N, S and Fe co-doped microcrystalline cellulose carbon microspheres as well as preparation method and application thereof

Through the preparation of N, S, Fe co-doped microcrystalline cellulose carbon microspheres, the multi-component and spherical structures are used to improve the impedance matching of electromagnetic wave absorbing materials, the problems of narrow absorption bandwidth and impedance imbalance in the prior art are solved, and the problem of narrow absorption bandwidth and impedance imbalance in the prior art is realized. Efficient electromagnetic wave absorption and energy conversion.

CN119079974APending Publication Date: 2024-12-06OCEAN UNIV OF CHINA +2
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411199744.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The impedance matching of existing electromagnetic wave absorption materials is poor, resulting in too narrow effective absorption bandwidth, and the absorption of electromagnetic waves by a single component material only depends on dielectric loss, resulting in impedance imbalance and it is difficult to effectively absorb electromagnetic waves.

Method used

Using the preparation method of co-doped microcrystalline cellulose carbon microspheres, the preparation method of N, S, Fe co-doped microcrystalline cellulose, water and triazine compounds are mixed to form binary microspheres, and then mixed with ferromagnetic substances to form ternary microspheres. The ball is carbonized under a protective atmosphere to form carbon microspheres with C, N, O, S, and Fe elements, and the polarization loss and interface loss of the material are improved by using multi-component and spherical structures to achieve impedance matching.

Benefits of technology

The attenuation ability of the material is improved, the reflection ability of electromagnetic waves is enhanced, and the absorption rate reaches 99%. At the same time, due to rich resources, low cost and environmentally friendly, the efficient conversion of electromagnetic energy into thermal energy is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079974A_ABST
    Figure CN119079974A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of electromagnetic wave absorbing materials, and provides N, S and Fe co-doped microcrystalline cellulose carbon microspheres as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing microcrystalline cellulose, water and a triazine compound, and reacting to obtain binary microspheres; mixing a ferromagnetic substance, water and the binary microspheres, and reacting to obtain ternary microspheres; and under a protective atmosphere, carbonizing the ternary microspheres to obtain the N, S and Fe co-doped microcrystalline cellulose carbon microspheres. According to the carbon microspheres, a sphere formed by polymerizing microcrystalline cellulose serves as a sphere inner shell, and a triazine compound and a ferromagnetic substance serve as a sphere outer shell. Due to the existence of multiple components, the polarization loss of the material can be improved, due to the existence of the spherical structure, the interface loss of the material can be improved, and under the action of multiple loss mechanisms, the carbon microsphere wave-absorbing material can achieve good impedance matching and improve the attenuation capacity, so that the electromagnetic wave reflecting capacity of the material is enhanced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electromagnetic wave absorbing materials, and in particular to N, S, Fe co-doped microcrystalline cellulose carbon microspheres and a preparation method and application thereof. Background Art

[0002] The development of electronic information technology, such as the continuous optimization of electronic products such as communication tools, medical equipment, and military equipment, has brought great convenience to contemporary society. At the same time, their power has also increased exponentially, resulting in a significant increase in electromagnetic radiation on the ground, generating a large amount of electromagnetic radiation source pollution. Electromagnetic wave absorbing materials can convert electromagnetic waves into other forms of energy and dissipate them. Therefore, it is of great significance to study electromagnetic wave absorbing materials with strong dissipation capacity. Electromagnetic wave absorbing materials prepared with sugar balls made of polysaccharide cellulose as carbon-based materials have the advantages of being non-toxic, environmentally friendly, and low in price. However, the impedance matching of the single-component polymerized sugar balls is poor, resulting in an effective absorption bandwidth that is too narrow, and the absorption of electromagnetic waves by the single-component polymerized sugar balls is achieved only by dielectric loss attenuation, resulting in impedance imbalance. In addition, in addition to the composition of the electromagnetic wave absorbing material, the structure also has a great influence on the absorption performance of the electromagnetic wave absorbing material. Based on the above analysis, the reasonable optimization of the composition and structure of the absorber has become a problem that needs to be solved urgently. Summary of the invention

[0003] The purpose of the present invention is to overcome the problems existing in the prior art and provide a N, S, Fe co-doped microcrystalline cellulose carbon microsphere and a preparation method and application thereof.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] The present invention provides a method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres, comprising the following steps:

[0006] (1) mixing microcrystalline cellulose, water and a triazine compound and reacting them to obtain binary microspheres;

[0007] (2) mixing the ferromagnetic material, water and the binary microspheres and reacting them to obtain the ternary microspheres;

[0008] (3) Carbonizing the ternary microspheres under a protective atmosphere to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

[0009] Preferably, the triazine compound in step (1) comprises cyanuric acid and / or thiocyanuric acid.

[0010] Preferably, in step (1), the mass ratio of microcrystalline cellulose, water and triazine compound is 2.5-10:40-80:1-5.

[0011] Preferably, the reaction temperature in step (1) is 180-220° C., and the reaction time is 8-12 h.

[0012] Preferably, the ferromagnetic material in step (2) includes one or more of ferric citrate, ferric acetylacetonate, ferrous gluconate and ferric phosphate.

[0013] Preferably, in step (2), the mass ratio of the ferromagnetic substance, water and binary microspheres is 0.1-1:30-60:5-10.

[0014] Preferably, the reaction temperature in step (2) is 180-220° C., and the reaction time is 8-12 h.

[0015] Preferably, the protective atmosphere in step (3) is nitrogen or argon, and the gas flow rate of the protective atmosphere is 200-300 mg / L;

[0016] The heating rate of the carbonization in step (3) is 2-5°C / min, the target temperature of the carbonization is 700-900°C, and the insulation time to reach the target temperature is 1.5-2.5h.

[0017] The present invention also provides N, S, Fe co-doped microcrystalline cellulose carbon microspheres prepared by the preparation method of the N, S, Fe co-doped microcrystalline cellulose carbon microspheres.

[0018] The present invention also provides the application of the N, S and Fe co-doped microcrystalline cellulose carbon microspheres in electromagnetic wave absorption.

[0019] The beneficial effects of the present invention are:

[0020] The invention provides a method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres, comprising the following steps: mixing microcrystalline cellulose, water, and triazine compounds, reacting to obtain binary microspheres; mixing ferromagnetic substances, water, and binary microspheres, reacting to obtain ternary microspheres; and carbonizing the ternary microspheres under a protective atmosphere to obtain N, S, and Fe co-doped microcrystalline cellulose carbon microspheres. The N, S, and Fe co-doped microcrystalline cellulose carbon microspheres prepared by the invention contain C, N, O, S, and Fe elements, and have a diameter of about 2 to 6 μm. The carbon microspheres use microcrystalline cellulose polymerized balls as the inner shells of the balls, and triazine compounds and ferromagnetic substances as the outer shells of the balls. Due to the presence of multiple components, the polarization loss of the material can be increased, and due to the presence of the spherical structure, the interface loss of the material can be increased. Under the action of multiple loss mechanisms, the carbon microsphere absorbing material can achieve good impedance matching, and the attenuation capacity is improved, thereby enhancing the ability of the material to reflect electromagnetic waves.

[0021] The carbon-based material microcrystalline cellulose used in the present invention is not only rich in resources, low in cost and environmentally friendly. By modifying the single-component polymer sugar spheres with triazine compounds, N / NS atoms can form defects after carbonization, causing dipole polarization, and promoting the attenuation of electromagnetic waves; the introduction of ferromagnetic substances increases the magnetic loss, so that the absorber attenuates electromagnetic waves under the action of dielectric loss and magnetic loss; in addition, by modifying the single-component polymer sugar spheres and preparing them into a core-shell structure, multiple reflections of electromagnetic waves can be promoted, which is beneficial for the material to maximize the conversion of electromagnetic energy into heat energy. The carbon microspheres finally prepared have an absorption rate of up to 99% for electromagnetic waves. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The scanning electron microscope characterization images of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Examples 1 to 3; Figure 1 In the figure, a is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 1, b is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 2, and c is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 3;

[0023] Figure 2 This is the reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 1;

[0024] Figure 3 This is the reflection loss diagram (Frequency—frequency, Reflection Loss—reflection loss) of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 2;

[0025] Figure 4 This is the reflection loss diagram of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 3 (Frequency—frequency, Reflection Loss—reflection loss). DETAILED DESCRIPTION

[0026] The present invention provides a method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres, comprising the following steps:

[0027] (1) mixing microcrystalline cellulose, water and a triazine compound and reacting them to obtain binary microspheres;

[0028] (2) mixing the ferromagnetic material, water and the binary microspheres and reacting them to obtain the ternary microspheres;

[0029] (3) Carbonizing the ternary microspheres under a protective atmosphere to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

[0030] In the present invention, the microcrystalline cellulose and triazine compounds in step (1) are preferably purchased; the microcrystalline cellulose is preferably purchased from Shandong Qilu Biotechnology Group Co., Ltd.; the triazine compounds preferably include cyanuric acid and / or thiocyanuric acid; cyanuric acid and thiocyanuric acid are preferably purchased from Sinopharm Chemical Reagent Co., Ltd.

[0031] In the present invention, the mass ratio of microcrystalline cellulose, water and triazine compound in step (1) is preferably 2.5-10:40-80:1-5, more preferably 5-9.9:50-70:1.485-4, and more preferably 6-7:60-65:1.495-3.475.

[0032] In the present invention, in step (1), the main function of the microcrystalline cellulose is to provide a carbon source to form an inner shell of the sphere; the main function of the triazine compound is to provide a nitrogen source and a sulfur source to form an outer shell of the sphere.

[0033] In the present invention, when the mass fraction of the triazine compound is 1 to 5 parts, if the mass fraction of microcrystalline cellulose is less than 2.5 parts, the yield of the prepared binary microspheres is low; if the mass fraction of microcrystalline cellulose is more than 10 parts, the particle size of the prepared binary microspheres is large, the microspheres are sticky, and even broken; when the mass fraction of microcrystalline cellulose is 2.5 to 10 parts, if the mass fraction of the triazine compound is less than 1 part, the prepared binary microspheres cannot form a ball shell structure, and if the mass fraction of the triazine compound is more than 5 parts, the shell surface of the prepared binary microspheres is uneven.

[0034] In the present invention, the mixing in step (1) preferably comprises the following steps: dispersing microcrystalline cellulose in water, performing a first ultrasound, then adding a triazine compound, and performing a second ultrasound to obtain a mixed solution; the temperature of the first ultrasound is preferably 20-30°C, more preferably 22-28°C, and more preferably 25-26°C; the time of the first ultrasound is preferably 10-30min, more preferably 15-25min, and more preferably 18-20min; the temperature of the second ultrasound is preferably 20-30°C, more preferably 22-28°C, and more preferably 25-26°C; the time of the second ultrasound is preferably 10-30min, more preferably 15-25min, and more preferably 18-20min.

[0035] In the present invention, the reaction temperature in step (1) is preferably 180-220°C, more preferably 190-210°C, and more preferably 200-205°C; the reaction time is preferably 8-12h, more preferably 9-11h, and more preferably 9.5-10h.

[0036] In the present invention, in step (1), when the reaction time is 8 to 12 hours, if the reaction temperature is lower than 180°C, the prepared binary microspheres will not form balls; if the reaction temperature is higher than 220°C, the preparation process will be unsafe and equipment loss will increase; when the reaction temperature is 180 to 220°C, if the reaction time is shorter than 8 hours, the reaction will not proceed completely and binary microspheres cannot be prepared; if the reaction time is longer than 12 hours, the preparation time will be long and equipment loss will increase.

[0037] In the present invention, after the reaction in step (1) is completed, the obtained system is filtered to obtain a two-component solid sample; the two-component solid sample is washed and dried in sequence to obtain a binary microsphere; the washing preferably comprises the following steps: the two-component solid sample is alkali-washed to remove unreacted microcrystalline cellulose to obtain an alkali-washed solid sample, and then the alkali-washed solid sample is washed with water to remove unreacted triazine compounds to complete the washing; the reagent used for alkali washing is preferably sodium hydroxide solution, and the volume fraction of the sodium hydroxide solution is preferably 10-20%, more preferably 12-18%, and more preferably 15-16%; the number of alkali washings is preferably ≥2 times, more preferably ≥3 times, and more preferably ≥4 times; in a single alkali washing, The mass volume ratio of the two-component solid sample to the sodium hydroxide solution is preferably 1g:50-100mL, further preferably 1g:60-90mL, and more preferably 1g:70-80mL; the number of water washings is preferably ≥2 times, further preferably ≥3 times, and more preferably ≥4 times; in the case of a single water washing, the mass volume ratio of the solid sample after alkali washing to water is preferably 1g:50-100mL, further preferably 1g:60-90mL, and more preferably 1g:70-80mL; the drying temperature is preferably 50-60°C, further preferably 52-58°C, and more preferably 55-56°C; the drying time is preferably 12-24h, further preferably 16-20h, and more preferably 17-18h.

[0038] In the present invention, the ferromagnetic material in step (2) preferably includes one or more of ferric citrate, ferric acetylacetonate, ferrous gluconate and ferric phosphate, and ferric citrate, ferric acetylacetonate, ferrous gluconate and ferric phosphate are preferably purchased from Sinopharm Chemical Reagent Co., Ltd.

[0039] In the present invention, the mass ratio of the ferromagnetic substance, water and binary microspheres in step (2) is preferably 0.1-1:30-60:5-10, more preferably 0.2-0.8:40-50:6-9, and more preferably 0.5-0.6:45-47:7-8.

[0040] In the present invention, when the mass fraction of binary microspheres is 5 to 10 parts, if the mass fraction of ferromagnetic material is less than 0.1 parts, magnetism cannot be well introduced, and if the mass fraction of ferromagnetic material is higher than 1 parts, the density of the prepared ternary microspheres is large; when the mass fraction of ferromagnetic material is 0.1 to 1 parts, if the mass fraction of binary microspheres is less than 5 parts, the yield of the prepared ternary microspheres is low, and if the mass fraction of binary microspheres is higher than 10 parts, the prepared ternary microspheres are agglomerated.

[0041] In the present invention, the mixing in step (2) preferably comprises the following steps: dispersing the ferromagnetic material in water, performing a first ultrasound, then adding the binary microspheres, and performing a second ultrasound to obtain a mixed solution; the temperature of the first ultrasound is preferably 20-30°C, more preferably 22-28°C, and more preferably 25-26°C; the time of the first ultrasound is preferably 20-60min, more preferably 30-50min, and more preferably 40-45min; the temperature of the second ultrasound is preferably 20-30°C, more preferably 22-28°C, and more preferably 25-26°C; the time of the second ultrasound is preferably 20-60min, more preferably 30-50min, and more preferably 40-45min.

[0042] In the present invention, the reaction temperature in step (2) is preferably 180-220°C, more preferably 190-210°C, and more preferably 200-205°C; the reaction time is preferably 8-12h, more preferably 9-11h, and more preferably 9.5-10h.

[0043] In the present invention, in step (2), when the reaction time is 8 to 12 hours, if the reaction temperature is lower than 180°C, ternary microspheres cannot be prepared; if the reaction temperature is higher than 220°C, the preparation process is unsafe and equipment loss increases; when the reaction temperature is 180 to 220°C, if the reaction time is shorter than 8 hours, the reaction is not thorough; if the reaction time is longer than 12 hours, the preparation time is long and equipment loss increases.

[0044] In the present invention, after the reaction of step (2) is completed, the obtained system is filtered to obtain a three-component solid sample; the three-component solid sample is washed and dried in sequence to obtain a ternary microsphere; the washing preferably comprises the following steps: the three-component solid sample is washed with alcohol to remove unreacted binary microspheres to obtain an alcohol-washed solid sample, and then the alcohol-washed solid sample is washed with water to remove unreacted ferromagnetic substances to complete the washing; the reagent used for alcohol washing is preferably an ethanol solution, and the volume fraction of the ethanol solution is preferably 10-20%, more preferably 12-18%, and more preferably 15-16%; the number of alcohol washings is preferably ≥2 times, more preferably ≥3 times, and more preferably ≥4 times; in a single alcohol washing, the three groups The mass volume ratio of the solid sample to the ethanol solution is preferably 1g:50-100mL, further preferably 1g:60-90mL, more preferably 1g:70-80mL; the number of water washings is preferably ≥2 times, further preferably ≥3 times, more preferably ≥4 times; in a single water washing, the mass volume ratio of the solid sample after alcohol washing to water is preferably 1g:50-100mL, further preferably 1g:60-90mL, more preferably 1g:70-80mL; the drying temperature is preferably 50-60°C, further preferably 52-58°C, more preferably 55-56°C; the drying time is preferably 12-24h, further preferably 16-20h, more preferably 17-18h.

[0045] In the present invention, the protective atmosphere in step (3) is preferably nitrogen or argon, and the gas flow rate of the protective atmosphere is preferably 200-300 mg / L, more preferably 220-280 mg / L, and more preferably 250-260 mg / L; the purpose of using the protective atmosphere is to maintain the stability of the sample structure.

[0046] In the present invention, the heating rate of the carbonization in step (3) is preferably 2-5°C / min, more preferably 3-4°C / min, and more preferably 3.5°C / min; the target temperature of the carbonization is preferably 700-900°C, more preferably 750-850°C, and more preferably 800°C; the holding time to reach the target temperature is preferably 1.5-2.5h, more preferably 1.7-2.3h, and more preferably 2h. The purpose of carbonization is to obtain N, S, and Fe co-doped microcrystalline cellulose carbon microspheres during the pyrolysis and carbonization process.

[0047] In the present invention, when the target temperature of carbonization and the holding time to reach the target temperature are within the described range, if the heating rate is lower than 2°C / min, nitrogen or argon will be wasted; if the heating rate is higher than 5°C / min, the structure may be destroyed; when the target temperature of carbonization and the heating rate are within the described range, if the holding time is shorter than 1.5h, sufficient pyrolysis and carbonization cannot be achieved; if the holding time is longer than 2.5h, nitrogen or argon will be wasted.

[0048] In the present invention, after the carbonization in step (3) is completed, the carbonization is naturally cooled to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres; the target temperature of the natural cooling is preferably ≤40°C, more preferably ≤35°C, and more preferably ≤30°C.

[0049] The present invention also provides N, S, Fe co-doped microcrystalline cellulose carbon microspheres prepared by the preparation method of the N, S, Fe co-doped microcrystalline cellulose carbon microspheres. The structure of the N, S, Fe co-doped microcrystalline cellulose carbon microspheres is a double-layer core-shell structure. The diameter of the N, S, Fe co-doped microcrystalline cellulose carbon microspheres is preferably 2 to 6 μm, further preferably 3 to 5 μm, and more preferably 4 μm.

[0050] The present invention also provides the application of the N, S and Fe co-doped microcrystalline cellulose carbon microspheres in electromagnetic wave absorption.

[0051] In the present invention, the absorption rate of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres to electromagnetic waves in the frequency band of 2 to 18 GHz is preferably ≥99%, more preferably ≥99.3%, and even more preferably ≥99.6%.

[0052] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0053] Example 1

[0054] 9.9 parts by mass of microcrystalline cellulose were dispersed in 80 parts by mass of water, and ultrasonicated at 25°C for 30 minutes, and then 1.485 parts by mass of cyanuric acid were added, and ultrasonicated at 25°C for 30 minutes to obtain a mixed solution, and the mixed solution was transferred to a polytetrafluoroethylene-lined reactor, and reacted in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours. After the reaction, the obtained system was filtered to obtain a two-component solid sample, and the two-component solid sample was alkali-washed with a sodium hydroxide solution with a volume fraction of 20% (the number of alkali washings was 4 times, and the mass volume ratio of the two-component solid sample to the sodium hydroxide solution was 1g:100mL for a single alkali washing) to obtain an alkali-washed solid sample, and then the alkali-washed solid sample was washed with water (the number of water washings was 4 times, and the mass volume ratio of the alkali-washed solid sample to water was 1g:100mL for a single water washing), and finally dried in an oven at 55°C for 20 hours to obtain binary microspheres;

[0055] Disperse 0.2 parts by mass of ferric acetylacetonate in 30 parts by mass of water, ultrasonicate for 20 minutes at 25°C, then add 10 parts by mass of binary microspheres, continue ultrasonicate for 30 minutes at 25°C to obtain a mixed solution, transfer the mixed solution to a polytetrafluoroethylene-lined reactor, react in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours, and after the reaction, filter the obtained system to obtain a three-component solid sample; wash the three-component solid sample with an ethanol solution with a volume fraction of 20% (the number of alcohol washings is 4 times, and the mass volume ratio of the three-component solid sample to the sodium hydroxide solution is 1g:100mL for a single alcohol washing) to obtain an alcohol-washed solid sample, and then wash the alcohol-washed solid sample with water (the number of water washings is 4 times, and the mass volume ratio of the alcohol-washed solid sample to water is 1g:100mL for a single water washing), and finally dry it in an oven at 55°C for 17 hours to obtain a ternary microsphere;

[0056] The ternary microspheres contained in the crucible were placed in a vacuum tube furnace filled with argon (the gas flow rate of argon was 300 mg / L), heated to 800°C at a heating rate of 4°C / min, and kept at 800°C for 1.5 hours for carbonization. After the carbonization was completed, they were naturally cooled to 25°C to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

[0057] Example 2

[0058] Disperse 5 parts by mass of microcrystalline cellulose in 60 parts by mass of water, ultrasonicate for 30 minutes at 25°C, then add 1.495 parts by mass of cyanuric acid, and continue ultrasonicate for 30 minutes at 25°C to obtain a mixed solution, transfer the mixed solution to a polytetrafluoroethylene-lined reactor, and react in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours. After the reaction, filter the obtained system to obtain a two-component solid sample, and wash the two-component solid sample with a sodium hydroxide solution with a volume fraction of 20% (the number of alkali washings is 4 times, and the mass volume ratio of the two-component solid sample to the sodium hydroxide solution is 1g:100mL for a single alkali washing) to obtain an alkali-washed solid sample, and then wash the alkali-washed solid sample with water (the number of water washings is 4 times, and the mass volume ratio of the alkali-washed solid sample to water is 1g:100mL for a single water washing), and finally dry it in an oven at 55°C for 18 hours to obtain binary microspheres;

[0059] Disperse 0.1 parts by mass of ferric citrate in 30 parts by mass of water, ultrasonicate for 20 minutes at 25°C, then add 6 parts by mass of binary microspheres, continue ultrasonicate for 30 minutes at 25°C to obtain a mixed solution, transfer the mixed solution to a polytetrafluoroethylene-lined reactor, react in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours, and after the reaction, filter the obtained system to obtain a three-component solid sample; wash the three-component solid sample with an ethanol solution with a volume fraction of 20% (the number of alcohol washings is 4 times, and the mass volume ratio of the three-component solid sample to the sodium hydroxide solution is 1g:100mL for a single alcohol washing) to obtain an alcohol-washed solid sample, and then wash the alcohol-washed solid sample with water (the number of water washings is 4 times, and the mass volume ratio of the alcohol-washed solid sample to water is 1g:100mL for a single water washing), and finally dry it in an oven at 55°C for 17 hours to obtain a ternary microsphere;

[0060] The ternary microspheres contained in the crucible were placed in a vacuum tube furnace filled with argon (the gas flow rate of argon was 220 mg / L), heated to 800°C at a heating rate of 2°C / min, and kept at 800°C for 1.5 hours for carbonization. After the carbonization was completed, they were naturally cooled to 25°C to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

[0061] Example 3

[0062] 6 parts by mass of microcrystalline cellulose were dispersed in 60 parts by mass of water, and ultrasonicated at 25°C for 30 minutes, and then 3.475 parts by mass of thiocyanuric acid were added, and ultrasonicated at 25°C for 30 minutes to obtain a mixed solution, and the mixed solution was transferred to a polytetrafluoroethylene-lined reactor, and reacted in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours. After the reaction, the obtained system was filtered to obtain a two-component solid sample, and the two-component solid sample was alkali-washed with a sodium hydroxide solution with a volume fraction of 20% (the number of alkali washings was 4 times, and the mass volume ratio of the two-component solid sample to the sodium hydroxide solution was 1g:100mL for a single alkali washing) to obtain an alkali-washed solid sample, and then the alkali-washed solid sample was washed with water (the number of water washings was 4 times, and the mass volume ratio of the alkali-washed solid sample to water was 1g:100mL for a single water washing), and finally dried in an oven at 55°C for 16 hours to obtain binary microspheres;

[0063] Disperse 0.6 parts by mass of ferric acetylacetonate in 60 parts by mass of water, ultrasonicate for 20 minutes at 25°C, then add 6 parts by mass of binary microspheres, continue ultrasonicate for 30 minutes at 25°C to obtain a mixed solution, transfer the mixed solution to a polytetrafluoroethylene-lined reactor, react in an electric constant temperature blast drying oven at a temperature of 200°C for 11 hours, and after the reaction, filter the obtained system to obtain a three-component solid sample; wash the three-component solid sample with an ethanol solution with a volume fraction of 20% (the number of alcohol washings is 4 times, and the mass volume ratio of the three-component solid sample to the sodium hydroxide solution is 1g:100mL for a single alcohol washing) to obtain an alcohol-washed solid sample, and then wash the alcohol-washed solid sample with water (the number of water washings is 4 times, and the mass volume ratio of the alcohol-washed solid sample to water is 1g:100mL for a single water washing), and finally dry it in an oven at 55°C for 17 hours to obtain a ternary microsphere;

[0064] The ternary microspheres contained in the crucible were placed in a vacuum tube furnace filled with nitrogen (the gas flow rate of nitrogen was 250 mg / L), heated to 800°C at a heating rate of 2°C / min, and kept at 800°C for 2 hours for carbonization. After the carbonization, they were naturally cooled to 25°C to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

[0065] The N, S, and Fe co-doped microcrystalline cellulose carbon microspheres prepared in Examples 1 to 3 were analyzed and characterized by electron microscopy under conventional conditions using a scanning electron microscope sold by Japan HITACHI Company under the trade name S 4800 scanning electron microscope, and scanning electron microscope characterization images of the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Examples 1 to 3 were obtained, as shown in FIG. Figure 1 As shown; Figure 1 In the figure, a is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 1, b is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 2, and c is a scanning electron microscope characterization image of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 3. Figure 1 It can be seen that the shape of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres is regular spheres, but a small amount of irregular small-sized microspheres are also produced during the solvothermal reaction.

[0066] The N, S, and Fe co-doped microcrystalline cellulose carbon microspheres prepared in Example 1 were uniformly mixed with paraffin in a weight ratio of 1:5, and the mixture was pressed into concentric ring samples with an inner diameter of 3.04 mm, an outer diameter of 7.0 mm, and a thickness of 2.0 mm using a mold sold by Tianjin Jinfulun Technology Co., Ltd. under the trade name of XYM-H ring precision mold. A dual-port vector network analyzer sold by Agilent under the trade name of PNA Network Analyzer N5224A was used to test the electromagnetic performance parameters of the concentric ring samples at room temperature, and the reflection loss of the concentric ring samples in the frequency range of 2 to 18 GHz was calculated by transmission line theory. To ensure the accuracy of the test results, the front and back sides of the concentric ring samples were tested 3 times, and the average value was taken. At the same time, the electromagnetic properties of the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres obtained in Examples 2 and 3 were tested by the same method, and the reflection loss diagram of the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 1 was obtained, as shown in FIG. Figure 2 As shown; the reflection loss diagram of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 2, as shown Figure 3 As shown; the reflection loss diagram of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 3, as shown Figure 4 As shown. Figures 2 to 4 It can be seen that the minimum reflection loss of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 1 is -50.29dB when the matching thickness is 5.54mm, and the corresponding effective bandwidth is 1.70GHz; the minimum reflection loss of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 2 is -42.74dB when the matching thickness is 5.0mm, and the corresponding effective bandwidth is 2.60GHz; the minimum reflection loss of N, S, and Fe co-doped microcrystalline cellulose carbon microspheres in Example 3 is -50.96dB when the matching thickness is 3.0mm, and the corresponding effective bandwidth is 4.72GHz. The above results show that the absorption rate of electromagnetic waves by N, S, and Fe co-doped microcrystalline cellulose carbon microspheres obtained in Examples 1 to 3 reaches 99%.

[0067] It can be seen from the above embodiments that the present invention provides a method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres, comprising the following steps: mixing microcrystalline cellulose, water, and triazine compounds, reacting to obtain binary microspheres; mixing ferromagnetic substances, water, and binary microspheres, reacting to obtain ternary microspheres; and carbonizing the ternary microspheres under a protective atmosphere to obtain N, S, and Fe co-doped microcrystalline cellulose carbon microspheres. The N, S, and Fe co-doped microcrystalline cellulose carbon microspheres prepared by the present invention contain C, N, O, S, and Fe elements, and have a diameter of about 2 to 6 μm. The carbon microspheres use a ball formed by polymerization of microcrystalline cellulose as the inner shell of the ball, and a triazine compound and a ferromagnetic substance as the outer shell of the ball. Due to the presence of multiple components, the polarization loss of the material can be increased, and due to the presence of the spherical structure, the interface loss of the material can be increased. Under the action of multiple loss mechanisms, the carbon microsphere absorbing material can achieve good impedance matching, and the attenuation capacity is improved, thereby enhancing the ability of the material to reflect electromagnetic waves.

[0068] The carbon-based material microcrystalline cellulose used in the present invention is not only rich in resources, low in cost and environmentally friendly. By modifying the single-component polymer sugar spheres with triazine compounds, N / NS atoms can form defects after carbonization, causing dipole polarization, and promoting the attenuation of electromagnetic waves; the introduction of ferromagnetic substances increases the magnetic loss, so that the absorber attenuates electromagnetic waves under the action of dielectric loss and magnetic loss; in addition, by modifying the single-component polymer sugar spheres and preparing them into a core-shell structure, multiple reflections of electromagnetic waves can be promoted, which is beneficial for the material to maximize the conversion of electromagnetic energy into heat energy. The carbon microspheres finally prepared have an absorption rate of up to 99% for electromagnetic waves.

[0069] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres, characterized in that: It includes the following steps: (1) mixing microcrystalline cellulose, water and a triazine compound and reacting them to obtain binary microspheres; (2) mixing the ferromagnetic material, water and the binary microspheres and reacting them to obtain the ternary microspheres; (3) Carbonizing the ternary microspheres under a protective atmosphere to obtain the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres.

2. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 1, characterized in that: The triazine compound in step (1) includes cyanuric acid and / or thiocyanuric acid.

3. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 1 or 2, characterized in that: The mass ratio of the microcrystalline cellulose, water and triazine compound in step (1) is 2.5-10:40-80:1-5.

4. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 3, characterized in that: The reaction temperature in step (1) is 180-220° C., and the reaction time is 8-12 hours.

5. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 4, characterized in that: The ferromagnetic material in step (2) includes one or more of ferric citrate, ferric acetylacetonate, ferrous gluconate and ferric phosphate.

6. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 5, characterized in that: The mass ratio of the ferromagnetic substance, water and binary microspheres in step (2) is 0.1-1:30-60:5-10.

7. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 6, characterized in that: The reaction temperature in step (2) is 180-220° C., and the reaction time is 8-12 hours.

8. The method for preparing N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 7, characterized in that: The protective atmosphere in step (3) is nitrogen or argon, and the gas flow rate of the protective atmosphere is 200-300 mg / L; The heating rate of the carbonization in step (3) is 2-5°C / min, the target temperature of the carbonization is 700-900°C, and the insulation time to reach the target temperature is 1.5-2.5h.

9. N, S, Fe co-doped microcrystalline cellulose carbon microspheres prepared by the method for preparing N, S, Fe co-doped microcrystalline cellulose carbon microspheres according to any one of claims 1 to 8.

10. Use of the N, S, and Fe co-doped microcrystalline cellulose carbon microspheres according to claim 9 in electromagnetic wave absorption.

Citation Information

Patent Citations

  • Hydrothermal preparation method of magnetic carbon micro-spheres

    CN104437362A

  • Method for preparing carbon microsphere adsorbent under catalysis of metal salt with low-temperature hydrothermal method

    CN105582888A

  • Nitrogen and oxygen element doped bowl-shaped hollow carbon microsphere and preparation method thereof

    CN115849336A

  • Preparation method of modified carbon-based wave-absorbing material

    CN116443848A

  • Application of biomass spherical carbon material as wave-absorbing material