Lead-carbon battery and preparation method of bagasse-based hard carbon negative electrode active material of lead-carbon battery

The bagasse-based hardcarbon material was prepared by carbonizing and acid treatment, and combining chemical reduction and deposition technology, which solved the problems of irreversible sulfation and hydrogen evolution reaction of lead-acid battery negative electrodes, significantly improving the electrochemical performance of lead-carbon battery and Capacity retention rate.

CN119079976APending Publication Date: 2024-12-06GUANGXI UNIVERSITY OF TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411225088.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The negative electrode of traditional lead-acid batteries has problems with irreversible sulfation and hydrogen evolution reaction, which leads to a decline in battery performance and is difficult to meet the requirements of partially charged recycling modes of batteries in energy storage scenarios.

Method used

The preparation method of bagasse-based hardcoat negative electrode active material is adopted. By carbonizing and acidizing the bagasse, and combining with chemical reduction and deposition technology, bagasse-based hardcoat material containing nanometal particles is prepared, and the structure of the material is improved in a coordinated manner. Electrochemical properties.

Benefits of technology

It significantly improves the electrochemical performance of lead-carbon batteries, reduces hydrogen evolution and sulfurization reactions, improves conductivity and capacity retention, and adapts to the application requirements of lead-carbon batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119079976A_ABST
    Figure CN119079976A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of lead batteries, and particularly relates to a preparation method of a bagasse-based hard carbon negative electrode active material for a lead-carbon battery, which comprises the following steps: carbonizing bagasse, and carrying out acid treatment to obtain bagasse carbon; the bagasse carbon, a metal M source and a reducing agent are subjected to chemical reduction deposition, and the bagasse-based hard carbon negative electrode active material is prepared. The metal M source is a water-soluble salt containing a metal M element, and the metal M element comprises at least one of antimony, lead and bismuth; and the reducing agent is a component capable of reducing a metal M source into a metal M simple substance. The invention also comprises the negative electrode active material prepared by the preparation method and application of the negative electrode active material in the lead-carbon battery. The material prepared by the preparation method disclosed by the invention can meet the lead-carbon application requirements, can solve the problems of hydrogen evolution, sulfation, impedance and the like of the lead-carbon battery, and can remarkably improve the performance of the lead-carbon battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lead-carbon materials, and in particular relates to the technical field of carbon additives for lead-carbon batteries. Background Art

[0002] Due to the development of the automobile industry and the electric bicycle industry, the lead-acid battery and lead smelting industry have developed rapidly in the past few decades. If the nearly 60 million tons of lead in various lead alloys and lead-acid batteries in society are not controlled, the harm to the whole society will be immeasurable. Such a huge amount of lead can only be metabolized in a controllable industrial system so that lead can continue to serve mankind and ensure that the harm coefficient of lead to mankind is minimized. Sullivan conducted a life cycle assessment of lead-acid batteries, nickel-cadmium batteries, nickel-hydrogen batteries, sodium-sulfur batteries and lithium-ion batteries and believed that lead-acid batteries have the lowest production energy consumption and the lowest CO2 and pollutant emissions. Deaniel et al. constructed a life cycle assessment of the lead-acid battery recycling process and concluded that lead-acid batteries are recycled by recycled lead, which is significantly better than the impact of lead-acid battery landfill disposal on the environment in terms of resource consumption, atmospheric pollutant emissions, wastewater and solid waste emissions. In China, the lead utilization rate of the lead-acid battery industry and the lead recovery rate of the recycled lead industry have been greatly improved in this century. Therefore, as one of the most widely used commercial power sources, lead-acid batteries have the advantages of good safety, mature industrial technology, simple assembly technology, and strong recyclability, and there is still much room for development in the energy storage market.

[0003] Traditional lead-acid batteries have the problem of irreversible sulfation of the negative electrode, and cannot meet the requirements of the partial charge state cycle use mode of the battery in energy storage scenarios. Since the 1990s, ALABC has organized lead-acid battery companies and research institutions to jointly develop a new generation of lead-acid batteries that meet the requirements of energy storage applications. Hu Xinguo called this new generation of lead-acid batteries with carbon materials added to the negative electrode the third generation of lead-acid batteries - lead-carbon batteries. The national standard GRIT3620O-2018 defines this type of battery with lead dioxide as the positive electrode, lead-carbon composite electrode as the negative electrode, and sulfuric acid solution as the electrolyte as a lead-carbon battery.

[0004] The selection of carbon additives is crucial to the performance of lead-carbon batteries. Pure carbon additives are prone to cause severe hydrogen evolution reactions, resulting in rapid capacity decay of the battery, which is not conducive to the performance of lead-carbon batteries. Summary of the invention

[0005] In view of the problems faced by lead-carbon active materials, such as easy hydrogen evolution, large material impedance, and unsatisfactory electrochemical performance, the present invention provides a method for preparing a bagasse-based hard carbon negative electrode active material that is adapted to the application requirements of lead-carbon batteries, aiming to solve the problems faced by lead-carbon battery applications and improve the adaptability of the material in lead-carbon batteries.

[0006] The second object of the present invention is to provide a bagasse-based hard carbon negative electrode active material prepared by the preparation method and its application in a lead-carbon battery.

[0007] The third object of the present invention is to provide a lead-carbon battery comprising the bagasse-based hard carbon negative electrode active material, and its negative electrode and negative electrode material.

[0008] Different from other battery systems, the negative electrode of the lead-carbon battery has serious problems of hydrogen evolution and sulfation. Although there are some improvement methods in the prior art to address this problem, these methods will further cause new problems such as impedance, making it difficult for the material to meet the requirements of low hydrogen evolution, low sulfation and low impedance required by the lead-carbon battery. In view of this problem, the present invention has provided the following improvement scheme after in-depth research, specifically:

[0009] A method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery, wherein bagasse is carbonized and acid-treated to obtain bagasse carbon;

[0010] The bagasse charcoal, metal M source and reducing agent are subjected to chemical reduction deposition to obtain the bagasse-based hard carbon negative electrode active material;

[0011] The metal M source is a water-soluble salt containing a metal M element, and the metal M element includes at least one of antimony, lead, and bismuth;

[0012] The reducing agent is a component that can reduce the metal M source to a single metal M.

[0013] In response to the problems faced by lead-carbon batteries, the present invention innovatively uses bagasse as raw material, carbonizes and acid-treats it, and cooperates with chemical reduction deposition to induce dispersed deposition of metal M nanoparticles. This can unexpectedly achieve synergy, adapt to lead-carbon application requirements, solve the problems of hydrogen evolution, sulfation, impedance, etc. faced by lead-carbon batteries, and can significantly improve the performance of lead-carbon batteries.

[0014] In the present invention, the combination of the physicochemical characteristics of the bagasse and the chemical reduction deposition process of the metal M is the key to synergistically improving the adaptability of the lead-carbon battery. Studies have shown that the physicochemical structure of bagasse can adapt to the application of lead-carbon. In addition, it is also helpful to synergistically combine with the chemical reduction deposition to induce the chemical reduction deposition of metal M, improve its particle size, dispersion distribution state, exposure behavior of active sites and structural stability, and then through a dual mechanism, synergistically improve the adaptability of the material to lead-carbon and improve the performance of the lead-carbon battery.

[0015] In the present invention, the bagasse is subjected to ball milling treatment before carbonization; wherein the ball milling time is 0.5 to 3 hours;

[0016] In the present invention, the atmosphere in the carbonization stage is an oxygen-free or low-oxygen atmosphere; preferably at least one of nitrogen and an inert gas;

[0017] In the present invention, the carbonization temperature is 600 to 1000°C, more preferably 850 to 950°C, and even more preferably 880 to 920°C.

[0018] In the present invention, the carbonization time is 1-3h.

[0019] In the present invention, the carbonized product is placed in an acid solution for acid treatment;

[0020] In the present invention, the acid solution is an aqueous solution of an inorganic acid;

[0021] In the present invention, the solute concentration of the inorganic acid in the acid solution is 0.5 to 3 M, and can further be 1.5 to 2.5 M;

[0022] In the present invention, the acid treatment time is 1 to 48 hours, and further can be 20 to 30 hours.

[0023] In the present invention, the molar weight ratio of the metal M source to the bagasse carbon is 1-5 mmol / g, preferably 2-3 mmol / g. That is, 1-5 mmol of the metal M source is used per gram of bagasse hard carbon.

[0024] In the present invention, the concentration of the metal M source in the starting solution of chemical reduction deposition is 0.02-0.05M.

[0025] In the present invention, the reducing agent is at least one of NaBH4, Ar / H2 mixed gas and hydrazine hydrate.

[0026] In the present invention, the reducing agent is not less than the theoretical molar amount for completely reducing the metal M source, and can be 1 to 10 times the theoretical molar amount in consideration of the cost.

[0027] In the present invention, the temperature of the chemical reduction deposition stage is 0 to 50° C., and considering the convenience of operation, it can be further room temperature, for example, 20 to 40° C.;

[0028] Preferably, the chemical reduction deposition time is 15 to 60 minutes, and further can be 30 to 40 minutes.

[0029] The present invention also provides a bagasse-based hard carbon negative electrode active material prepared by the preparation method; the material comprises bagasse carbon and nano-metal M particles chemically deposited on the surface of the carbon.

[0030] The preparation method of the present invention can give the prepared material the characteristics of high hydrogen evolution potential and high electrical conductivity, and the material prepared by the preparation method can unexpectedly adapt to the application characteristics of lead-carbon batteries and can improve the electrochemical performance of lead-carbon batteries.

[0031] The present invention also provides a negative electrode material for a lead-carbon battery, comprising a negative electrode active material, wherein the negative electrode active material comprises a bagasse-based hard carbon negative electrode active material prepared by the preparation method of the present invention;

[0032] Preferably, the negative electrode material further comprises a conductive agent and a binder.

[0033] In the present invention, in the negative electrode material, except for the bagasse-based hard carbon negative electrode active material prepared by the preparation method of the present invention, the other components, contents and occurrence structure relationships of the components can be conventional.

[0034] The present invention also provides a negative electrode for a lead-carbon battery, comprising a current collector and a negative electrode material composited on the surface of the current collector, wherein the negative electrode material is the negative electrode material of the present invention.

[0035] The present invention also provides a lead-carbon battery, which comprises the negative electrode described in the present invention.

[0036] The lead-carbon battery of the present invention, except for the bagasse-based hard carbon negative electrode active material, other components, contents and structural occurrence relationships can be conventional.

[0037] Beneficial effects:

[0038] The present invention innovatively combines the chemical reduction deposition process of bagasse and metal M, thereby achieving synergy of physical and chemical characteristics, thus unexpectedly making it adaptable to the application requirements of lead-carbon batteries, solving the problems of hydrogen evolution, irreversible lead sulfation, impedance, etc. of lead-carbon batteries, and effectively improving the performance of lead-carbon batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The SEM morphology of the SBHC prepared in step 1 of Example;

[0040] Figure 2 The BET specific surface area and BJH pore size distribution of the SBHC prepared in step 1 of Example;

[0041] Figure 3 The lead-carbon battery with the SBHC additive prepared in step 1 of Example has 100% DoD capacity under PSoC test conditions;

[0042] Figure 4 The SEM morphology of Sb / SBHC prepared in Example 1 (scale is 5 μm);

[0043] Figure 5 The SEM morphology of Sb / SBHC prepared in Example 1 (scale is 500 nm);

[0044] Figure 6 TEM test results of Sb / SBHC prepared in Example 1;

[0045] Figure 7 The XRD, Raman and N2 adsorption-desorption test results of Sb / SBHC prepared in Example 1 are shown;

[0046] Figure 8 The thermogravimetric test results of Sb / SBHC prepared in Example 1;

[0047] Fig. 9 The lead-carbon battery with Sb / SBHC additive prepared in Example 1 has 100% DoD capacity under PSoC test conditions. DETAILED DESCRIPTION

[0048] The invention provides a method for preparing a bagasse-based hard carbon negative electrode active material for a lead-carbon battery. The method comprises carbonizing bagasse and subjecting the bagasse to acid treatment to obtain bagasse charcoal. Subsequently, the bagasse charcoal, a metal M source and a reducing agent are subjected to chemical reduction deposition to obtain the bagasse-based hard carbon negative electrode active material.

[0049] The present invention provides a method for preparing an optional bagasse-based hard carbon negative electrode active material, comprising the following steps:

[0050] a. Grind bagasse into powder using a planetary ball mill for 0.5 to 3 hours;

[0051] b. Move the ball-milled bagasse powder into a tube furnace for carbonization under Ar atmosphere at a carbonization temperature of 600-1000°C for 1-3 hours;

[0052] c. Soak the obtained bagasse hard carbon in acid, then wash it to neutrality and dry it. The acid can be sulfuric acid, hydrochloric acid, nitric acid, or phosphoric acid. The acid concentration is 0.5 to 3 M and the soaking time is 1 to 48 hours.

[0053] d. Soak 1g of bagasse hard carbon in 50ml of 0.01-0.1mol / L metal salt solution (including antimony, lead, bismuth and other salts) and ultrasonicate, then add 35ml of 0.1-0.5mol / L NaBH4 methanol solution, stir, centrifuge and wash, and dry.

[0054] The following is a specific implementation plan:

[0055] Example 1

[0056] Step 1:

[0057] The bagasse was ground into powder by a planetary ball mill for 2 h; the milled bagasse powder was moved into a tube furnace for carbonization under Ar atmosphere at a carbonization temperature of 900 °C for 2 h; the obtained bagasse hard carbon was soaked in 2M hydrochloric acid for 24 h, washed to neutrality and then dried to obtain bagasse hard carbon (SBHC);

[0058] Structural characterization: Figure 1 The scanning electron microscope image of SBHC shows that SBHC has an obvious porous structure. Figure 2 As shown in Figure 2, the BET specific surface area of ​​SHBC is 672.3 m 2 / g, the pores are mainly micropores (0.7~0.9nm).

[0059] Performance test: The hydrogen evolution behavior of the SBHC electrode was studied by linear sweep voltammetry (LSV) test using an electrochemical workstation. The scanning potential range was -1.40V to -1.1V, and the scanning rate was 10mV / s. Under the potential of -1.40V, the hydrogen evolution current value of the SBHC electrode was -0.363A / g. To test the battery capacity, a charge and discharge test was performed under PSoC conditions. The test method is as follows: (1) At 0.1C 10 The fully charged lead-carbon battery was discharged to a voltage of 1.80 V at a current density of 0.1 C. 10 Constant current charging to 2.4V and then constant voltage charging for nh; (3) 0.1C 10 Discharge to 1.80V; (4) Cycle (2) and (3) 4 times, return to step (1) to monitor the change in battery capacity; (5) Repeat step (4). Where n is the depth of charge, and the value of n is 8 for 0-80% SoC cycle and 6 for 0-60% SoC cycle. Figure 3 As shown, under PSoC test conditions, the initial capacity of the lead-carbon battery with SBHC as an additive at 100% DoD is 4.71 Ah. After the 100th cycle, the 100% DoD discharge capacity drops to 1.71 Ah.

[0060] Step 2:

[0061] 1 g of bagasse hard carbon was immersed in 50 ml of 0.04 mol / L SbCl3 methanol solution and ultrasonicated, then 35 ml of 0.3 mol / L NaBH4 methanol solution was added, stirred at room temperature for 30 to 40 minutes, centrifuged for washing, and dried to obtain bagasse-based biomass carbon-antimony nanoparticle composite material (Sb / SBHC).

[0062] Structural characterization: Figure 4 and 5This is a field emission scanning electron microscope (FESEM) of Sb / SBHC. The results show that a large number of Sb nanoparticles (about 50nm) are in situ grown in the macropores of SBHC. Figure 6 a is a transmission electron microscope (TEM) image of Sb / SBHC. Obviously, a large number of Sb nanoparticles are also embedded in the carbon skeleton. Figure 6 b shows that the diameter of one of the Sb particles is 51 nm under high magnification. Figure 6 c and 6d are high-resolution TEM images of Sb nanoparticles, where the interplanar spacing of 0.23 nm corresponds to the (104) plane of Sb with a hexagonal structure. This result can also be seen from Figure 7 This is confirmed by the X-ray diffraction (XRD) pattern of a. The diffraction peak at 21.8° belongs to the characteristic structure of hard carbon, and the other diffraction peaks correspond to hexagonal Sb (ICSD: PDF 35-0732). Figure 7 b is the Raman spectrum of Sb / SBHC, where 1350 and 1596 cm -1 The two typical peaks at belong to the D band and G band of carbon respectively. D / I G The intensity ratio is 0.97, indicating the abundance of topological defects. Figure 7 c is the N2 adsorption-desorption isotherm and pore size distribution curve of Sb / SBHC with typical type IV behavior. The BET specific surface area of ​​Sb / SBHC is 506.5 m 2 / g, and its pores are mainly micropores (1-2nm), mesopores (3-11nm) and macropores (100-200nm), which are quite different from SBHC. This may be due to the fact that under the long-term ultrasonic action, the SbCl3 solution completely infiltrates the pores of SBHC. During the reduction process, the Sb nanoparticles grown in situ on the carbon skeleton fill the pores of SBHC, forming a hierarchical pore structure of micropores-mesopores-macropores. This stacked porous structure is conducive to the diffusion of the electrolyte, and the large surface area easily induces capacitive behavior during the electrochemical reaction, thereby improving the rate performance and increasing the discharge capacity. Figure 8 As shown, the final Sb content in the composite material was calculated to be 44 wt % by thermogravimetric analysis (TGA) of Sb / SBHC in air.

[0063] Performance test: The hydrogen evolution behavior of SBHC electrode and Sb / SBHC composite electrode was studied by LSV. Under the potential condition of -1.40V, the hydrogen evolution current value of Sb / SBHC composite electrode (-0.142A / g) is 39.1% of the hydrogen evolution current value of SBHC electrode (-0.363A / g). Fig. 9As shown, under PSoC test conditions, the initial capacity of the lead-carbon battery with Sb / SBHC as an additive at 100% DoD is 4.37 Ah. After the 100th cycle, the 100% DoD discharge capacity drops to 2.76 Ah, showing a higher capacity retention rate than the SBHC additive battery.

[0064] It can be seen from Example 1 that by chemically loading SBHC, excellent lead-carbon battery performance can be obtained.

[0065] Example 2

[0066] According to the sample preparation method of Example 1, the methanol solution of SbCl3 was replaced with 50 ml of 0.04 mol / L lead acetate aqueous solution to obtain the Pb / SBHC composite additive. The test conditions were consistent with those of Example 1. Under the potential of -1.40 V, the hydrogen evolution current value (-0.187 A / g) of the Pb / SBHC composite electrode was 51.5% of the hydrogen evolution current value (-0.363 A / g) of the SBHC electrode. Under the PSoC test conditions, the initial capacity of the lead-carbon battery with Pb / SBHC as an additive at 100% DoD was 4.42 Ah. After the 100th cycle, the 100% DoD discharge capacity dropped to 2.41 Ah, showing a higher capacity retention rate than the SBHC additive battery.

[0067] According to the embodiments, after the in-situ growth of metal nanoparticles, the specific surface area of ​​the composite additive decreases, the hydrogen evolution potential increases, and the hydrogen evolution reaction is effectively suppressed.

[0068] Example 3

[0069] Compared with Example 1, the only difference is that the carbonization problem in step 1 is changed to 700°C, 800°C, and 1000°C respectively. The other operations and parameters are the same as those in Example 1. The specific surface area of ​​SBHC obtained at this temperature is shown in Table 1 below:

[0070] Table 1

[0071] Case Carbonization temperature Specific surface area 1 700℃ <![CDATA[208.7m 2 / g]]> 2 800℃ <![CDATA[458.2m 2 / g]]> 3 1000℃ <![CDATA[651.5m 2 / g]]>

[0072] As shown in the results, with the increase of carbonization temperature, the specific surface area of ​​bagasse biochar first gradually increases, reaching the highest at 900°C (Example 1), and then the specific surface area decreases slightly when the carbonization temperature is increased to 1000°C, indicating that further increase of carbonization temperature cannot improve the performance of bagasse-based biochar, but will lead to increased energy consumption. 900°C is the preferred temperature for bagasse carbonization process.

[0073] Example 4

[0074] Compared with Example 1, the only difference is that the concentration of the metal solution in step 2 is changed, and the amount of the metal solution and other conditions are the same as in Example 1. The specific surface area of ​​the finally obtained bagasse-based biomass carbon-antimony nanoparticle composite material (Sb / SBHC) is shown in Table 2.

[0075] Table 2

[0076] Case Group <![CDATA[Concentration of SbCl3]]> Specific surface area 1 0.02 <![CDATA[628.7m 2 / g]]> 2 0.03 <![CDATA[567.2m 2 / g]]> 3 0.05 <![CDATA[507.8m 2 / g]]>

[0077] It can be seen that as the concentration of SbCl3 methanol solution increases, the specific surface area of ​​the composite material is 2 / g) showed a trend of first decreasing and then leveling off, indicating that the adsorption of antimony metal particles by sugarcane bagasse-based biochar reached its maximum when the concentration of SbCl3 methanol solution was 0.04 mol / L.

[0078] Comparative Example 1

[0079] Compared with Example 1, the only difference is that peanut shells are used to replace sugarcane bagasse, and the other operations and parameters are the same as those in Example 1. A peanut shell-based biomass carbon-antimony nanoparticle composite material is obtained. By comparison, it is found that the specific surface area of ​​the biomass hard carbon obtained using peanut shells is 362.3 m 2 / g, which is much smaller than bagasse hard carbon. The specific surface area of ​​the composite material of peanut shell-based biomass carbon-antimony nanoparticles is 220.4m 2 / g, antimony is concentrated on the surface of peanut shell-based hard carbon, and the particle distribution is uneven.

[0080] Comparative Example 2

[0081] Compared with Example 1, the only difference is that in step 2, no reducing agent is added, and other operations and parameters are the same as Example 1. A bagasse-based biomass carbon-SbCl3 composite is obtained, which cannot inhibit the hydrogen evolution reaction.

[0082] Comparative Example 3

[0083] Compared with Example 1, the only difference is that in step 2, the sugarcane bagasse hard carbon is soaked in 50 ml of a methanol solution of SbCl3 with a concentration of 0.04 mol / L, ultrasonically dried, and then moved into a tube furnace for thermal reduction at 400° C. in a 5% H2 / Ar atmosphere to obtain a thermally reduced sugarcane bagasse-based biomass carbon-antimony nanoparticle composite material (H-Sb / SBHC). By comparison, it is found that the Sb content in the composite material obtained by this method is low, only 23wt%, the raw material utilization rate is low, and the energy consumption is high.

[0084] Comparative Example 4

[0085] Compared with Example 1, the only difference is that in step 2, bismuth chloride is used to replace the Sb, and other operations and parameters are the same as Example 1. Under PSoC test conditions, the initial capacity of the lead-carbon battery with Bi / SBHC as an additive at 100% DoD is 4.15 Ah, and after the 100th cycle, the 100% DoD discharge capacity drops to 2.26 Ah.

[0086] The battery performance results of some of the materials successfully prepared by the present invention are shown in Table 3:

[0087] Table 3

[0088]

[0089] It can be seen from Table 3 that the material obtained by the process method of the present invention has excellent performance.

Claims

1. A method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery, characterized in that: Carbonizing and acid-treating bagasse to obtain bagasse charcoal; The bagasse charcoal, metal M source and reducing agent are subjected to chemical reduction deposition to obtain the bagasse-based hard carbon negative electrode active material; The metal M source is a water-soluble salt containing a metal M element, and the metal M element includes at least one of antimony, lead, and bismuth; The reducing agent is a component that can reduce the metal M source to a single metal M.

2. The method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery according to claim 1, characterized in that: Before carbonization, the bagasse is pre-milled; the ball milling time is 0.5 to 3 hours; Preferably, the atmosphere in the carbonization stage is an oxygen-free or low-oxygen atmosphere; preferably at least one of nitrogen and an inert gas; Preferably, the carbonization temperature is 600-1000°C; Preferably, the carbonization time is 1-3 hours.

3. The method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery according to claim 1, characterized in that: placing the carbonized product in an acid solution for acid treatment; Preferably, the acid solution is an aqueous solution of an inorganic acid; Preferably, the solute concentration of the inorganic acid in the acid solution is 0.5 to 3 M; Preferably, the acid treatment time is 1 to 48 hours.

4. The method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery according to claim 1, characterized in that: The reducing agent is at least one of NaBH4, Ar / H2 mixed gas and hydrazine hydrate.

5. The method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery according to claim 1, characterized in that: The molar weight ratio of the metal M source to the bagasse charcoal is 1 to 5 mmol / g, preferably 2 to 3 mmol / g.

6. The method for preparing bagasse-based hard carbon negative electrode active material for lead-carbon battery according to claim 1, characterized in that: The temperature during the chemical reduction deposition stage is 0 to 50°C; Preferably, the chemical reduction deposition time is 15 to 60 minutes.

7. A bagasse-based hard carbon negative electrode active material prepared by the preparation method according to any one of claims 1 to 6; characterized in that: The charcoal comprises bagasse charcoal and nano-metal M particles chemically deposited on the surface of the charcoal.

8. A negative electrode material for a lead-carbon battery, comprising a negative electrode active material, characterized in that: The negative electrode active material comprises a bagasse-based hard carbon negative electrode active material prepared by the preparation method according to any one of claims 1 to 6; Preferably, the negative electrode material further comprises a conductive agent and a binder.

9. A negative electrode for a lead-carbon battery, comprising a current collector and a negative electrode material composited on the surface thereof, characterized in that: The negative electrode material is the negative electrode material according to claim 8.

10. A lead-carbon battery, characterized in that: The negative electrode according to claim 9 is included.

Citation Information

Patent Citations

  • A process of preparing a hard carbon composite material

    CN108140818A

  • Preparation method and application of self-template-based nitrogen-doped bagasse biochar electrode material

    CN118125437A

  • Hard carbon negative electrode material for sodium-ion battery and preparation method therefor