color glaze are: spraying glaze amount: 450g / m 2 , specific gravity is 1.50g / ml.

[0068] The specific spraying method is: mix the required raw materials evenly in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.6% (325 mesh sieve), age for 24 hours, control the specific gravity to 1.50, and use the glaze spraying process to apply the glaze to the surface of the brick with dry particles.

[0069] Two caliber spray guns are used to spray transparent color glaze: 0.52mm spray gun A and 0.62mm spray gun B. There are two groups of spray gun A and four groups of spray gun B. The installation order of the six groups of spray guns is: spray gun A→spray gun B→spray gun B→spray gun B→spray gun A. In order to avoid uneven local glaze spraying and large deviation of glaze spraying amount between the two sides and the middle position, the distance between spray gun A and spray gun B is 30cm, and the distance between spray gun B and spray gun B is 20cm. And with the middle position of the brick blank as the reference line, the six groups of spray guns are 5cm away from the reference line position respectively, and are arranged in sequence according to the reference line, one left and one right, which can effectively ensure that the glaze spraying amount on both sides of the brick blank is close to that in the middle position. The height of the nozzle and the surface of the brick blank is 80cm, the spray gun is inclined at a 45-degree angle to the surface of the brick blank, the gun mouth is tilted backward, and the spray gun is perpendicular to the brick surface. Spraying transparent color glaze is easy to blow away the dry particles. When spraying transparent colored glaze, the pressure of the high-pressure glaze spraying machine is set to 4.5 MPa.

[0070] (9) The bricks sprayed with transparent color glaze are dried in the pre-kiln drying kiln and then fired in the kiln at a temperature of 1160°C for 50 minutes. After firing, the tiles with cloisonné enamel effect are obtained. The glossiness and dirt absorption are measured, and the glaze surface and the cloisonné enamel effect are observed.

[0071] Example 3

[0072] The present embodiment of a building ceramic tile with cloisonné enamel effect comprises, from bottom to top, a body layer, a glaze layer, a pattern layer, a glue layer, a dry particle layer, and a transparent coloring glaze layer. The specific preparation method is:

[0073] (1) The green body is obtained by pressing. The chemical composition of the green body powder includes: by mass percentage, ignition loss: 4.6%, SiO2: 70%, Al2O3: 19.2%, Fe2O3: 0.3%, TiO2: 0.1%, CaO: 0.3%, MgO: 0.5%, K2O: 3.0%, Na2O: 2.0%. The particle size distribution of the powder includes: by mass percentage, 20 mesh: 0.6%, above 30 mesh: 18%, 30-60 mesh: 72%, 60-80 mesh: 7%, below 80 mesh: 2.4%.

[0074] (2) The formed green body is polished by a grinding machine and then dried in a drying kiln to obtain a green body with a certain strength. The drying kiln is a four-layer drying kiln with a length of 100M. The drying time can be 50min, and the moisture content of the green body after drying is controlled at 0.3wt%.

[0075] (3) Spray water to moisten the surface of the blank. Water spraying amount: 90g / m 2 , using two spray guns, nozzle size: 0.60mm.

[0076] (4) Apply the top glaze layer by bell jar glazing method. The process parameters of the top glaze are: glaze amount 550g / m 2 , specific gravity is 1.89g / ml, flow rate is 29 seconds. The chemical composition of the glaze includes, by mass percentage, loss on ignition: 3.0%, SiO2: 60%, Al2O3: 20%, Fe2O3: 0.12%, TiO2: 0.04%, CaO: 0.5%, MgO: 1.2%, K2O: 0.9%, Na2O: 4.24%, BaO: 5.5%, ZrO2: 4.5%, the sum of the mass percentages of the chemical composition is 100%. The fineness requirement of the glaze is that the residue on the sieve of the 325 mesh screen reaches 0.7wt%.

[0077] (5) After applying the top glaze layer, the surface of the blank is printed with a digital inkjet machine using metallic ink and new sinking function ink to print the cloisonné enamel pattern file. The color and texture of the design pattern can be appropriately adjusted according to the requirements of the metal flash and sinking effect.

[0078] (6) After the inkjet printing pattern, the surface of the brick blank is printed with digital glue using a glue dryer. The file for printing the glue is a file with metallic glitter and sinking effect produced by printing the cloisonné pattern file using a digital inkjet machine. Through precise alignment, ensure that the position of the digital glue printing is completely consistent with the cloisonné pattern printed by the digital inkjet machine. The grayscale value of the digital glue printing is 60%, and the thermal decomposition temperature of the digital glue is 700°C.

[0079] (7) Gold-plated dry particles and golden flash dry particles are placed on the surface of the brick blank printed with digital glue, and the fan speed is controlled to 1800r / min. The dry particles not on the digital glue layer are sucked away by the fan to obtain a dry particle layer with a thickness of 2mm. The particle grading is 100-200 mesh: 90%, above 100 mesh: 8%, below 200 mesh: 2%.

[0080] The parameters of steps (5) to (7) are:

[0081]

[0082] (8) Spray transparent color glaze on the surface of the brick with Bugan particles:

[0083] Transparent color glaze formula: 7 parts of sodium feldspar, 36 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 10 parts of strontium carbonate, 8 parts of quartz, 9 parts of dolomite, 5 parts of calcite, 8 parts of burnt talc, 5 parts of zinc oxide, and 1 part of zirconium silicate.

[0084] The process parameters for spraying transparent color glaze are: spraying glaze amount: 400g / m 2 , specific gravity is 1.45g / ml.

[0085] The specific spraying method is: mix the required raw materials evenly in proportion, put them into a ball mill, add 38% water, 0.13% carboxymethyl cellulose, and 0.3% sodium tripolyphosphate, control the ball fineness to 0.5% (325 mesh sieve), age for 20 hours, control the specific gravity to 1.45, and use the glaze spraying process to apply the glaze to the surface of the brick with dry particles.

[0086] Two caliber spray guns are used to spray transparent color glaze: 0.52mm spray gun A and 0.62mm spray gun B. There are two groups of spray gun A and four groups of spray gun B. The installation order of the six groups of spray guns is: spray gun A→spray gun B→spray gun B→spray gun B→spray gun A. In order to avoid uneven local glaze spraying and large deviation of glaze spraying amount between the two sides and the middle position, the distance between spray gun A and spray gun B is 30cm, and the distance between spray gun B and spray gun B is 20cm. And with the middle position of the brick blank as the reference line, the six groups of spray guns are 5cm away from the reference line position respectively, and are arranged in sequence according to the reference line, one left and one right, which can effectively ensure that the glaze spraying amount on both sides of the brick blank is close to that in the middle position. The height of the nozzle and the surface of the brick blank is 80cm, the spray gun is inclined at a 45-degree angle to the surface of the brick blank, the gun mouth is tilted backward, and the spray gun is perpendicular to the brick surface. Spraying transparent color glaze is easy to blow away the dry particles. When spraying transparent colored glaze, the pressure of the high-pressure glaze spraying machine is set to 4 MPa.

[0087] (9) After spraying transparent color glaze, the brick blank is dried in the pre-kiln drying kiln and then fired in the kiln. The firing temperature is 1150℃ and the firing time is 45 minutes. After firing, the tile with cloisonné effect on the surface is obtained. The glossiness and dirt absorption are measured, and the glaze surface and the cloisonné effect are observed visually.

[0088] Example 4

[0089] The parameters of steps (5) to (7) are:

[0090]

[0091] The formula of transparent coloring glaze is: 10 parts of albite, 33 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 12 parts of strontium carbonate, 6 parts of quartz, 9 parts of dolomite, 8 parts of calcite, 8 parts of burned talc, 2 parts of zinc oxide, and 1 part of zirconium silicate.

[0092] Other raw materials and preparation methods are the same as those in Example 1.

[0093] Example 5

[0094] The parameters of steps (5) to (7) are:

[0095]

[0096] Other raw materials and preparation methods are the same as those in Example 1.

[0097] Example 6

[0098] The parameters of steps (5) to (7) are:

[0099]

[0100] Other raw materials and preparation methods are the same as those in Example 1.

[0101] Example 7

[0102] The parameters of steps (5) to (7) are:

[0103]

[0104] Other raw materials and preparation methods are the same as those in Example 1.

[0105] Example 8

[0106] The parameters of steps (5) to (7) are:

[0107]

[0108] Other raw materials and preparation methods are the same as those in Example 1.

[0109] Comparative Example 1

[0110] The parameters of steps (5) to (7) are:

[0111]

[0112] Other raw materials and preparation methods are the same as those in Example 1.

[0113] Comparative Example 2

[0114] The parameters of steps (5) to (7) are:

[0115]

[0116] Other raw materials and preparation methods are the same as those in Example 1.

[0117] Comparative Example 3

[0118] The parameters of steps (5) to (7) are:

[0119]

[0120] Other raw materials and preparation methods are the same as those in Example 1.

[0121] Comparative Example 4

[0122] The parameters of steps (5) to (7) are:

[0123]

[0124] Other raw materials and preparation methods are the same as those in Example 1.

[0125] The properties of the tiles prepared in Examples 1-8 and Comparative Examples 1-4 were tested, and the results are shown in Table 1.

[0126] Test methods and instruments used:

[0127] Antifouling performance: According to the antifouling performance determination method in GB / T3810.14-2015 ceramic tile test method, three types of oily inks, black, red and blue, were applied to the tile surface for testing.

[0128] Water absorption rate: According to the water absorption rate determination method in GB / T3810.3-2015 ceramic tile test method, the TZY-3 digital ceramic water absorption rate tester produced by Tianjin Yougong Testing Equipment Co., Ltd. is used for testing.

[0129] Wear resistance: According to the wear resistance determination method of glazed tiles in GB / T3810.7-2015 ceramic tile test method, the tile wear resistance tester produced by Shenzhen Opuri Testing Equipment Co., Ltd. was used for testing.

[0130] Gloss: According to the gloss measurement method in GB / T13891-2015 ceramic tile test method, the MN60 gloss meter produced by Shanghai Liangyan Intelligent Technology Co., Ltd. was used for testing.

[0131] The product excellence rate is tested according to enterprise standard requirements. Generally, enterprise standard requirements for ceramic products are higher than industry standards, and industry standards are higher than national standards.

[0132] Table 1 Performance of each tile

[0133]

[0134]

[0135]

[0136] The table shows that the antifouling performance of the tile prepared by the present invention reaches grade A, the wear resistance reaches grade 5, the water absorption rate is qualified, and the surface has a metal wire texture effect and an enamel color effect. By comparing Example 1 with each comparative example, it can be seen that the combination of gold-plated dry particles, golden flash dry particles and metal ink can achieve a unique metal texture effect on the brick surface, and the new sinking functional ink and colored dry particles matching the enamel effect pattern can achieve a thick and gorgeous enamel color effect.

[0137] Comparative Example 5

[0138] The formula of the transparent color glaze in this comparative example is: 12 parts of albite, 20 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 13 parts of strontium carbonate, 25 parts of quartz, 8 parts of dolomite, 14 parts of calcite, 8 parts of burned talc, 8 parts of zinc oxide, and 1 part of zirconium silicate.

[0139] Other raw materials and preparation methods are the same as those in Example 1.

[0140] Comparative Example 6

[0141] The formula of the transparent color glaze in this comparative example is: 22 parts of albite, 17 parts of potassium feldspar, 8 parts of kaolin, 3 parts of calcined kaolin, 3 parts of strontium carbonate, 20 parts of quartz, 5 parts of dolomite, 13 parts of calcite, 9 parts of burned talc, 9 parts of zinc oxide, and 1 part of zirconium silicate.

[0142] Other raw materials and preparation methods are the same as those in Example 1.

[0143] The properties of the tiles prepared in Example 1 and Comparative Examples 5-6 were tested, and the results are shown in Table 2.

[0144] Table 2 Performance of each tile

[0145]

[0146]

[0147] The data comparison in the table shows that the transparent color glaze formula of the present invention can achieve a cloisonné enamel effect on the surface of the tile. Increasing the quartz content in the formula helps the color to turn blue, and adjusting the ratio of strontium carbonate, dolomite, calcite, talc and zinc oxide at the same time can achieve the purpose of ensuring stable glaze color and excellent anti-fouling performance.

[0148] In summary, the present invention utilizes a digital glue dry granulator to position dry granules with different effects, and uses metal ink and sinking ink to achieve the purpose of enriching patterns and metal effects through inkjet printing. Among them, gold-plated dry granules, golden flash dry granules and metal ink are used in combination to achieve a unique metal texture effect on the brick surface; a new type of sinking functional ink is developed and colored dry granules are used to match the enamel effect pattern to achieve a thick and gorgeous enamel color effect; a digital glue dry granulator is used to position dry granules with different effects, combined with unique effect dry granule crystallization technology and new sinking functional ink technology, to achieve a cloisonné enamel effect on the surface of building ceramic tiles. At the same time, the present invention adopts golden dry particles with iron chrome brown and titanium yellow as crystal seeds and digital glue dry particle machine positioning technology combined with digital inkjet printing technology, so that the digital glue printing and the design pattern file are accurately overlapped, and the golden dry particles are applied and bonded with the digital glue to achieve accurate overlap with the design pattern texture; the colored dry particles with cobalt oxide, copper oxide, titanium dioxide, etc. as the main raw materials and the digital glue dry particle machine positioning technology combined with digital inkjet printing technology are used to make the digital glue printing and the design pattern file accurately overlap, and the colored dry particles are applied and bonded with the digital glue to achieve accurate overlap with the design pattern texture. In addition, the present invention has developed a transparent color glaze formula that can make the surface of the tile achieve a cloisonné enamel effect. Increasing the quartz content in the formula helps the color to turn blue, and at the same time adjusting the ratio of strontium carbonate, dolomite, calcite, burnt talc and zinc oxide, so as to achieve the purpose of ensuring the glaze color stability and excellent anti-fouling performance.

[0149] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A building ceramic tile with cloisonné enamel effect, It is characterized in that The architectural ceramic tile with cloisonné enamel effect comprises, from bottom to top, a body layer, a glaze layer, a pattern layer, a glue layer, a dry particle layer, and a transparent color-generating glaze layer; The pattern layer is a cloisonné enamel pattern file printed on the glaze layer using a digital inkjet machine using metallic ink and a new type of sinking functional ink; The glue layer is made by printing digital glue on the surface of the blank layer after the inkjet printing pattern with a glue dryer. The file for printing the glue is a file with metallic glitter and sinking effect produced by printing the cloisonné pattern file with a digital inkjet machine. Through precise alignment, it is ensured that the position of the digital glue printing is completely consistent with the cloisonné pattern printed by the digital inkjet machine. The dry particle layer is coated with golden dry particles and / or colored dry particles.

2. The architectural ceramic tile with cloisonné effect according to claim 1, It is characterized in that The chemical composition of the green body powder on the green body layer includes: in terms of mass percentage, loss on ignition: 3.8-4.6%, SiO 2 :65-70%、Al 2 O 3 :18-22%,Fe 2 O 3 :0.3-0.8%, TiO 2 :0.1-0.2%, CaO: 0.3-0.8%, MgO: 0.5-1.0%, K 2 O:3.0-4.0% and Na 2 O: 2.0-3.0%; the particle gradation of the green body powder includes: in terms of mass percentage, 20 mesh: ≦1%, above 30 mesh: 10-20%, 30-60 mesh: 65-75%, 60-80 mesh: ≦12%, below 80 mesh: ≦6%.

3. The architectural ceramic tile with cloisonné effect according to claim 1, It is characterized in that The chemical composition of the glaze on the surface glaze layer includes: in terms of mass percentage, loss on ignition: 2.0-5.0%, SiO 2 :55-65%、Al 2 O 3 :18-21%,Fe 2 O 3 :0.1-0.2%, TiO 2 :0.03-0.05%, CaO: 0.5-1.0%, MgO: 1.0-2.0%, K 2 O: 0.8-1.2%, Na 2 O:4.0-5.0%, BaO:5.0-6.0%, ZrO 2 :4.0-5.0%, the sum of the mass percentages of the chemical components is 100%; the fineness requirement of the glaze is that the residue on the sieve of the 325-mesh sieve reaches 0.5-0.8wt%.

4. The architectural ceramic tile with cloisonné effect according to claim 1, It is characterized in that The particle gradation of the dry particle layer includes: in terms of mass percentage, 85%-90% of 100-200 meshes, 5%-10% of those above 100 meshes, and less than 5% of those below 200 meshes.

5. The architectural ceramic tile with cloisonné effect according to claim 1, It is characterized in that The formula of the transparent color glaze is: a part of sodium feldspar (0≤a≤43), b parts of potassium feldspar (a+b=43), 8 parts of kaolin, 3 parts of calcined kaolin, c parts of strontium carbonate (6≤c≤12), d parts of quartz (6≤d≤20), e parts of dolomite (8≤e≤12), f parts of calcite (3≤f≤10), g parts of talc (4≤g≤12), h parts of zinc oxide (2≤h≤6), and 1 part of zirconium silicate, wherein c+d+e+f+g+h=45.

6. A method for preparing a building ceramic tile with cloisonné effect as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: (1) making a green body, which is polished and dried to obtain a green body with a certain strength; (2) spraying water to moisten the surface of the blank and applying a glaze layer; (3) using a digital inkjet printer to print a cloisonné enamel pattern file on the surface of the blank after the top glaze layer is applied; (4) using a glue dryer to print digital glue on the surface of the brick blank after the cloisonné enamel pattern is printed by inkjet printing; (5) Gold-plated dry particles and golden glitter dry particles are applied to the surface of the brick blank printed with digital glue; (6) spraying transparent coloring glaze on the surface of the brick with Bugan particles; (7) Dry and fire the bricks sprayed with transparent colored glaze to obtain tiles with cloisonné enamel effect on the surface.

7. A method for preparing a building ceramic tile with cloisonné effect according to claim 6, It is characterized in that In step (1), the drying is carried out in a drying kiln, which is a four-layer drying kiln with a length of 100M. The drying time is 40-60min, and the moisture content of the green body after drying is controlled to be 0.2-0.4wt%.

8. The method for preparing a building ceramic tile with cloisonné effect according to claim 6, It is characterized in that In step (2), the water spraying is carried out using two spray guns with nozzle sizes of 0.52-0.62 mm, and the water spraying amount is 60-100 g / m 2 The process parameters of the glaze layer are: the glaze amount is 480-580g / m 2 , specific gravity is 1.82-1.92g / ml, and flow rate is 26-32 seconds.

9. The method for preparing a building ceramic tile with cloisonné effect according to claim 6, It is characterized in that In step (4), the grayscale value of the digital glue printing is 10-100%, and the thermal decomposition temperature of the digital glue is 600-800°C.

10. The method for preparing a building ceramic tile with cloisonné effect according to claim 6, It is characterized in that In step (6), the process parameters for spraying the transparent color glaze are: spraying amount: 350-450g / m 2 , specific gravity is 1.40-1.50g / ml; two caliber spray guns are used for spraying transparent colored glaze: 0.52mm spray gun A and 0.62mm spray gun B; among them, spray gun A is divided into two groups, and spray gun B is divided into four groups; the installation order of the six groups of spray guns is: spray gun A→spray gun B→spray gun B→spray gun B→spray gun A; the distance between spray gun A and spray gun B is 30cm, and the distance between spray gun B and spray gun B is 20cm, and the middle position of the brick is taken as the reference line, and the six groups of spray guns are 5cm away from the reference line respectively, and are arranged in sequence one left and one right according to the reference line; the height between the nozzle and the surface of the brick is 80-90cm, and the spray gun is inclined at a 45-degree angle to the surface of the brick; when spraying transparent colored glaze, the pressure of the high-pressure glaze spraying machine is set to 4-4.5mpa.