BN nanowire-rGO composite electromagnetic wave absorbing material and preparation method and application thereof
Through a one-step composite method of melamine, boric acid and graphene oxide, BN nanowire-rGO composite material was prepared, which solved the electromagnetic parameter regulation and agglomeration of composite materials, achieved efficient electromagnetic wave absorption performance, simplified the process and reduced energy consumption .
Patent Information
- Application Number
- CN202411202634.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, there are problems such as difficult to regulate electromagnetic parameters, complex composite methods, and rGO agglomeration in the preparation process of BN and rGO composite materials, which limit their promotion and optimization in electromagnetic wave absorption and other applications.
By using the one-step composite method of melamine and boric acid and graphene oxide, the mass ratio of melamine to boric acid and the concentration of graphene oxide aqueous solution, and after freeze-drying and calcining, BN nanowire-rGO composite material is prepared to form a stem-leaf structure. To improve electromagnetic wave absorption performance.
The precise regulation of the electromagnetic parameters of composite materials is achieved, which significantly improves its electromagnetic wave absorption performance, simplifies the preparation process, reduces energy consumption, and avoids the generation of impurities, providing efficient electromagnetic wave absorption materials.
Smart Images

Figure CN119095360A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electromagnetic wave absorbing materials, and specifically relates to a BN nanowire-rGO composite electromagnetic wave absorbing material and a preparation method and application thereof. Background Art
[0002] Traditional absorbing materials such as ferrites have disadvantages such as a single loss mechanism, high density, high temperature resistance and easy oxidation. They are difficult to meet people's basic requirements for electromagnetic wave absorbers with thin microwave absorption coatings, effective absorption bandwidth, light weight and high absorption intensity. Therefore, it is particularly important to prepare high-efficiency electromagnetic absorbing materials with the characteristics of strong, light, wide and thin.
[0003] Boron nitride (BN), as a graphene-like material, has almost the same lattice parameters as graphene and similar properties, such as low density, high mechanical strength, good chemical corrosion resistance, good oxidation resistance, good lubricity, good thermal conductivity, etc. Moreover, BN has excellent resistivity (10 -16 ~10 -18 Ω·cm) and wide band gap (6.0eV) can be used to adjust the dielectric properties and impedance matching properties of carbon materials and improve the electromagnetic wave absorption performance of carbon materials. At the same time, graphene (rGO) is considered to be a promising electromagnetic wave absorber material due to its light weight, good chemical stability, excellent conductivity and strong dielectric loss performance. However, impedance mismatch and a single attenuation mechanism severely limit the widespread application of rGO.
[0004] So far, many preparation methods of step-by-step composites of rGO and other materials have been reported. For example, Yuan et al. wrapped vanadium nitride nanowires in reduced graphene oxide, and the prepared layered composite material showed excellent electromagnetic wave absorption performance. When filled with 15wt%, the minimum reflection value was -41.5dB at a thickness of 1.5mm, and the effective absorption bandwidth was 3.9GHz. Chang et al. prepared La attached to rGO sheets by electrostatic adsorption. 0.8 CoO3 particles, due to the generation of magnetic loss and dielectric loss, improve their electromagnetic wave absorption performance. There are few reports on the preparation of BN and rGO composite materials. Especially in the process of combining these two materials to form a composite material, there are problems such as difficulty in controlling electromagnetic parameters, complex composite methods, and rGO agglomeration. These problems limit the further promotion and optimization of BN and rGO composites in electromagnetic wave absorption and other potential applications. Therefore, exploring a simpler composite preparation process and achieving precise control of the electromagnetic parameters of the composite material have become important directions of current research. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a BN nanowire-rGO composite electromagnetic wave absorption material and its preparation method and application in view of the deficiencies in the above-mentioned prior art. Boron nitride is synthesized by melamine and boric acid and then composited with graphene oxide in one step. This process is simple, easy to control, and energy-saving. The obtained BN nanowire-rGO has good composite and good electromagnetic wave absorption performance.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention discloses a method for preparing a BN nanowire-rGO composite material, comprising the following steps:
[0008] Melamine, boric acid and graphene aqueous solution are dissolved and mixed, and heated to obtain a dispersion; the dispersion is freeze-dried to obtain a precursor, the precursor is calcined under an inert atmosphere, and a BN nanowire-rGO composite material is obtained after cooling.
[0009] The mass ratio of melamine to boric acid is 1:(1-3), and the total mass of melamine and boric acid is 0.6-1.0 g.
[0010] The concentration of the graphene oxide aqueous solution is 1-5 mg / mL, and the added amount is 2.5-7.5 mL.
[0011] The heating is carried out in an oil bath with a temperature of 80-100°C.
[0012] The total heating time is 1 to 4 hours.
[0013] The freeze-drying time is 24 to 48 hours.
[0014] The calcination treatment temperature is 1000-1200° C., and the heating rate is 2-5° C. / min.
[0015] The inert atmosphere is N2 atmosphere.
[0016] The present invention also discloses a BN nanowire-rGO composite material prepared according to the above preparation method, wherein the microstructure of the BN nanowire-rGO composite material is a stem-leaf structure.
[0017] The invention also discloses the application of the BN nanowire-rGO composite material in the field of electromagnetic wave absorption.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention proposes a method for preparing a BN nanowire-rGO composite material with electromagnetic wave absorption performance, wherein the composite material is composited with graphene while synthesizing boron nitride, and the mass ratio of melamine and boric acid is controlled, the concentration of the graphene oxide aqueous solution is controlled, and a BN nanowire-rGO composite material with excellent electromagnetic wave absorption performance is prepared through one-step directional freeze drying and calcination. The composite material has a structural advantage that the one-dimensional structure and the two-dimensional structure are interlaced to build an internal conductive network, which is convenient for the internal migration and transition of electrons, effectively enhances the conductivity loss, and can effectively improve the agglomeration phenomenon of rGO. The multi-dimensional structure composite will effectively increase the interface area of the system, thereby significantly improving its interface loss performance. The BN nanowire-rGO composite material prepared by this method has broad application prospects in electromagnetic wave absorption, the prepared product is free of impurities, and the entire preparation process has simple steps, simple operation, and high repeatability.
[0020] Furthermore, the dosage of melamine and boric acid plays an important regulatory role in the synthesis of BN, and the appropriate ratio can synthesize linear BN without a template.
[0021] Furthermore, the problem of rGO agglomeration can be improved by adjusting the appropriate composite ratio.
[0022] Furthermore, the appropriate concentration of graphene oxide aqueous solution can adjust the composite ratio of rGO and BN, thereby effectively regulating the dielectric constant of the composite material, so that the composite material has better electromagnetic wave absorption performance.
[0023] Furthermore, suitable oil bath temperature and time can obtain BN nanowires with good shapes.
[0024] Furthermore, the gas raw material of the present invention is common experimental inert gas N2. The inert gas is used as a protective atmosphere in the experiment to avoid the introduction of impurities and the generation of oxides, so the purity of the product is relatively high.
[0025] The preparation method of a BN nanowire-rGO composite material proposed in the present invention is simple, easy to control, and energy-saving compared to the existing synthesis process, has good electromagnetic wave absorption performance, and has good application potential in the field of electromagnetic wave absorption.
[0026] The microstructure of the BN nanowire-rGO composite material prepared by the present invention is that BN and rGO are combined in a tight stem-leaf structure, which is crucial for the development of absorbing materials with high-efficiency electromagnetic wave absorption performance, because the structural design not only adjusts the dielectric constant of the system, but also extends the propagation path of the electromagnetic wave, thereby increasing the conductive loss and interface loss.
[0027] In summary, the method of the present invention has a simple process, and the prepared BN nanowires with heterogeneous interfaces can optimize the impedance matching problem of the composite material. The preparation process of the composite material is simple, easy to control, energy-saving and environmentally friendly, and the product has no other impurities generated, while showing excellent wave absorbing performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solution of the embodiment of the present invention, the following briefly introduces the drawings required for use in the embodiment:
[0029] Figure 1 This is a SEM image of the surface of the BN nanowire-rGO composite material prepared in Example 1;
[0030] Figure 2 This is a SEM image of the interior of the BN nanowire-rGO composite material prepared in Example 1;
[0031] Figure 3 The real part (a) and imaginary part (b) of the dielectric constant of the BN nanowire-rGO composite materials with different composite ratios prepared in Example 1, Example 4 and Example 5 as absorbers, respectively, where 2.5, 5 and 7.5 represent the addition amount of rGO aqueous solution of 2.5 mL, 5 mL and 7.5 mL, respectively;
[0032] Figure 4 Three-dimensional reflection loss diagrams of BN nanowire-rGO composite materials prepared in Example 1, Example 4 and Example 5 as absorbers rGO (a) BN / rGO-2.5 (b), BN / rGO-5 (c) and BN / rGO-7.5 (d) where 2.5, 5 and 7.5 represent the addition amount of rGO aqueous solution of 2.5 mL, 5 mL and 7.5 mL respectively;
[0033] Figure 5 The reflection loss of BN / rGO-5 at different thicknesses prepared in Example 1 of the present invention;
[0034] Figure 6 The effective absorption width of BN / rGO-5 prepared in Example 1 of the present invention at different thicknesses; DETAILED DESCRIPTION
[0035] The present invention provides a BN nanowire-rGO composite electromagnetic wave absorbing material and a preparation method thereof, comprising the following steps:
[0036] S1. Weigh melamine and boric acid in a certain mass ratio, mix the melamine and boric acid with a graphene aqueous solution, heat and stir in an oil bath for a certain period of time, and obtain a uniform dispersion A;
[0037] S2, pouring the dispersion A into a mold for directional freeze drying for a certain period of time;
[0038] S3. The dried product is calcined in a high-temperature tube furnace under a N2 atmosphere to obtain a BN nanowire-rGO composite material.
[0039] The microstructure of the BN nanowire-rGO composite material prepared by the above method is a stem-leaf structure and is used in the field of electromagnetic wave absorption.
[0040] In the dielectric property test, in order to detect the electromagnetic wave absorption performance of the BN nanowire-rGO composite material prepared by the present invention, the electromagnetic wave absorption performance analysis was performed using a vector network analyzer (MS 46322B) transmission line method. In order to study the microwave absorption performance of the material, it is first necessary to prepare a test sample (a ring with an inner diameter and an outer diameter of 3.04 mm and 7.00 mm, respectively) by uniformly mixing the BN nanowire-rGO composite material and paraffin in a certain mass ratio, and test the electromagnetic parameters of the sample in the frequency range of 2 to 18 GHz.
[0041] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. The components of the embodiments of the present invention described and shown in the drawings here can usually be arranged and designed in various different configurations. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents selected embodiments of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0042] In the following examples, unless otherwise specified, all materials used can be obtained through common channels; and the test methods adopted are conventional methods in the art.
[0043] Example 1
[0044] Weigh 0.8 g of melamine and boric acid in total with a mass ratio of 1:1.5, add 5 mL of 5 mg / mL graphene aqueous solution, dissolve the three in 15 mL of aqueous solution, and then stir magnetically in an oil bath at 90°C for 4 h to obtain a uniform dispersion A;
[0045] Pour dispersion A into a mold and freeze-dry for 48 h to obtain precursor B;
[0046] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1100°C at 2°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0047] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0048] The BN nanowire-rGO composite material SEM Figure 1 and Figure 2 As shown; the material has well-matched real and imaginary parts of the dielectric constant, such as Figure 3 As shown; the material has good electromagnetic wave absorption performance, such as Figure 4 As shown in the figure, the material has good minimum reflection loss. When the thickness is 3.50mm, the minimum reflection loss reaches -44.7dB. Figure 5 As shown; the material has a good effective absorption width, such as Figure 6 As shown, the effective absorption width reaches 5.52 GHz at a thickness of 2.05 mm.
[0049] Example 2
[0050] Weigh 0.6 g of melamine and boric acid in a total weight ratio of 1:1, add 5 mL of 2 mg / mL graphene aqueous solution, dissolve the three in 15 mL of aqueous solution, and then stir magnetically in an oil bath at 80°C for 2 h to obtain a uniform dispersion A;
[0051] Pour dispersion A into a mold and freeze-dry for 24 h to obtain precursor B;
[0052] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1100°C at 3°C / min, kept at that temperature for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0053] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0054] Example 3
[0055] Weigh 1.0 g of melamine and boric acid in a mass ratio of 1:2, add 5 mL of 3 mg / mL graphene aqueous solution, dissolve the three in 15 mL of aqueous solution, and then stir magnetically in an oil bath at 100 °C for 3 h to obtain a uniform dispersion A;
[0056] Pour dispersion A into a mold and freeze-dry for 48 h to obtain precursor B;
[0057] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1200°C at 4°C / min, kept warm for 2 hours, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0058] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0059] Example 4
[0060] Weigh 0.7 g of melamine and boric acid in a total weight ratio of 1:1.5, add 7.5 mL of 1 mg / mL graphene aqueous solution, dissolve the three in 12.5 mL of aqueous solution, and then stir magnetically in an oil bath at 80°C for 3 h to obtain a uniform dispersion A;
[0061] Pour dispersion A into a mold and freeze-dry for 40 h to obtain precursor B;
[0062] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1200°C at 5°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0063] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0064] Example 5
[0065] Weigh 0.8 g of melamine and boric acid in a total weight ratio of 1:3, add 2.5 mL of 2 mg / mL graphene aqueous solution, dissolve the three in 17.5 mL of aqueous solution, and then stir magnetically in an oil bath at 90°C for 4 h to obtain a uniform dispersion A;
[0066] Pour dispersion A into a mold and freeze-dry for 24 h to obtain precursor B;
[0067] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1200°C at 5°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0068] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0069] Example 6
[0070] Weigh 0.7 g of melamine and boric acid in a total weight ratio of 1:2.5, add 7.5 mL of 3 mg / mL graphene aqueous solution, dissolve the three in 12.5 mL of aqueous solution, and then stir magnetically in an oil bath at 100°C for 2 h to obtain a uniform dispersion A;
[0071] Pour dispersion A into a mold and freeze-dry for 40 h to obtain precursor B;
[0072] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1100°C at 4°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0073] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0074] Example 7
[0075] Weigh 1.0 g of melamine and boric acid in a mass ratio of 1:3, add 5 mL of 1 mg / mL graphene aqueous solution, dissolve the three in 15 mL of aqueous solution, and then stir magnetically in an oil bath at 100°C for 1 h to obtain a uniform dispersion A;
[0076] Pour dispersion A into a mold and freeze-dry for 24 h to obtain precursor B;
[0077] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1000°C at 3°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0078] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0079] Example 8
[0080] Weigh 0.6 g of melamine and boric acid in a total weight ratio of 1:1, add 5 mL of 3 mg / mL graphene aqueous solution, dissolve the three in 15 mL of aqueous solution, and then stir magnetically in an oil bath at 90°C for 2 h to obtain a uniform dispersion A;
[0081] Pour dispersion A into a mold and freeze-dry for 30 h to obtain precursor B;
[0082] The obtained precursor B was placed in a sealed crucible, protected by flowing N2 in a high-temperature tube furnace, heated to 1100°C at 5°C / min, kept warm for 2h, and then naturally cooled to room temperature to obtain a BN nanowire-rGO composite material.
[0083] The composite material was used as a wave absorber and paraffin to prepare a 5wt% annular sample for dielectric property testing.
[0084] In order to detect the electromagnetic wave absorption performance of the BN nanowire-rGO composite material prepared in the present invention, the dielectric performance thereof is evaluated. The dielectric performance test is performed using a vector network analyzer (MS 46322B) for analysis.
[0085] See also Figure 1 and Figure 2 , it can be seen that the BN-rGO composite material is well composited, and BN grows evenly on the surface and inside of graphene, presenting a good stem-leaf structure.
[0086] See also Figure 3 , which is the relative frequency diagram of the real and imaginary parts of the dielectric constant of the composite material, it can be seen that the addition of BN can effectively reduce the dielectric constant of reduced graphene oxide, so that the real part of the dielectric constant and the imaginary part of the dielectric constant achieve a good match. At the same time, as the amount of rGO added increases, the corresponding real and imaginary parts both increase, proving that the adjustment of the composite ratio of rGO and BN has a positive effect on the electromagnetic wave absorption performance.
[0087] See also Figure 4 , as the three-dimensional reflection loss diagram of the absorbing material, the corresponding loss diagram can see the minimum reflection loss (RL min )At the corresponding composite ratio, the minimum reflection loss of BN / rGO-5 is more than 4 times that of rGO.
[0088] See also Figure 5 and Figure 6 ,It can be seen that the effective absorption width of BN / rGO-5 is significantly improved, and ,the full coverage of Ku, X, and C bands, as well as most of the ,coverage of the S band can be achieved at different thicknesses.
[0089] In summary, the present invention provides a method for preparing and applying a BN nanowire-rGO electromagnetic wave absorbing material, wherein melamine powder and boric acid are uniformly mixed in a certain mass ratio, and then dissolved in a graphene aqueous solution; the solution is freeze-dried and heat-treated in an inert atmosphere to obtain a BN nanowire-rGO composite material, and the composite ratio of BN and rGO is adjusted to adjust the dielectric real and imaginary values of the composite material to achieve optimal impedance matching, and a microwave absorbing material with good performance is prepared by a simple process. The method of the present invention is simple and easy to control, and the obtained BN nanowire-rGO composite material has no other impurities generated, and can be suitable for large-scale production, and has good electromagnetic wave absorption performance.
[0090] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a BN nanowire-rGO composite material, characterized in that: The following steps are involved: Melamine, boric acid and graphene aqueous solution are dissolved and mixed, and heated to obtain a dispersion; the dispersion is freeze-dried to obtain a precursor, the precursor is calcined under an inert atmosphere, and a BN nanowire-rGO composite material is obtained after cooling.
2. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The mass ratio of melamine to boric acid is 1:(1-3), and the total mass of melamine and boric acid is 0.6-1.0 g.
3. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The concentration of the graphene oxide aqueous solution is 1-5 mg / mL, and the added amount is 2.5-7.5 mL.
4. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The heating is carried out in an oil bath with a temperature of 80-100°C.
5. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The total heating time is 1 to 4 hours.
6. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The freeze-drying time is 24 to 48 hours.
7. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The calcination treatment temperature is 1000-1200° C., and the heating rate is 2-5° C. / min.
8. The method for preparing a BN nanowire-rGO composite material according to claim 1, characterized in that: The inert atmosphere is N2 atmosphere.
9. A BN nanowire-rGO composite material prepared according to the preparation method according to any one of claims 1 to 8, characterized in that: The microstructure of the BN nanowire-rGO composite material is a stem-leaf structure.
10. Use of the BN nanowire-rGO composite material according to claim 9 in the field of electromagnetic wave absorption.