Carbon fiber composite material for notebook computer shell and preparation process of carbon fiber composite material
A carbon fiber composite material for laptop shells, with a coated epoxy resin and resin layer thickness gradient, addresses the brittleness issue, enhancing impact resistance and mechanical strength.
Patent Information
- Application Number
- CN202411224342.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-03
AI Technical Summary
Carbon fiber composite materials used in laptop shells made with thermosetting resin have brittle surfaces that are prone to breaking upon impact.
A carbon fiber composite material is developed with a carbon fiber layer coated with an epoxy resin composition and a resin layer comprising PC, ABS, PMMA, or PET on both surfaces, featuring a thickness gradient, and a preparation process involving precuring and molding under specific conditions to enhance impact resistance.
The composite material exhibits improved impact resistance, mechanical strength, and heat dissipation, reducing the likelihood of shell damage from drops.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon fiber composite materials, in particular to a carbon fiber composite material for a notebook computer shell and a preparation process thereof. Background Art
[0002] Carbon fiber composite materials have many advantages such as high strength, high modulus, low specific gravity, low expansion coefficient, corrosion resistance, etc. They not only have the high strength and firmness of aluminum-magnesium alloys, but also have the plasticity of engineering plastics, making their comprehensive performance excellent. Carbon fiber composite materials used in laptop shells are mainly divided into four types, short carbon fiber reinforced composite materials, thermosetting continuous carbon fiber composite materials, thermoplastic continuous carbon fiber composite materials and carbon fiber composite films. Among them, the molding process of thermosetting continuous carbon fiber composite materials is to impregnate the carbon fiber cloth with resin and then lay the cloth flat in the mold, heat it to cure the thermosetting resin and form it, and prepare the laptop shell. The commonly used thermosetting resin is epoxy resin, and the surface of the laptop shell made of it is brittle and easy to break when it falls. Therefore, we propose a carbon fiber composite material for laptop shells and its preparation process. Summary of the invention
[0003] The object of the present invention is to provide a carbon fiber composite material for a notebook computer shell and a preparation process thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: A carbon fiber composite material for a laptop computer shell, comprising a carbon fiber layer and a resin layer; the resin layer is arranged on the upper surface and the lower surface of the carbon fiber layer;
[0005] The carbon fiber layer is obtained by coating one or more layers of carbon fiber cloth with an epoxy resin composition and curing the resulting layer.
[0006] Furthermore, the material of the resin layer is a mixture of one or more of PC (polycarbonate), ABS (acrylonitrile-butadiene-styrene copolymer), PMMA (polymethyl methacrylate), PET (polyethylene terephthalate), and PU (polyurethane).
[0007] Furthermore, the thickness of the carbon fiber cloth is 0.11-0.39 mm, and the weight is 110-360 g / m 2 .
[0008] Furthermore, the thickness of the resin layer decreases stepwise from the outside to the inside, with an average thickness of 0.15 to 0.20 mm;
[0009] The middle of the resin layer is the key area, with a thickness of 0.10 to 0.25 mm;
[0010] The outer thickness of the resin layer is 0.20 to 0.36 mm.
[0011] Furthermore, the thickness of the carbon fiber composite material is 1.2 to 4.4 mm.
[0012] A preparation process of a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0013] Taking carbon fiber cloth and laying it flat in a mold, coating it with an epoxy resin composition, and precuring it to form a precured carbon fiber layer;
[0014] The polyurethane resin is sequentially injected onto the upper surface and the lower surface of the pre-cured carbon fiber layer to form a resin layer; and the carbon fiber layer is formed by molding to obtain a carbon fiber composite material.
[0015] Furthermore, before coating the epoxy resin composition, the carbon fiber cloth is heated to 90-130° C.;
[0016] After coating, the epoxy resin composition is cast to impregnate the carbon fiber cloth;
[0017] The pre-curing process conditions are: temperature 90-100°C, time 30-60 minutes.
[0018] Furthermore, the molding process conditions are: molding temperature 95-120° C., molding time 80-100 min, and molding pressure 0.5-1.2 MPa.
[0019] Further, the epoxy resin composition includes the following components by mass: 12 to 18 parts of modified epoxy resin and 2 to 6 parts of curing agent;
[0020] The curing agent is one of diethylaminopropylamine and diethyltoluenediamine;
[0021] The mass ratio of the epoxy resin composition to the carbon fiber is (30-46):100.
[0022] In the above technical solution, the carbon fiber cloth is coated and impregnated with an epoxy resin composition made of epoxy resin and curing agent to form a carbon fiber layer, which has the advantages of light weight, high strength, fast heat dissipation, and good shielding effect. A resin layer with high toughness is arranged on the upper and lower surfaces of the carbon fiber layer, which helps to improve the impact resistance of the prepared carbon fiber composite material. In the plane direction, the thickness of the outer circle of the resin layer is relatively high, which helps to prevent the corners of the prepared laptop shell from being crushed when it falls.
[0023] Further, the modified epoxy resin is prepared by the following process:
[0024] S1. Heat the diisocyanate to 80-85°C, slowly add the polyglycol, and react for 100-150 minutes; wash and dry to obtain a long-chain diisocyanate;
[0025] S2, mixing long-chain diisocyanate and hydroxyethyl acrylate, heating to 85-90°C, reacting for 150-200 minutes; washing, drying, and obtaining unsaturated isocyanate;
[0026] S3, mixing unsaturated isocyanate and epoxy resin, heating to 85-90° C., and reacting for 5-6 hours to obtain unsaturated epoxy resin;
[0027] S4. Dissolve the monomer and initiator in acetone, add unsaturated epoxy resin and mix, remove the acetone by vacuum distillation; place in a rheometer, mix and react at 172-178° C. for 6-8 minutes to obtain a modified epoxy resin.
[0028] Further, in S1, the diisocyanate is one of isophorone diisocyanate, toluene diisocyanate, 1,6-hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, meta-xylylene diisocyanate, tetramethyl dimethylene diisocyanate, dodecylbenzene-2,4-diisocyanate, 4,4-diisocyanate dicyclohexylmethane, 1,4-cyclohexane dimethyl diisocyanate, and 1,6-diisocyanate-2,2,4-trimethylhexane;
[0029] The polyglycol is a mixture of one or more of polyethylene glycol, polypropylene glycol, hydroxyl-terminated polydimethylsiloxane, polytetramethylene glycol, and polycarbonate glycol;
[0030] The -NCO / -OH ratio of diisocyanate and polydiol is 2:1.
[0031] Furthermore, in S2, the -NCO / -OH ratio of the long-chain diisocyanate and hydroxyethyl acrylate is 2:1.
[0032] Furthermore, in S3, the -NCO / -OH ratio of the unsaturated isocyanate and the epoxy resin is 1:1.
[0033] Further, in S4, the monomers include: by mass, 10 parts of polybutadiene, 4 to 6 parts of styrene, and 1.5 to 4.4 parts of acrylonitrile;
[0034] The initiator is dicumyl peroxide (DCP);
[0035] The mass ratio of unsaturated epoxy resin, monomer and initiator is 100:(9-15):(0.15-0.25);
[0036] The ratio of monomer to acetone is 10 g / 10 mL;
[0037] The rheological rotor speed is 40-50 rpm.
[0038] In the above technical scheme, the epoxy resin is modified, specifically: diisocyanate is reacted with polydiol and hydroxyethyl acrylate in sequence to prepare an isocyanate compound containing allyl group, which is recorded as unsaturated isocyanate; then the isocyanate in its molecular chain reacts with the hydroxyl group in the epoxy resin to obtain an epoxy resin with unsaturated bonds, which is recorded as unsaturated epoxy resin; finally, the obtained unsaturated epoxy resin is co-extruded with polybutadiene, styrene and acrylonitrile under the action of an initiator to form a composite epoxy resin with an ABS copolymer molecular structure, so that the toughness, processing performance and electrical properties of the prepared modified epoxy resin are effectively improved, and the impact resistance of the carbon fiber composite material is improved. At the same time, the modified epoxy resin has a higher bonding ability with the carbon fiber cloth and is less likely to be peeled off, which helps to further improve the mechanical properties of the carbon fiber composite material.
[0039] Further, the polyurethane resin is prepared by the following process:
[0040] Mix 1,6-hexamethylene diisocyanate and polycarbonate diol, stir for 30 minutes in a nitrogen atmosphere; heat to 70-75°C, stir and react for 90-120 minutes; add hydroxyl-terminated polybutadiene, and continue to react for 120-150 minutes to obtain a prepolymer;
[0041] Add hydroxyethyl acrylate, chain extender and catalyst, raise the temperature to 80-85°C, react for 30-60 minutes to obtain polyurethane;
[0042] The polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and an initiator are mixed, extruded in a twin-screw extruder, granulated and dried to obtain a polyurethane resin.
[0043] Further, the polyurethane resin is prepared from the following components by mass: 17.6-23.9 parts of 1,6-hexamethylene diisocyanate, 13-18 parts of hydroxy-terminated polybutadiene, 10-20 parts of polycarbonate diol, 1-2 parts of hydroxyethyl acrylate, 7.2-9.0 parts of chain extender; 3-5 parts of acrylonitrile, 1-2 parts of styrene, 2.4-3.0 parts of dodecafluoroheptyl methacrylate;
[0044] Further, the chain extender is one of methyl propylene glycol, 2,3-butanediol, 1,4-butanediol, and ethylene glycol;
[0045] The catalyst is dibutyltin dilaurate, and the amount used is 0.13-0.17wt% of the total mass of the polyurethane material system;
[0046] The initiator is dicumyl peroxide, and the dosage is 0.5-1.0wt% of the total weight of the polyurethane resin material system.
[0047] In the extrusion process, the extrusion temperature is 185-235°C, and the twin-screw speed is 100-120r / min.
[0048] In the above technical scheme, a prepolymerization method is adopted to react diisocyanate with diol under the action of a catalyst to obtain a polyurethane prepolymer, whose polymerization degree is closer and the molecular arrangement tends to be orderly, and then a chain extender is added to synthesize polyurethane, thereby obtaining a polyurethane with a more regular and orderly molecular structure. The diol is a polycarbonate diol and a terminal hydroxyl polybutadiene, which helps the polyurethane resin to have better heat resistance, impact resistance, wear resistance, mechanical properties and processing properties.
[0049] Hydroxyethyl acrylate is added in the later stage of the polyurethane prepolymerization reaction to introduce an allyl double bond, so that the prepared polyurethane is co-extruded with acrylonitrile, styrene, and dodecafluoroheptyl methacrylate, which further improves the corrosion resistance and heat resistance of the polyurethane, increases the water contact angle of the resin layer, and improves the water resistance, thereby preparing a polyurethane resin with higher strength and heat resistance and a resin layer prepared therefrom; and the resin layer has a partial molecular chain structure similar to that of the carbon fiber layer, which improves the bonding strength between the two, improves the strength and toughness of the prepared carbon fiber composite material, and alleviates the drop breakage phenomenon.
[0050] Compared with the prior art, the present invention has the following beneficial effects:
[0051] The present invention describes a carbon fiber composite material for a laptop shell and its preparation process. The carbon fiber cloth is coated and impregnated with an epoxy resin composition prepared by epoxy resin and curing agent to form a carbon fiber layer, which has the advantages of light weight, high strength, fast heat dissipation, good shielding effect, etc. A resin layer with high toughness is arranged on the upper and lower surfaces of the carbon fiber layer, which helps to improve the impact resistance of the prepared carbon fiber composite material. DETAILED DESCRIPTION
[0052] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] In the following specific implementations,
[0054] Carbon fiber cloth: CO6644B, thickness 0.3mm, weight 317g / m2, from Toray Corporation of Japan;
[0055] The thickness of the resin layer decreases stepwise from the outside to the inside. The thickness of the key area is 0.10mm; the thickness of the outer periphery of the resin layer is 0.20mm.
[0056] Polyethylene glycol: average number average molecular weight 2000, from Sigma-Aldrich Shanghai Trading Co., Ltd.;
[0057] Polytetrahydrofuran diol: average number average molecular weight 2000, from Sigma-Aldrich Shanghai Trading Co., Ltd.;
[0058] Hydroxyl-terminated polydimethylsiloxane: average number average molecular weight 550, from Sigma-Aldrich Shanghai Trading Co., Ltd.;
[0059] Epoxy resin: EL127, from Nan Ya Plastics Industrial Co., Ltd.;
[0060] Polybutadiene: B-1000, from Nippon Soda Co., Ltd.;
[0061] Hydroxyl-terminated polybutadiene: JP-200, from Nippon Soda Co., Ltd.;
[0062] Polycarbonate diol: SYHP1000, from Shanghai Shuyu Chemical Co., Ltd.;
[0063] The following “parts” are all parts by mass.
[0064] Embodiment 1: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following process:
[0065] Step 1: preparing epoxy resin composition:
[0066] S1. Heat isophorone diisocyanate to 80°C, slowly add polyethylene glycol, and react for 150 minutes; wash and dry to obtain a long-chain diisocyanate; the -NCO / -OH ratio of isophorone diisocyanate and polyethylene glycol is 2:1;
[0067] S2, mixing long-chain diisocyanate and hydroxyethyl acrylate, heating to 85°C, reacting for 200 minutes; washing, drying, and obtaining unsaturated isocyanate; the -NCO / -OH ratio of the long-chain diisocyanate and hydroxyethyl acrylate is 2:1;
[0068] S3, mixing unsaturated isocyanate and epoxy resin, heating to 85°C, and reacting for 6 hours to obtain unsaturated epoxy resin; the -NCO / -OH ratio of unsaturated isocyanate and epoxy resin is 1:1;
[0069] S4, dissolving the monomer and initiator dicumyl peroxide in acetone, adding unsaturated epoxy resin and mixing, removing acetone by vacuum distillation; placing in a rheometer, mixing and reacting at 172°C for 8 minutes, with the rheological rotor speed at 40 rpm, to obtain a modified epoxy resin; the monomer includes 10 parts of polybutadiene, 4 parts of styrene, and 1.5 parts of acrylonitrile; the ratio of monomer to acetone is 10g / 10mL; the mass ratio of unsaturated epoxy resin, monomer, and initiator is 100:9:0.15;
[0070] S5, mixing 12 parts of modified epoxy resin and 4 parts of curing agent diethylaminopropylamine to obtain an epoxy resin composition;
[0071] Step 2: preparing polyurethane resin:
[0072] Mix 1,6-hexamethylene diisocyanate and polycarbonate diol, stir for 30 minutes in a nitrogen atmosphere; heat to 70°C, stir and react for 120 minutes; add terminal hydroxyl polybutadiene, continue to react for 150 minutes to obtain a prepolymer; add hydroxyethyl acrylate, hydroxyethyl acrylate, chain extender methyl propylene glycol, 0.13wt% catalyst dibutyltin dilaurate, heat to 80°C, react for 60 minutes to obtain a polyurethane;
[0073] The polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and 0.5wt% initiator dicumyl peroxide are mixed, extruded in a twin-screw extruder, the extrusion temperature is 185-235°C, and the twin-screw speed is 100r / min; granulated, dried, to obtain a polyurethane resin; the polyurethane resin is prepared from the following components by weight: 17.6 parts of 1,6-hexamethylene diisocyanate, 13 parts of hydroxyl-terminated polybutadiene, 10 parts of polycarbonate diol, 1 part of hydroxyethyl acrylate, 7.2 parts of a chain extender; 3 parts of acrylonitrile, 1 part of styrene, 2.4 parts of dodecafluoroheptyl methacrylate;
[0074] Step 3: Preparation of carbon fiber composite material:
[0075] Take the carbon fiber cloth and lay it flat in the mold, heat it to 90°C, apply the 90°C epoxy resin composition on the surface of the carbon fiber, cast it, and impregnate the carbon fiber cloth. Repeat the above operation 3 times; pre-curing to form a pre-cured carbon fiber layer. The pre-curing process conditions are: temperature 90°C, time 60min; the mass ratio of epoxy resin to carbon fiber is 30:100;
[0076] The polyurethane resin is sequentially injected onto the upper surface and the lower surface of the pre-cured carbon fiber layer to form a resin layer; and the molding process conditions are as follows: molding temperature 95°C, molding time 100min, and molding pressure 0.5MPa to form a carbon fiber layer and obtain a carbon fiber composite material.
[0077] Embodiment 2: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following process:
[0078] Step 1: preparing epoxy resin composition:
[0079] S1. Hexamethylene diisocyanate is heated to 82°C, polytetrahydrofuran diol is slowly added, and the reaction is carried out for 120 minutes; the mixture is washed and dried to obtain a long-chain diisocyanate; the -NCO / -OH ratio of hexamethylene diisocyanate and polytetrahydrofuran diol is 2:1;
[0080] S2, mixing long-chain diisocyanate and hydroxyethyl acrylate, heating to 88°C, reacting for 180 minutes; washing, drying, and obtaining unsaturated isocyanate; the -NCO / -OH ratio of the long-chain diisocyanate and hydroxyethyl acrylate is 2:1;
[0081] S3, mixing unsaturated isocyanate and epoxy resin, heating to 88°C, and reacting for 5.5h to obtain unsaturated epoxy resin; the -NCO / -OH ratio of unsaturated isocyanate and epoxy resin is 1:1;
[0082] S4, dissolving the monomer and initiator dicumyl peroxide in acetone, adding unsaturated epoxy resin and mixing, removing acetone by vacuum distillation; placing in a rheometer, mixing and reacting at 175°C for 7 minutes, with the rheological rotor speed at 45 rpm, to obtain a modified epoxy resin; the monomer includes 10 parts of polybutadiene, 5 parts of styrene, and 3 parts of acrylonitrile; the ratio of monomer to acetone is 10 g / 10 mL; the mass ratio of unsaturated epoxy resin, monomer, and initiator is 100:12:0.20;
[0083] S5, mixing 15 parts of modified epoxy resin and 4 parts of curing agent diethyltoluenediamine to obtain an epoxy resin composition;
[0084] Step 2: preparing polyurethane resin:
[0085] 1,6-hexamethylene diisocyanate and polycarbonate diol were mixed and stirred for 30 minutes in a nitrogen atmosphere; heated to 72°C and stirred for 105 minutes; hydroxy-terminated polybutadiene was added and the reaction was continued for 135 minutes to obtain a prepolymer; hydroxyethyl acrylate, chain extender 2,3-butanediol, and 0.15wt% catalyst dibutyltin dilaurate were added, the temperature was raised to 82°C, and the reaction was carried out for 45 minutes to obtain a polyurethane; polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and 0.8 wt% initiator dicumyl peroxide is mixed, extruded in a twin-screw extruder, the extrusion temperature is 185-235°C, and the twin-screw speed is 110r / min; granulated, dried, to obtain a polyurethane resin; the polyurethane resin is prepared from the following components by weight: 20.8 parts of 1,6-hexamethylene diisocyanate, 15.5 parts of terminal hydroxyl polybutadiene, 15 parts of polycarbonate diol, 1.5 parts of hydroxyethyl acrylate, 8.1 parts of a chain extender; 4 parts of acrylonitrile, 1.5 parts of styrene, and 2.7 parts of dodecafluoroheptyl methacrylate;
[0086] Step 3: Preparation of carbon fiber composite material:
[0087] Take the carbon fiber cloth and lay it flat in the mold, heat it to 110°C, apply the 90°C epoxy resin composition on the surface of the carbon fiber, cast it, and impregnate the carbon fiber cloth. Repeat the above operation 3 times; pre-cure to form a pre-cured carbon fiber layer. The pre-curing process conditions are: temperature 95°C, time 45min; the mass ratio of epoxy resin to carbon fiber is 38:100;
[0088] The polyurethane resin is sequentially injected onto the upper surface and the lower surface of the pre-cured carbon fiber layer to form a resin layer; and the molding is performed under the following process conditions: a molding temperature of 110°C, a molding time of 90 minutes, and a molding pressure of 0.8 MPa to form a carbon fiber layer and obtain a carbon fiber composite material.
[0089] Embodiment 3: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following process:
[0090] Step 1: preparing epoxy resin composition:
[0091] S1. Heat 1,4-cyclohexanedimethyl diisocyanate to 85°C, slowly add hydroxyl-terminated polydimethylsiloxane, and react for 100 minutes; wash and dry to obtain a long-chain diisocyanate; the -NCO / -OH ratio of 1,4-cyclohexanedimethyl diisocyanate and hydroxyl-terminated polydimethylsiloxane is 2:1;
[0092] S2, mixing long-chain diisocyanate and hydroxyethyl acrylate, heating to 90°C, reacting for 150 minutes; washing, drying, and obtaining unsaturated isocyanate; the -NCO / -OH ratio of the long-chain diisocyanate and hydroxyethyl acrylate is 2:1;
[0093] S3, mixing unsaturated isocyanate and epoxy resin, heating to 90°C, and reacting for 5 hours to obtain unsaturated epoxy resin; the -NCO / -OH ratio of unsaturated isocyanate and epoxy resin is 1:1;
[0094] S4, dissolving the monomer and initiator dicumyl peroxide in acetone, adding unsaturated epoxy resin and mixing, removing acetone by vacuum distillation; placing in a rheometer, mixing and reacting at 178°C for 6 minutes, with the rheological rotor speed at 50 rpm, to obtain a modified epoxy resin; the monomer includes 10 parts of polybutadiene, 6 parts of styrene, and 4.4 parts of acrylonitrile; the ratio of monomer to acetone is 10g / 10mL; the mass ratio of unsaturated epoxy resin, monomer, and initiator is 100:15:0.25;
[0095] S5, mixing 18 parts of modified epoxy resin and 4 parts of curing agent diethylaminopropylamine to obtain an epoxy resin composition;
[0096] Step 2: preparing polyurethane resin:
[0097] 1,6-hexamethylene diisocyanate and polycarbonate diol were mixed and stirred for 30 minutes in a nitrogen atmosphere; heated to 75°C and stirred for 90 minutes; hydroxy-terminated polybutadiene was added and the reaction was continued for 120 minutes to obtain a prepolymer; hydroxyethyl acrylate, chain extender 1,4-butanediol, and 0.17wt% catalyst dibutyltin dilaurate were added, the temperature was raised to 85°C, and the reaction was carried out for 30 minutes to obtain a polyurethane; polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and 1 .0wt% initiator dicumyl peroxide is mixed, extruded in a twin-screw extruder, the extrusion temperature is 185-235°C, and the twin-screw speed is 120r / min; granulated, dried, to obtain a polyurethane resin; the polyurethane resin is prepared from the following components by mass: 23.9 parts of 1,6-hexamethylene diisocyanate, 18 parts of terminal hydroxyl polybutadiene, 20 parts of polycarbonate diol, 2 parts of hydroxyethyl acrylate, 9.0 parts of a chain extender; 5 parts of acrylonitrile, 2 parts of styrene, and 3.0 parts of dodecafluoroheptyl methacrylate;
[0098] Step 3: Preparation of carbon fiber composite material:
[0099] Take the carbon fiber cloth and lay it flat in the mold, heat it to 130℃, apply the 90℃ epoxy resin composition on the surface of the carbon fiber, cast it, and impregnate the carbon fiber cloth. Repeat the above operation 3 times; pre-cure to form a pre-cured carbon fiber layer. The pre-curing process conditions are: temperature 100℃, time 30min; the mass ratio of epoxy resin to carbon fiber is 46:100
[0100] The polyurethane resin is sequentially injected onto the upper surface and the lower surface of the pre-cured carbon fiber layer to form a resin layer; and the molding is performed under the following process conditions: a molding temperature of 120°C, a molding time of 80 minutes, and a molding pressure of 0.5 MPa to form a carbon fiber layer and obtain a carbon fiber composite material.
[0101] Comparative Example 1: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0102] Step 1: preparing epoxy resin composition:
[0103] S1. Mix isophorone diisocyanate and hydroxyethyl acrylate, raise the temperature to 85°C, and react for 200 minutes; wash and dry to obtain unsaturated isocyanate; the -NCO / -OH ratio of isophorone diisocyanate and hydroxyethyl acrylate is 2:1;
[0104] S2, mixing unsaturated isocyanate and epoxy resin, heating to 85°C, and reacting for 6 hours to obtain unsaturated epoxy resin; the -NCO / -OH ratio of unsaturated isocyanate and epoxy resin is 1:1;
[0105] S3, dissolving the monomer and initiator dicumyl peroxide in acetone, adding unsaturated epoxy resin and mixing, removing acetone by vacuum distillation; placing in a rheometer, mixing and reacting at 172°C for 8 minutes, with the rheological rotor speed at 40 rpm, to obtain a modified epoxy resin; the monomer includes 10 parts of polybutadiene, 4 parts of styrene, and 1.5 parts of acrylonitrile; the ratio of monomer to acetone is 10 g / 10 mL; the mass ratio of unsaturated epoxy resin, monomer, and initiator is 100:9:0.15;
[0106] S4, mixing 12 parts of modified epoxy resin and 4 parts of curing agent diethylaminopropylamine to obtain an epoxy resin composition;
[0107] Steps 2-3 are the same as those in Example 1 to obtain a carbon fiber composite material.
[0108] Comparative Example 2: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0109] Step 1: preparing epoxy resin composition:
[0110] S1. Mix isophorone diisocyanate and hydroxyethyl acrylate, raise the temperature to 85°C, and react for 200 minutes; wash and dry to obtain unsaturated isocyanate; the -NCO / -OH ratio of isophorone diisocyanate and hydroxyethyl acrylate is 2:1;
[0111] S2, mixing unsaturated isocyanate and epoxy resin, heating to 85°C, and reacting for 6 hours to obtain unsaturated epoxy resin; the -NCO / -OH ratio of unsaturated isocyanate and epoxy resin is 1:1;
[0112] S3, mixing an unsaturated epoxy resin and an initiator dicumyl peroxide; placing the mixture in a rheometer, mixing and reacting for 8 minutes at a temperature of 172° C., with a rheological rotor speed of 40 rpm, to obtain a modified epoxy resin; the monomers include 10 parts of polybutadiene, 4 parts of styrene, and 1.5 parts of acrylonitrile; the mass ratio of the unsaturated epoxy resin to the initiator is 100:0.15;
[0113] S4, mixing 12 parts of modified epoxy resin and 4 parts of curing agent diethylaminopropylamine to obtain an epoxy resin composition;
[0114] Steps 2-3 are the same as those in Example 1 to obtain a carbon fiber composite material.
[0115] Comparative Example 3: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0116] Step 1, preparing an epoxy resin composition: mixing 12 parts of epoxy resin and 6 parts of curing agent diethylaminopropylamine to obtain an epoxy resin composition;
[0117] Steps 2-3 are the same as those in Example 1 to obtain a carbon fiber composite material.
[0118] Comparative Example 4: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0119] Step 2: preparing polyurethane resin:
[0120] Mix 1,6-hexamethylene diisocyanate and polycarbonate diol, stir for 30 minutes in a nitrogen atmosphere; heat to 70°C, stir and react for 150 minutes to obtain a prepolymer; add hydroxyethyl acrylate, chain extender methyl propylene glycol, 0.13wt% catalyst dibutyltin dilaurate, heat to 80°C, react for 60 minutes to obtain a polyurethane;
[0121] The polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and 0.5wt% initiator diisopropylbenzene peroxide are mixed, and extruded in a twin-screw extruder at an extrusion temperature of 185-235°C and a twin-screw speed of 100r / min; granulated and dried to obtain a polyurethane resin; the polyurethane resin is prepared from the following components by weight: 17.6 parts of 1,6-hexamethylene diisocyanate, 20 parts of polycarbonate diol, 1 part of hydroxyethyl acrylate, 7.2 parts of a chain extender; 3 parts of acrylonitrile, 1 part of styrene, and 2.4 parts of dodecafluoroheptyl methacrylate;
[0122] Steps 1 and 3 are the same as those in Comparative Example 3 to obtain a carbon fiber composite material.
[0123] Comparative Example 5: A process for preparing a carbon fiber composite material for a laptop computer shell, comprising the following processes:
[0124] Step 2: preparing polyurethane resin:
[0125] 1,6-hexamethylene diisocyanate and polycarbonate diol were mixed, stirred for 30 minutes in a nitrogen atmosphere; heated to 70°C, stirred and reacted for 150 minutes to obtain a prepolymer; hydroxyethyl acrylate, chain extender methyl propylene glycol, 0.13wt% catalyst dibutyltin dilaurate were added, the temperature was raised to 80°C, reacted for 60 minutes, and a polyurethane resin was obtained; the polyurethane resin was prepared from the following components by mass: 17.6 parts of 1,6-hexamethylene diisocyanate, 23 parts of polycarbonate diol, and 7.2 parts of chain extender;
[0126] Steps 1 and 3 are the same as those in Comparative Example 3 to obtain a carbon fiber composite material.
[0127] Experiment: Take the carbon fiber composite materials obtained in Examples 1-3 and Comparative Examples 1-5, prepare samples, test their properties respectively and record the test results:
[0128] Taking GB / T 1447 as reference standard, the tensile properties of the samples were tested using an electronic universal testing machine at a tensile rate of 2 mm / min.
[0129] Taking GB / T 1449 as reference standard, the three-point bending performance test of the sample was carried out using an electronic universal testing machine;
[0130] Taking ASTM D7136 as the reference standard, an electronic universal testing machine was used to test the impact resistance of the sample. The mass of the impact object was 11.2 kg and the shape of the punch was a hemisphere.
[0131] Tensile strength(MPa) Bending strength(MPa) <![CDATA[Impact toughness (kJ / m 2 ) <!-- 7 -->]]> Example 1 235.3 260.4 146 Example 2 241.8 267.9 152 Example 3 248.2 275.6 159 Comparative Example 1 227.2 252.3 140 Comparative Example 2 198.5 227.8 114 Comparative Example 3 190.7 220.1 108 Comparative Example 4 165.3 207.6 63 Comparative Example 5 156.4 196.9 59
[0132] According to the data in the above table, we can clearly draw the following conclusions:
[0133] The carbon fiber composite materials obtained in Examples 1-3 are compared with the carbon fiber composite materials obtained in Comparative Examples 1-5. The test results show that:
[0134] 1. Compared with the comparative example, the carbon fiber composite materials obtained in Examples 1-3 have higher tensile strength, flexural strength and impact toughness data, which fully demonstrates that the present invention achieves the improvement of the mechanical properties and impact resistance of the prepared carbon fiber composite materials.
[0135] 2. Compared with Example 1, the epoxy resin composition in Comparative Example 1, wherein the modified epoxy resin is prepared from isophorone diisocyanate, hydroxyethyl acrylate, epoxy resin and monomer, does not contain polyethylene glycol; the epoxy resin composition in Comparative Example 2, wherein the modified epoxy resin is prepared from isophorone diisocyanate, hydroxyethyl acrylate and epoxy resin, does not contain polyethylene glycol and monomer; the epoxy resin composition in Comparative Example 3 consists of epoxy resin and curing agent. Compared with Comparative Example 3, the polyurethane resin preparation component in Comparative Example 4 does not contain terminal hydroxyl polybutadiene; the polyurethane resin preparation component in Comparative Example 5 does not contain terminal hydroxyl polybutadiene and olefin monomer. The carbon fiber composite materials obtained in Comparative Examples 1-5 have decreased tensile strength, flexural strength and impact toughness data. It can be seen that the configuration of the carbon fiber composite material components and their processes of the present invention can promote the improvement of their mechanical properties and impact resistance.
[0136] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0137] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A preparation process of carbon fiber composite material for notebook computer shell, Features: Including the following processes: Taking carbon fiber cloth and laying it flat in a mold, coating it with an epoxy resin composition, and precuring it to form a precured carbon fiber layer; injecting polyurethane resin onto the upper surface and the lower surface of the pre-cured carbon fiber layer in sequence to form a resin layer; The carbon fiber layer is formed by molding to obtain a carbon fiber composite material.
2. A process for preparing a carbon fiber composite material for a laptop computer shell according to claim 1, Features: The thickness of the resin layer decreases stepwise from the outside to the inside, with an average thickness of 0.15 to 0.20 mm; The middle of the resin layer is a key area with a thickness of 0.10 to 0.25 mm; the outer thickness of the resin layer is 0.20 to 0.36 mm.
3. A process for preparing a carbon fiber composite material for a laptop computer shell according to claim 1, Features: The epoxy resin composition comprises the following components by weight: 12 to 18 parts of modified epoxy resin and 2 to 6 parts of curing agent.
4. A process for preparing a carbon fiber composite material for a notebook computer shell according to claim 3, Features: The modified epoxy resin is prepared by the following process: Heat the diisocyanate to 80-85°C, slowly add the polyglycol, and react for 100-150 minutes to obtain a long-chain diisocyanate; Mix long-chain diisocyanate and hydroxyethyl acrylate, raise the temperature to 85-90°C, and react for 150-200 minutes to obtain unsaturated isocyanate; Mix unsaturated isocyanate and epoxy resin, raise the temperature to 85-90°C, and react for 5-6 hours to obtain unsaturated epoxy resin; The monomer and the initiator are dissolved in acetone, and unsaturated epoxy resin is added and mixed, and distilled under reduced pressure; the mixture is placed in a rheometer, and mixed and reacted for 6 to 8 minutes at a temperature of 172 to 178° C. to obtain a modified epoxy resin.
5. A process for preparing a carbon fiber composite material for a notebook computer shell according to claim 4, Features: The diisocyanate is one of isophorone diisocyanate, toluene diisocyanate, 1,6-hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, meta-xylylene diisocyanate, tetramethyl dimethylene diisocyanate, dodecylbenzene-2,4-diisocyanate, 4,4-diisocyanate dicyclohexylmethane, 1,4-cyclohexane dimethyl diisocyanate, and 1,6-diisocyanate-2,2,4-trimethylhexane; The polyglycol is a mixture of one or more of polyethylene glycol, polypropylene glycol, hydroxyl-terminated polydimethylsiloxane, polytetramethylene glycol, and polycarbonate glycol.
6. A process for preparing a carbon fiber composite material for a notebook computer shell according to claim 4, Features: The monomers include: by mass, 10 parts of polybutadiene, 4 to 6 parts of styrene, and 1.5 to 4.4 parts of acrylonitrile; The mass ratio of unsaturated epoxy resin, monomer and initiator is 100:(9-15):(0.15-0.25).
7. The process for preparing a carbon fiber composite material for a notebook computer shell according to claim 1, Features: The polyurethane resin is prepared by the following process: Mix 1,6-hexamethylene diisocyanate and polycarbonate diol, stir for 30 minutes in a nitrogen atmosphere; heat to 70-75°C, stir and react for 90-120 minutes; add hydroxyl-terminated polybutadiene, and continue to react for 120-150 minutes to obtain a prepolymer; Add hydroxyethyl acrylate, chain extender and catalyst, raise the temperature to 80-85°C, react for 30-60 minutes to obtain polyurethane; The polyurethane, acrylonitrile, styrene, dodecafluoroheptyl methacrylate and an initiator are mixed, extruded in a twin-screw extruder, granulated and dried to obtain a polyurethane resin.
8. The process for preparing a carbon fiber composite material for a notebook computer shell according to claim 7, Features: The polyurethane resin is prepared from the following mass components: 17.6-23.9 parts of 1,6-hexamethylene diisocyanate, 13-18 parts of hydroxy-terminated polybutadiene, 10-20 parts of polycarbonate diol, 1-2 parts of hydroxyethyl acrylate, 7.2-9.0 parts of chain extender; 3-5 parts of acrylonitrile, 1-2 parts of styrene, 2.4-3.0 parts of dodecafluoroheptyl methacrylate; The chain extender is one of methyl propylene glycol, 2,3-butanediol, 1,4-butanediol and ethylene glycol.
9. The process for preparing a carbon fiber composite material for a notebook computer shell according to claim 7, Features: In the extrusion process, the extrusion temperature is 185-235°C, and the twin-screw speed is 100-120r / min.
10. A carbon fiber composite material for a laptop computer shell, Features: The method is prepared by the preparation process described in any of claims 1 to 9.
Citation Information
Patent Citations
Continuous fiber laminated plate and preparation method thereof
CN102049895A
Manufacturing method of carbon fiber shell
CN102285017A
Method for synthesizing epoxy vinyl ester resin
CN102558456A
Method for manufacturing electronic product composite material shell through resin transfer molding process
CN103802333A
Laptop protective shell
CN105623242A
Cited By
High-performance notebook computer shell composite material and preparation method thereof
CN119859406A
A high-performance laptop computer shell composite material and preparation method thereof
CN119859406B