Contact lens forming method

Through the combination of hydrophilic amphoteric polymer mold and coating material, the problem of insufficient comfort during wearing of contact lens materials is solved, the wear resistance and stain resistance of the lens are improved, and the eye health of the user is improved.

CN119078252APending Publication Date: 2024-12-06XIAN KESIMEI OPTICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411201235.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Traditional contact lens materials have problems such as insufficient comfort, poor wear resistance and stain resistance during wearing, which affects the user's eye health and user experience.

Method used

Using hydrophilic amphoteric polymer molds and coating materials, contact lens lenses with excellent performance are formed through molding, coating and hydration treatment steps. The method includes mixing hydrophilic monomer, initiator and crosslinking agent, molding treatment to form a polymer sheet, and plasma polymerization treatment under an atmosphere of ethanol and wet air, and finally hydrating in water to enhance the biological of the lens Compatibility and wear resistance.

Benefits of technology

It significantly improves the wear comfort, wear resistance and stain resistance of contact lenses, enhances the biocompatibility of the lenses, extends the service life and improves corneal health.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119078252A_ABST
    Figure CN119078252A_ABST
Patent Text Reader

Abstract

The invention discloses a contact lens forming method which is characterized by comprising the following steps: preparing a polymeric monomer mixture: mixing and stirring a solution containing a hydrophilic monomer, an initiator and a cross-linking agent to form the polymeric monomer mixture; mold pressing: dropwise adding the polymeric monomer mixture to a hydrophilic and hydrophobic amphoteric polymer mold to form a transparent polymer sheet; coating treatment: coating the surface of at least one side of the polymer sheet with a coating material, then carrying out plasma polymerization treatment on the coated polymer sheet in a mixed gas atmosphere of ethanol and wetting air, and carrying out plasma treatment in a non-polymerizable gas atmosphere to obtain a contact lens substrate; step 4, hydration: preparing a softening solution, and soaking the contact lens substrate in the softening solution; and soaking the contact lens substrate in water to obtain the contact lens. The performance of the contact lens is improved, and the wearing comfort is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of contact lens molding, in particular to a contact lens molding method. Background Art

[0002] Contact lenses are formed by connecting molecules of different chemicals. The materials used for contact lenses are also constantly improving. Traditionally, contact lens materials are mainly divided into two categories: hard contact lenses and soft contact lenses. In recent years, with the development of science and technology, modern contact lens materials have gradually developed. As a product directly attached to the cornea of ​​the eye, the quality of contact lenses is directly related to the eye health of consumers. Therefore, the control of their performance is crucial. Summary of the invention

[0003] According to one aspect of the present application, a method for molding a contact lens is provided, which improves the performance of the contact lens and increases the wearing comfort.

[0004] A method for forming a contact lens, characterized in that it comprises:

[0005] Step 1: preparing a polymerization monomer mixture: mixing and stirring a solution including a hydrophilic monomer, an initiator and a cross-linking agent to form a polymerization monomer mixture;

[0006] Step 2, molding: molding the polymerized monomer mixture, dropping the polymerized monomer mixture onto a hydrophilic and hydrophobic polymer mold, standing for 10-30 minutes, and then performing a polymerization cross-linking reaction to form a transparent polymer sheet;

[0007] Step 3, coating treatment: coating the coating material on at least one side of the surface of the polymer sheet, and then subjecting the coated polymer sheet to plasma polymerization treatment in a mixed gas atmosphere of ethanol and humidified air, and plasma treatment in a non-polymerizable gas atmosphere, thereby forming a surface coating to obtain a contact lens substrate, wherein the non-polymerizable gas refers to a gas that does not have the property of being deposited on the surface after plasma treatment;

[0008] Step 4, hydration: prepare a softening liquid, which is an immersion liquid; immerse the contact lens substrate in the softening liquid for at least 30 minutes; and immerse the contact lens substrate in water for at least 15 minutes to obtain a contact lens.

[0009] Further, the coating material includes a mixture of solution A and solution B;

[0010] The solution A comprises 2-carboxyethyl methacrylate, styrene, (di)benzoyl peroxide and glycidyl methacrylate;

[0011] The solution B includes 2-carboxyethyl methacrylate and ethoxyethanol.

[0012] Further, the hydrophilic monomer includes 2-carboxyethyl methyl acrylate and N-vinyl pyrrolidine;

[0013] The initiator includes azobisisobutyronitrile;

[0014] The crosslinking agent includes tetraethylene glycol diacrylate and methyl methacrylate.

[0015] Furthermore, the preparation method of the hydrophilic and hydrophobic polymer mold includes:

[0016] (1) spraying an olefin monomer containing a hydrophilic group on a mold substrate, increasing the temperature to initiate a polymerization reaction, and forming a continuous hydrophilic polymer film on the surface of the substrate;

[0017] (2) laser etching is used to arrange and distribute regular hollow structures on a continuous hydrophilic polymer film;

[0018] (3) Filling the hollow structure with a hydrophobic monomer, increasing the temperature to initiate a polymerization reaction to form a hydrophobic polymer micromodule, and obtaining a hydrophilic and hydrophobic amphiphilic polymer mold.

[0019] Further, the configuration of the polymerization monomer mixture comprises the following steps:

[0020] (1) Material purification: Use vacuum distillation to remove the inhibitor or water in the material to be purified;

[0021] (2) Weighing: Weigh the corresponding components of the hydrophilic monomer, initiator and cross-linking agent according to the ratio into a clean container;

[0022] (3) Stirring: Add a magnetic stirrer to the weighed polymerization solution, seal the container, place on a stirrer and stir at 2-8°C for 4-6 hours;

[0023] (4) Filtration: Use filter membrane or filter paper to remove impurities and filter.

[0024] Furthermore, soaking the contact lens substrate in water for at least 15 minutes includes placing the contact lens substrate in saline with a pH value of 8 to 11, and performing alternating hydration treatment in distilled water at a temperature of 60 to 90° C. for 8 to 20 hours.

[0025] The beneficial effects of this application include:

[0026] The present application provides a method for molding a contact lens, wherein the polymerization monomer mixture is dripped onto a hydrophilic and hydrophobic polymer mold for a molding reaction. The hydrophilic and hydrophobic polymer mold improves the comfort and performance of the contact lens, and further a coating treatment is performed to improve the wear resistance, anti-fouling and biocompatibility of the lens. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a schematic diagram of a process for forming a contact lens. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] See also Figure 1 The present invention provides a method for forming a contact lens, characterized in that it comprises:

[0030] Step 1: preparing a polymerization monomer mixture: mixing and stirring a solution including a hydrophilic monomer, an initiator and a cross-linking agent to form a polymerization monomer mixture;

[0031] Step 2, molding: molding the polymerized monomer mixture, dropping the polymerized monomer mixture onto a hydrophilic and hydrophobic polymer mold, standing for 10-30 minutes, and then performing a polymerization cross-linking reaction to form a transparent polymer sheet;

[0032] Step 3, coating treatment: coating the coating material on at least one side of the surface of the polymer sheet, and then subjecting the coated polymer sheet to plasma polymerization treatment in a mixed gas atmosphere of ethanol and humidified air, and plasma treatment in a non-polymerizable gas atmosphere, thereby forming a surface coating to obtain a contact lens substrate, wherein the non-polymerizable gas refers to a gas that does not have the property of being deposited on the surface after plasma treatment;

[0033] Step 4, hydration: prepare a softening liquid, which is an immersion liquid; immerse the contact lens substrate in the softening liquid for at least 30 minutes; and immerse the contact lens substrate in water for at least 15 minutes to obtain a contact lens.

[0034] Specifically, the method includes multiple key steps, each of which has its specific operations and requirements. First, it is the configuration of the polymer monomer mixture. This step requires mixing and fully stirring the three main components of hydrophilic monomer, initiator and cross-linking agent to form a polymer monomer mixture. The hydrophilic monomer is the main material constituting the lens, which determines the hydrophilicity and biocompatibility of the lens; the initiator is used to initiate the polymerization reaction so that the monomer molecules are connected into a polymer chain; the cross-linking agent is used to adjust the properties of the polymer to meet specific usage requirements. Next, it is the molding process. In this step, the polymer monomer mixture is dripped onto the hydrophilic and hydrophobic amphiphilic polymer mold and left to stand for a period of time (10-30 minutes) so that the mixture is evenly distributed in the mold and initially solidified. Then, the polymerization cross-linking reaction is carried out to form a stable chemical bond between the monomer molecules, thereby obtaining a transparent polymer sheet. Then, it is the coating process. The purpose of this step is to form a protective film on the surface of the polymer sheet to improve the wear resistance, anti-fouling and biocompatibility of the lens. First, the coating material is plated on at least one side of the polymer sheet; then, plasma polymerization is carried out in a mixed gas atmosphere of ethanol and humidified air to form a dense protective film on the surface of the sheet; finally, plasma treatment is carried out in a non-polymerizing gas atmosphere to further improve the performance of the film layer. The non-polymerizing gas plays a role in cleaning and activating the surface here, but does not form deposits on the surface. Finally, it is hydration treatment. This step is to make the lens softer and more comfortable. First, a softening liquid (usually an immersion liquid) is prepared; then, the contact lens base is immersed in the softening liquid for a period of time (at least 30 minutes) so that the lens fully absorbs water and becomes soft; finally, the lens is immersed in water for at least 15 minutes to remove the residual softening liquid and other impurities to obtain the final contact lens. In summary, this contact lens molding method can obtain contact lenses with excellent performance and high quality through precise steps and condition control.

[0035] It is worth noting that hydrophilic and hydrophobic polymer molds play a key role in the preparation of contact lenses, and their unique properties have a significant impact on the performance of the lenses. Hydrophilic and hydrophobic polymer molds combine the characteristics of hydrophilicity and hydrophobicity, which can form microscopic hydrophilic and hydrophobic areas on the surface of the lens. The hydrophilic area helps the lens to better contact with tears, improve the wettability, moisture retention and wearing comfort of the lens; while the hydrophobic area may help reduce the deposition of proteins and other pollutants, and improve the cleanliness and service life of the lens. The hydrophilic and hydrophobic structure in the mold may increase the gas exchange between the lens and the external environment through the design of micropores or microchannels, thereby improving the breathability of the lens. This is particularly important for reducing the problem of corneal hypoxia that may occur when wearing contact lenses, and helps to maintain the health of the cornea. The preparation process of hydrophilic and hydrophobic polymer molds involves cross-linking and strengthening of polymer materials, which helps to improve the mechanical properties of the lens, such as tensile strength, tear resistance and abrasion resistance. The improvement of these properties makes the lens more durable during use and able to resist damage from external forces. By adjusting the distribution and morphology of the hydrophilic and hydrophobic structures in the mold, customized design of lens functions can be achieved. For example, a drug release function can be introduced in a specific area on the lens surface to prevent eye diseases; or an optical correction function can be introduced to meet different vision correction needs. The precision and reproducibility of hydrophilic and hydrophobic polymer molds help to achieve mass production and quality control of contact lenses. The precision of the mold ensures that each lens has a consistent shape and size, thereby improving production efficiency and yield. At the same time, the durability of the mold also reduces the frequency of mold replacement during the production process and reduces production costs.

[0036] The coating material comprises a mixture of solution A and solution B;

[0037] The solution A comprises 2-carboxyethyl methacrylate, styrene, (di)benzoyl peroxide and glycidyl methacrylate;

[0038] The solution B includes 2-carboxyethyl methacrylate and ethoxyethanol.

[0039] Wherein, in terms of mass percentage, the ratio of solution A to solution B is 3:1;

[0040] 2-Carboxyethyl methacrylate: styrene: (di)benzoyl peroxide: glycidyl methacrylate = 60%: 30%: 0.5%: 10%; 2-Carboxyethyl methacrylate: ethoxyethanol = 65%: 35%.

[0041] Specifically, the performance of the lens is improved by forming a protective film on the surface of the polymer sheet. The coating material is composed of a mixture of solution A and solution B, each of which contains specific chemical components. 2-Carboxyethyl methacrylate is a hydrophilic and reactive monomer that is commonly used to prepare polymers with excellent biocompatibility and mechanical properties. During the coating process, it can be copolymerized with other monomers to form a stable protective film. Styrene is a commonly used monomer with good rigidity and transparency. Adding styrene to the coating material can improve the hardness and wear resistance of the protective film. Benzoyl peroxide (di) is a free radical initiator that can initiate monomer polymerization under heating or light conditions. In the coating process, it is used to initiate the polymerization of monomers in solution A to form a dense protective film. Glycidyl methacrylate contains epoxy groups and can react with a variety of substances, such as cross-linking, grafting, etc. In the coating material, it can increase the cross-linking density of the protective film and improve the water resistance and solvent resistance of the film. 2-Carboxyethyl methacrylate Like the same component in solution A, 2-carboxyethyl methacrylate also plays a role in providing hydrophilicity and reactivity in solution B. Ethoxyethanol is an organic solvent with good solubility and volatility. In the coating process, it can be used as a solvent to dissolve other components in solution B and evaporate in the subsequent treatment process, leaving a pure protective film. In addition, ethoxyethanol may also affect certain properties of the protective film, such as softness and wettability. In the coating process, solution A and solution B are first mixed evenly and then coated on at least one side of the polymer sheet. Next, plasma polymerization is carried out in a mixed gas atmosphere of ethanol and humidified air. Plasma polymerization is a method that uses high-energy particles in plasma to initiate monomer polymerization, which can quickly form a dense protective film at low temperature. Finally, plasma treatment is carried out in a non-polymerizing gas atmosphere to further improve the performance of the film layer.

[0042] The hydrophilic monomers include 2-carboxyethyl methyl acrylate and N-vinyl pyrrolidine;

[0043] The initiator includes azobisisobutyronitrile;

[0044] The crosslinking agent includes tetraethylene glycol diacrylate and methyl methacrylate.

[0045] It is worth noting that, according to mass percentage, 2-carboxyethyl methacrylate: N-vinylpyrrolidine: azobisisobutyronitrile: tetraethylene glycol diacrylate and methyl methacrylate = 50%-80%: 5%-20%: 0.1%-1%: 1%-10%: 5%-20%.

[0046] Specifically, methyl 2-carboxyethyl acrylate in the hydrophilic monomer is a monomer with hydrophilicity and reactivity, and is commonly used to prepare polymers with good biocompatibility. In contact lenses, it helps to maintain the wettability of the lens and improves the comfort of wearing. N-vinyl pyrrolidine is also a hydrophilic monomer, which has good water solubility and biocompatibility. During the polymerization process, it can be copolymerized with other monomers to form a polymer with excellent performance. In contact lenses, the addition of N-vinyl pyrrolidine can further enhance the hydrophilicity and comfort of the lens. Azobisisobutyronitrile (AIBN) is a commonly used free radical initiator, which can decompose under heating conditions to produce free radicals, thereby initiating monomer polymerization. In the molding process of contact lenses, AIBN is used to initiate the polymerization reaction of hydrophilic monomers, crosslinking agents and other components to form a stable polymer network. Tetraethylene glycol diacrylate is a multifunctional monomer, which contains two acrylate groups and can form crosslinking points during the polymerization process. In contact lenses, the addition of tetraethylene glycol diacrylate can increase the crosslinking density of the polymer, thereby enhancing the mechanical properties and stability of the lens. Methyl methacrylate (MMA) has good transparency and processing properties. In contact lenses, the addition of MMA can adjust the glass transition temperature, refractive index and other properties of the polymer to meet specific usage requirements. At the same time, MMA can also copolymerize with other monomers to form polymers with excellent properties.

[0047] When preparing the polymerizable monomer mixture, the hydrophilic monomer (2-carboxyethyl methacrylate and N-vinylpyrrolidine), initiator (azobisisobutyronitrile) and crosslinker (tetraethylene glycol diacrylate and methyl methacrylate) need to be mixed in a certain proportion and stirred thoroughly to ensure that the components are evenly dispersed. Subsequently, the mixture is molded to form a transparent polymer sheet, which is further coated and hydrated to finally obtain a contact lens.

[0048] The preparation method of the hydrophilic and hydrophobic polymer mold comprises:

[0049] (1) spraying an olefin monomer containing a hydrophilic group on a mold substrate, increasing the temperature to initiate a polymerization reaction, and forming a continuous hydrophilic polymer film on the surface of the substrate;

[0050] Among them, the preheating stage: first, preheat the silicon wafer to a relatively low temperature (such as between room temperature and 100°C) to remove moisture and impurities on the surface and make the silicon wafer reach a stable temperature state. Polymerization reaction stage: Then, gradually increase the temperature to above the decomposition temperature of the initiator, but not exceeding the tolerance limit of the monomer and the silicon wafer. For initiators such as (di)benzoyl peroxide, the decomposition temperature is usually between 60-100°C, but the specific temperature needs to be adjusted according to the type and purity of the initiator used. Insulation stage: After reaching the optimal polymerization reaction temperature, keep it for a period of time to ensure that the polymerization reaction is fully carried out. Cooling stage: After the polymerization reaction is completed, the silicon wafer is gradually cooled to room temperature. The cooling rate should not be too fast to avoid internal stress or cracking of the polymer film.

[0051] (2) laser etching is used to arrange and distribute regular hollow structures on a continuous hydrophilic polymer film;

[0052] Among them, laser types include ultraviolet lasers (such as Nd:YAG pulsed lasers with a wavelength of 355nm), femtosecond lasers, etc. These laser sources have high energy density and good focusing performance, and are suitable for etching nanopores. Laser power density is one of the key factors in the formation of nanopores. High power density can ensure that the material is vaporized and evaporated in an instant to form a precise nanopore structure. The specific power density needs to be determined according to the characteristics of the processed material and the required nanopore size. For pulsed lasers, the pulse width also has an important influence on the formation of nanopores. Lasers with short pulse widths can reduce the heat-affected zone and are conducive to the formation of finer nanopore structures. The repetition frequency determines the number of laser pulses per unit time, which affects the processing efficiency and consistency of the nanopores. The appropriate repetition frequency needs to be selected according to the processing requirements and equipment performance. Different materials have different physical and chemical properties, and their absorption and reflectivity of lasers are also different. Therefore, the characteristics of the processed material need to be considered when selecting laser etching parameters. The surface state of the material (such as roughness, oxide layer, etc.) will affect the effect of laser etching. The material needs to be properly pretreated before processing to ensure the quality of nanopore formation. The temperature of the processing environment will affect the thermal conductivity of the material and the processing effect of the laser. It is necessary to maintain a stable processing temperature to reduce the heat-affected zone and facilitate the formation of nanopores. In some cases, the atmosphere in the processing environment (such as inert gas protection) can reduce the oxidation and corrosion of the material and improve the quality of nanopore formation.

[0053] In this application, the selection of laser (such as Nd:YAG pulse laser, wavelength of 355nm), pulse width (5-8ns), exposure energy and other parameters are also critical.

[0054] (3) Filling the hollow structure with a hydrophobic monomer, increasing the temperature to initiate a polymerization reaction to form a hydrophobic polymer micromodule, and obtaining a hydrophilic and hydrophobic amphiphilic polymer mold.

[0055] Specifically, first, a layer of olefin monomer containing hydrophilic groups is sprayed on the mold substrate (such as silicon wafer, glass, etc.). These hydrophilic groups (such as hydroxyl, carboxyl, etc.) can give the polymer film good hydrophilic properties. Subsequently, by heating treatment, a polymerization reaction between the monomers is initiated, thereby forming a continuous and dense hydrophilic polymer film on the surface of the substrate. The purpose of this step is to construct a hydrophilic interface on the mold substrate, providing a basis for the subsequent formation of a hollow structure. The continuity and density of the hydrophilic film are crucial to the success of subsequent steps. The preparation of the mold substrate includes: placing polyvinyl chloride resin, phenolic resin, silicon carbide and silicon dioxide in a ball mill in proportion, and grinding them into a mixed powder of 400 mesh; adding a curing agent and a surfactant to the mixed powder and baking it in an oven for 25 to 30 minutes; when the oven temperature cools to room temperature, taking out the polymer material in the oven and forming a mold blank according to size requirements; placing the mold blank in an electric furnace and sintering it at a high temperature of 550 to 600°C; cleaning the dust, oil stains and sintered carbon on the surface of the mold blank substrate and polishing it to form a mold substrate.

[0056] After the hydrophilic polymer film is formed, it is processed by laser etching technology. The laser beam is irradiated on the surface of the film in a precise manner. By controlling the parameters such as the laser power, scanning speed and scanning path, the film is ablated or decomposed in a specific area, thereby forming a regular hollow structure on the film. These hollow structures have specific pore sizes (30-300nm) and pore depths (300nm-5μm) to meet the needs of subsequent steps. Laser etching technology can accurately control the formation of nanoscale structures, giving the mold unique hydrophilic and hydrophobic properties and microscopic morphology. After the hollow structure is formed, hydrophobic monomers (such as monomers containing elements such as fluorine and silicon) are filled into these structures. Then, the temperature is increased again to initiate the polymerization reaction, so that the hydrophobic monomers are polymerized into hydrophobic polymers inside the hollow structure. In this way, a hydrophilic and hydrophobic polymer mold is obtained, in which the hydrophilic polymer film is used as a substrate, and the hydrophobic polymer is filled in the hollow structure. By filling the hydrophobic monomer and initiating the polymerization reaction, the hydrophobic property can be introduced into the mold to form a hydrophilic and hydrophobic nanostructure. This structure not only helps to achieve specific functions in the contact lens manufacturing process (such as controlling moisture penetration, improving lens comfort, etc.), but also enhances the durability and stability of the mold.

[0057] It is worth noting that the hollow structure is distributed in the form of a ring lattice around the hydrophilic film. In the preparation of the lens, the hydrophilic and hydrophobic polymer mold combines the characteristics of hydrophilicity and hydrophobicity, which can form microscopic hydrophilic and hydrophobic areas on the surface of the lens. The hydrophilic area helps the lens to better contact with tears, improve the wettability and wearing comfort of the lens; while the hydrophobic area may help reduce the deposition of proteins and other pollutants, and improve the cleanliness and service life of the lens. Since the hydrophobic polymer micromodule is hydrophobic, the air on the surface of the template can be stably distributed on the surface of the hydrophobic micromodule in the form of microbubbles, and many microbubbles form a layer of air film on the surface of the template. The air film improves the wearing comfort of the lens to a certain extent. Due to the reduction of friction between water molecules and the surface of the lens, the sliding of the lens on the eyeball may be smoother, reducing the discomfort of the wearer. At the same time, the surface of the continuous hydrophilic component combines with water to form a relatively stable liquid film between the microbubbles, which helps to improve the stability of the microbubbles. The hydrophilic and hydrophobic polymer template provides a guarantee for reducing the friction resistance coefficient of the friction surface due to its special surface wetting properties, thereby improving wearing comfort.

[0058] The configuration of the polymerization monomer mixture comprises the following steps:

[0059] (1) Material purification: Use vacuum distillation to remove the inhibitor or water in the material to be purified;

[0060] (2) Weighing: Weigh the corresponding components of the hydrophilic monomer, initiator and cross-linking agent according to the ratio into a clean container;

[0061] (3) Stirring: Add a magnetic stirrer to the weighed polymerization solution, seal the container, place on a stirrer and stir at 2-8°C for 4-6 hours;

[0062] (4) Filtration: Use filter membrane or filter paper to remove impurities and filter.

[0063] Specifically, material purification is the first step in configuring the polymerization monomer mixture, the purpose of which is to remove impurities in the raw materials, especially inhibitors and moisture. These impurities may interfere with the progress of the polymerization reaction, resulting in a decrease in the reaction rate, a broadening of the molecular weight distribution of the product, or the generation of unnecessary by-products. These impurities can be effectively removed by using a vacuum distillation method, because the vacuum can reduce the boiling point of the substance, so that the impurities can be evaporated at a lower temperature. Among them, ensure that the air tightness of the vacuum distillation device is good to avoid the introduction of new impurities during the distillation process. Control the distillation temperature and pressure to fully remove impurities without destroying the main components of the raw materials. After the material is purified, the hydrophilic monomer, initiator and cross-linking agent need to be weighed into a clean container according to a predetermined ratio. The accuracy of this step is crucial to the success of the subsequent polymerization reaction, because different ratios will lead to differences in the performance of the polymer product. Among them, use an accurate weighing tool (such as an electronic balance) to weigh to ensure the accuracy of the ratio. The container must be clean and dry to avoid the introduction of new impurities. Add a magnetic stirrer to the weighed polymerization solution, then seal it and place it on a stirrer for stirring. The purpose of stirring is to mix all the components thoroughly and evenly to form a uniform polymerization monomer mixture. The stirring temperature and time need to be strictly controlled to ensure the mixing effect and avoid unnecessary side reactions. Among them, the stirring temperature should be controlled between 2-8°C to avoid high temperature inducing polymerization or causing decomposition of raw materials. The stirring time is generally 4-6 hours to ensure that all components are fully mixed. During the stirring process, attention should be paid to observing the state of the mixture, and any abnormalities should be handled in time. After the stirring is completed, the mixture needs to be filtered using a filter membrane or filter paper to remove impurities. The purpose of this step is to remove solid impurities or undissolved particles that may be generated during the stirring process to ensure the purity of the polymerization monomer mixture. Among them, select a suitable filter membrane or filter paper to ensure that impurities can be effectively removed without affecting the performance of the mixture. During the filtration process, attention should be paid to maintaining the cleanliness of the operating environment to avoid introducing new sources of pollution.

[0064] Soaking the contact lens substrate in water for at least 15 minutes comprises placing the contact lens substrate in saline with a pH value of 8 to 11, and performing alternating hydration treatment in distilled water at a temperature of 60 to 90° C. for 8 to 20 hours.

[0065] Specifically, the process involves placing the lens substrate in distilled water at a specific pH value and temperature for alternating hydration treatment. First, the contact lens substrate is placed in saline with a pH value of 8 to 11. This pH range is selected to ensure that the saline environment will not damage the lens material, but can effectively remove residues on the lens surface while promoting the formation of a hydrophilic layer. The specific composition of the saline may include water and a certain amount of salts (such as sodium chloride), and other ingredients may be added to adjust the pH value or provide additional functions. Subsequently, the lens will be subjected to alternating hydration treatment in distilled water at a temperature of 60 to 90°C. Distilled water is selected because it is relatively pure and does not contain impurities and microorganisms, which helps to reduce the risk of contamination of the lens during processing. High temperature treatment can accelerate the hydration process and make the lens reach the desired hydrophilicity and comfort more quickly. However, it should be noted that the temperature must be controlled within a safe range to avoid thermal damage or deformation to the lens material. Alternating hydration treatment means that the lens will be alternately immersed between saline and distilled water. This alternating treatment method helps to more thoroughly remove residues on the lens surface and promote the uniform formation of a hydrophilic layer. The specific alternating time and number of times will vary depending on the lens material, saline formula and manufacturer's requirements. The entire alternating hydration process needs to last 8 to 20 hours. This time range is selected to ensure that the lens can be fully hydrated and achieve the required performance requirements. During this period of time, the lens will undergo multiple alternating soaks of saline and distilled water to gradually improve its hydrophilicity and comfort.

[0066] The contact lens substrate is placed in saline with a pH value of 8 to 11 and alternately hydrated in distilled water at 60 to 90°C for 8 to 20 hours to improve the performance and user experience of the lens. This process provides the wearer with a better visual experience by removing residues on the lens surface, promoting the formation of a hydrophilic layer, and improving the comfort of the lens. However, the specific processing conditions (such as pH value, temperature, time, etc.) vary depending on the lens material and manufacturer's requirements.

[0067] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for forming a contact lens, characterized in that: include: Step 1: preparing a polymerization monomer mixture: mixing and stirring a solution including a hydrophilic monomer, an initiator and a cross-linking agent to form a polymerization monomer mixture; Step 2, molding: molding the polymerized monomer mixture, dropping the polymerized monomer mixture onto a hydrophilic and hydrophobic polymer mold, standing for 10-30 minutes, and then performing a polymerization cross-linking reaction to form a transparent polymer sheet; Step 3, coating treatment: coating the coating material on at least one side of the surface of the polymer sheet, and then subjecting the coated polymer sheet to plasma polymerization treatment in a mixed gas atmosphere of ethanol and humidified air, and plasma treatment in a non-polymerizable gas atmosphere, thereby forming a surface coating to obtain a contact lens substrate, wherein the non-polymerizable gas refers to a gas that does not have the property of being deposited on the surface after plasma treatment; Step 4, hydration: prepare a softening liquid, which is an immersion liquid; immerse the contact lens substrate in the softening liquid for at least 30 minutes; and immerse the contact lens substrate in water for at least 15 minutes to obtain a contact lens.

2. A method for forming a contact lens according to claim 1, characterized in that: The coating material comprises a mixture of solution A and solution B; The solution A comprises 2-carboxyethyl methacrylate, styrene, (di)benzoyl peroxide and glycidyl methacrylate; The solution B includes 2-carboxyethyl methacrylate and ethoxyethanol.

3. A method for forming a contact lens according to claim 1, characterized in that: The hydrophilic monomers include 2-carboxyethyl methyl acrylate and N-vinyl pyrrolidine; The initiator includes azobisisobutyronitrile; The crosslinking agent includes tetraethylene glycol diacrylate and methyl methacrylate.

4. A method for forming a contact lens according to claim 1, characterized in that: The preparation method of the hydrophilic and hydrophobic polymer mold comprises: (1) spraying an olefin monomer containing a hydrophilic group on a mold substrate, increasing the temperature to initiate a polymerization reaction, and forming a continuous hydrophilic polymer film on the surface of the substrate; (2) laser etching is used to arrange and distribute regular hollow structures on a continuous hydrophilic polymer film; (3) Filling the hollow structure with a hydrophobic monomer, increasing the temperature to initiate a polymerization reaction to form a hydrophobic polymer micromodule, and obtaining a hydrophilic and hydrophobic polymer mold.

5. A method for forming a contact lens according to claim 1, characterized in that: The preparation of the polymerization monomer mixture comprises the following steps: (1) Material purification: Use vacuum distillation to remove the inhibitor or water in the material to be purified; (2) Weighing: Weigh the corresponding components of the hydrophilic monomer, initiator and cross-linking agent according to the ratio into a clean container; (3) Stirring: Add a magnetic stirrer to the weighed polymer solution, seal the container, place on a stirrer and stir at 2-8°C for 4-6 hours; (4) Filtration: Use filter membrane or filter paper to remove impurities and filter.

6. A method for forming a contact lens according to claim 1, characterized in that: Soaking the contact lens substrate in water for at least 15 minutes comprises placing the contact lens substrate in saline with a pH value of 8 to 11, and performing alternating hydration treatment in distilled water at a temperature of 60 to 90° C. for 8 to 20 hours.