Method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber
By using magnesium oxide-based cobalt catalyst in thermal cracking of waste rubber, the thermal cracking temperature is reduced and single-wall carbon nanotubes are successfully prepared, which solves the problem of high-cost preparation of single-wall carbon nanotubes and achieves low cost and high efficiency Resource utilization.
Patent Information
- Application Number
- CN202411297825.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to prepare single-wall carbon nanotubes at low cost and efficiently, and rely on imported high-purity gas carbon sources, resulting in high production costs and low value of waste rubber thermal cracking products.
Using a transition metal cobalt catalyst supported by a magnesium oxide substrate, the chemical vapor deposition method uses waste rubber as a carbon source to reduce the thermal cracking temperature and achieve low-cost preparation of single-wall carbon nanotubes.
It reduces the production cost of single-wall carbon nanotubes, improves the recycling efficiency of waste rubber, realizes the renewable utilization of resources, simplifies the process flow, and reduces energy consumption.
Smart Images

Figure CN119079983A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of single-wall carbon nanotube preparation, and specifically relates to a method for preparing single-wall carbon nanotubes by thermal conversion of waste rubber. Background Art
[0002] Rubber is a basic material for industrial production and is known as "black gold". Today, the output value of my country's rubber industry has exceeded 2 trillion yuan, and rubber products have spread throughout all aspects of people's lives. Rubber products have the characteristics of short life and frequent replacement, so a large amount of waste rubber is also generated, which poses a huge threat to the environment. Traditional rubber processing methods are mainly landfilling. This treatment method occupies land resources and causes secondary pollution. Therefore, thermal treatment through high-temperature cracking to recover effective components has become the most effective method for recycling waste rubber. The products of thermal treatment of waste rubber mainly include carbon nanotubes, hydrogen, asphalt, combustible gas fuels and other substances. Although rubber recycling can be achieved, the related products have long been industrialized, so their value is relatively low.
[0003] Carbon nanotubes are divided into single-walled carbon nanotubes and multi-walled carbon nanotubes. Currently, most of the carbon nanotubes produced in industrial quantities are multi-walled carbon nanotubes. Single-walled carbon nanotubes are far superior to multi-walled carbon nanotubes in terms of acoustic, optical, electrical, thermal and mechanical properties. They are new technical materials that the country urgently needs, and their commercial value is far higher than that of multi-walled carbon nanotubes.
[0004] At present, the carbon sources for preparing single-walled carbon nanotubes are mainly high-purity methane and high-purity carbon monoxide. The high price of gas carbon sources makes the cost of preparing single-walled carbon nanotubes high, and the production process is difficult to achieve domestic production. At present, single-walled carbon nanotubes mainly rely on imports. The gas after thermal cracking of waste rubber contains a large amount of hydrocarbons, which can be used as a carbon source for preparing carbon nanotubes. In existing technical research, multi-walled carbon nanotubes are prepared by high-temperature cracking of rubber, which has relatively low value.
[0005] Based on this, the present invention successfully realizes the preparation of single-walled carbon nanotubes using waste rubber as a carbon source through catalyst design and temperature control in the preparation process. Summary of the invention
[0006] The purpose of the present invention is to solve the above-mentioned problems existing in the prior art, and a method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber is proposed. The method adopts a transition metal cobalt catalyst supported on a magnesium oxide substrate, and pyrolyzes a variety of rubber products with different components as a carbon source through chemical vapor deposition to prepare single-walled carbon nanotubes, thereby achieving high added value conversion of waste rubber products and low-cost preparation of single-walled carbon nanotubes.
[0007] The technical solution of the present invention is:
[0008] A method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber comprises the following steps:
[0009] (1) dissolving porous magnesium oxide and cobalt nitrate hexahydrate in a certain amount of deionized water in a mass ratio of 2:(0.5-1), mixing evenly, immersing for 3-5 hours, drying at 100-120° C., and grinding into powder to obtain a catalyst;
[0010] The mass ratio of the porous magnesium oxide to the cobalt nitrate hexahydrate is any ratio within the range of 2:(0.5-1), for example, 2:0.5, 2:0.6, 2:0.7, 2:0.8, 2:0.9 or 2:1, etc., but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0011] The above-mentioned immersion time is any time within the range of 3 to 5 hours, for example, it can be 3 hours, 3.5 hours, 3.7 hours, 3.8 hours, 3.9 hours, 4 hours, 4.1 hours, 4.2 hours, 4.3 hours, 4.5 hours or 5 hours, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0012] (2) crushing the waste rubber into particles of 1 to 2 cm, and placing them in a porcelain boat and a quartz boat respectively with the catalyst powder, and placing the quartz boat on the right side of a dual-temperature zone high-temperature vacuum sliding tube furnace, and placing the porcelain boat on the left side, setting the furnace to heat at a rate of 20°C / min, and introducing inert gas at a flow rate of 300 sccm to exclude air;
[0013] (3) Raise the temperature to 300°C to 400°C on the left side and 700°C to 800°C on the right side, then adjust the inert gas flow rate to continuously introduce it at a flow rate of 100 sccm for 25 to 45 minutes; then cool down and adjust the inert gas flow rate to 300 sccm until the temperature on one side of the waste rubber reaches room temperature, then stop the ventilation, and single-walled carbon nanotubes are obtained.
[0014] The temperature on the left side is any temperature in the range of 300℃ to 400℃, for example, it can be 300℃, 310℃, 320℃, 330℃, 340℃, 350℃, 360℃, 370℃, 380℃, 390℃ or 400℃; the temperature on the right side is any temperature in the range of 700℃ to 800℃, for example, it can be 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, 760℃, 770℃, 780℃, 790℃ or 800℃; but it is not limited to the listed values, and other unlisted values in the range are equally applicable.
[0015] The reaction time is any time within the range of 25 to 45 min, for example, it can be 25 min, 30 min, 32 min, 33 min, 34 min, 35 min, 36 min, 37 min, 38 min, 40 min or 45 min, but is not limited to the listed values, and other unlisted values within the range are also applicable.
[0016] Furthermore, the mass ratio of the porous magnesium oxide to the cobalt nitrate hexahydrate is 2:0.7.
[0017] Furthermore, the preparation step of the porous magnesium oxide is: calcining basic magnesium carbonate at 400° C. to 500° C. for 90 minutes to obtain porous magnesium oxide.
[0018] Furthermore, the mass ratio of the catalyst to the waste rubber particles is 1:1.
[0019] Furthermore, the waste rubber is waste rubber produced from any one or several rubber products including natural rubber, nitrile rubber, hydrogenated nitrile rubber, butadiene rubber, polyurethane rubber and isoprene rubber.
[0020] Furthermore, the inert gas includes argon and nitrogen.
[0021] Furthermore, in the step (1), the immersion time is 4 hours and the drying temperature is 120°C.
[0022] Furthermore, in step (3), after the left pyrolysis zone is heated to 300°C-400°C and stabilized, and the right heating zone is heated to 700°C-800°C and stabilized, the inert gas is adjusted to be continuously introduced at a flow rate of 100 sccm, and the reaction temperature and gas flow rate are maintained for 35 minutes.
[0023] Beneficial effects of the present invention:
[0024] (1) In the method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber provided by the present invention, the cracking temperature of the waste rubber is reduced to the range of 300°C-400°C. Compared with the traditional thermal cracking method which mostly adopts the range of 700°C-800°C, the energy consumption of the present method is greatly reduced. At the same time, the high added value conversion of waste rubber to single-walled carbon nanotubes is achieved, which greatly solves the problems of low recycling efficiency and serious pollution of waste rubber and realizes the renewable recycling of resources.
[0025] (2) The present invention uses waste rubber as a carbon source, which is inexpensive, widely available, and has a low pyrolysis temperature, greatly reducing the production cost of single-walled carbon nanotubes and providing a new path for the industrial preparation of single-walled carbon nanotubes. At the same time, the method is easy to operate, has a short reaction time, is economical and efficient, and is conducive to large-scale promotion and adoption. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of the butadiene rubber product of Example 1;
[0027] Figure 2 This is a transmission electron microscope image of the single-walled carbon nanotube prepared in Example 1;
[0028] Figure 3 is a scanning electron microscope image of the single-walled carbon nanotube prepared in Example 1;
[0029] Figure 4 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of natural rubber products in Example 4;
[0030] Figure 5 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of hydrogenated nitrile rubber products in Example 5;
[0031] Figure 6 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of polyurethane rubber products in Example 6;
[0032] Figure 7 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of nitrile rubber products in Example 7;
[0033] Figure 8 This is a Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of isoprene rubber products in Example 8;
[0034] Fig. 9 This is the Raman spectrum of single-walled carbon nanotubes prepared by thermal cracking of various rubber mixed products in Example 9. DETAILED DESCRIPTION
[0035] In order to further understand the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments, and the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] The experimental methods in the following examples, unless otherwise specified, are all conventional experimental operation methods. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial channels.
[0037] Example 1
[0038] This embodiment provides a method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber, comprising the following steps:
[0039] (1) calcining basic magnesium carbonate at 450° C. in a muffle furnace for 90 minutes to obtain the desired porous magnesium oxide;
[0040] Weigh 4 g of porous magnesium oxide and 1.4 g of cobalt nitrate hexahydrate and dissolve them in 100 mL of deionized water, mix them evenly, and soak them for 4 hours. Place the solution in an oven at 120° C. to dry and grind it into powder to obtain a catalyst;
[0041] (2) crushing the waste butadiene rubber into particles of 1 cm in size;
[0042] According to the mass ratio of 1:1, weigh appropriate amount of catalyst powder and waste butadiene rubber particles and put them into quartz boat and porcelain boat respectively, and put the quartz boat on the right side of the dual-temperature zone high-temperature vacuum sliding tube furnace, and put the porcelain boat on the left side of the tube furnace, connect the gas line, start the device, set the furnace temperature to rise at a rate of 20℃ / min, and introduce Ar at a flow rate of 300sccm to remove the air in the device;
[0043] (3) When the temperature of the left pyrolysis zone reaches 400°C and the temperature of the right heating zone reaches 800°C, the furnace is pulled to the waste particles and the catalyst respectively. After the furnace temperature stabilizes, the Ar flow rate is adjusted and Ar is continuously introduced at a flow rate of 100 sccm. After the reaction temperature and gas flow rate are maintained for 35 minutes, the furnace is pulled to both sides, the heating program is stopped and the temperature is lowered. The Ar flow rate is adjusted to 300 sccm until the temperature of the sample side reaches room temperature. Then, Ar is turned off and the quartz boat is taken out to obtain the single-walled carbon nanotube sample.
[0044] The prepared single-walled carbon nanotubes were characterized by Figure 1 The Raman spectrum of single-walled carbon nanotubes is shown. As can be seen from the figure, RBM peaks appear at wavelengths of 100-400 in the Raman spectrum, proving that the sample is a single-walled carbon nanotube.
[0045] Figure 2 This is a transmission electron microscope image of single-walled carbon nanotubes, proving that the sample tube wall is single-walled and the surface is clean and free of impurities. Figure 3 This is a scanning electron microscope image of single-walled carbon nanotubes, which proves that the single-walled carbon nanotube samples are dense and abundant, and the yield is high.
[0046] Example 2
[0047] This embodiment provides a method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber, comprising the following steps:
[0048] (1) calcining basic magnesium carbonate in a muffle furnace at 400° C. for 90 minutes to obtain the desired porous magnesium oxide;
[0049] Weigh 4 g of porous magnesium oxide and 1 g of cobalt nitrate hexahydrate and dissolve them in 100 mL of deionized water, mix them evenly, and soak them for 3 h. Place the solution in an oven at 100 °C to dry and grind it into powder to obtain a catalyst;
[0050] (2) crushing the waste butadiene rubber into particles of 2 cm in size;
[0051] According to the mass ratio of 1:1, weigh appropriate amount of catalyst powder and waste butadiene rubber particles and put them into quartz boat and porcelain boat respectively, and put the quartz boat on the right side of the dual-temperature zone high-temperature vacuum sliding tube furnace, and put the porcelain boat on the left side of the tube furnace, connect the gas line, start the device, set the furnace temperature to rise at a rate of 20℃ / min, and introduce Ar at a flow rate of 300sccm to remove the air in the device;
[0052] (3) When the temperature of the left pyrolysis zone reaches 300°C and the temperature of the right heating zone reaches 700°C, the furnace is pulled to the waste particles and the catalyst respectively. After the furnace temperature stabilizes, the Ar flow rate is adjusted and Ar is continuously introduced at a flow rate of 100 sccm. After the reaction temperature and gas flow rate are maintained for 45 minutes, the furnace is pulled to both sides, the heating program is stopped and the temperature is lowered. The Ar flow rate is adjusted to 300 sccm until the temperature of the sample side reaches room temperature. Then, Ar is turned off and the quartz boat is taken out to obtain the single-walled carbon nanotube sample.
[0053] Example 3
[0054] This embodiment provides a method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber, comprising the following steps:
[0055] (1) calcining basic magnesium carbonate in a muffle furnace at 500° C. for 90 minutes to obtain the desired porous magnesium oxide;
[0056] Weigh 4 g of porous magnesium oxide and 2 g of cobalt nitrate hexahydrate and dissolve them in 100 mL of deionized water, mix them evenly, and soak them for 5 h. Place the solution in an oven at 110° C. to dry and grind it into powder to obtain a catalyst;
[0057] (2) crushing the waste butadiene rubber into particles of 1.5 cm in size;
[0058] According to the mass ratio of 1:1, weigh appropriate amount of catalyst powder and waste butadiene rubber particles and put them into quartz boat and porcelain boat respectively, and put the quartz boat on the right side of the dual-temperature zone high-temperature vacuum sliding tube furnace, and put the porcelain boat on the left side of the tube furnace, connect the gas line, start the device, set the furnace temperature to rise at a rate of 20℃ / min, and introduce N2 at a flow rate of 300sccm to remove the air in the device;
[0059] (3) When the temperature of the left pyrolysis zone reaches 350°C and the temperature of the right heating zone reaches 750°C, the furnace is pulled to the waste particles and the catalyst respectively. After the furnace temperature stabilizes, the N2 flow rate is adjusted and N2 is continuously introduced at a flow rate of 100 sccm. After the reaction temperature and gas flow rate are maintained for 25 minutes, the furnace is pulled to both sides, the heating program is stopped and the temperature is lowered. The N2 flow rate is adjusted to 300 sccm until the temperature of the sample side reaches room temperature. Then, the N2 is turned off and the quartz boat is taken out to obtain the single-walled carbon nanotube sample.
[0060] Example 4
[0061] The difference between this embodiment and embodiment 1 is that waste natural rubber products are used to prepare single-walled carbon nanotubes.
[0062] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Figure 4 shown.
[0063] Example 5
[0064] The difference between this embodiment and embodiment 1 is that waste hydrogenated nitrile rubber products are used to prepare single-walled carbon nanotubes.
[0065] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Figure 5 shown.
[0066] Example 6
[0067] The difference between this embodiment and embodiment 1 is that waste polyurethane rubber products are used to prepare single-walled carbon nanotubes.
[0068] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Figure 6 shown.
[0069] Example 7
[0070] The difference between this embodiment and embodiment 1 is that waste nitrile rubber products are used to prepare single-walled carbon nanotubes.
[0071] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Figure 7 shown.
[0072] Example 8
[0073] The difference between this embodiment and embodiment 1 is that waste isoprene rubber products are used to prepare single-walled carbon nanotubes.
[0074] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Figure 8 shown.
[0075] Example 9
[0076] The difference between this embodiment and embodiment 1 is that a mixed product of various waste rubbers including natural rubber, nitrile rubber, hydrogenated nitrile rubber, butadiene rubber, polyurethane rubber or isoprene rubber is used to prepare single-walled carbon nanotubes.
[0077] The Raman spectrum of the prepared single-walled carbon nanotubes is shown in Fig. 9 shown.
[0078] The above description is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, modification, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing single-walled carbon nanotubes by thermal conversion of waste rubber, characterized in that: The following steps are involved: (1) dissolving porous magnesium oxide and cobalt nitrate hexahydrate in a certain amount of deionized water in a mass ratio of 2:(0.5-1), mixing evenly, immersing for 3-5 hours, drying at 100-120° C., and grinding into powder to obtain a catalyst; (2) crushing the waste rubber into particles of 1 to 2 cm, and placing them in a porcelain boat and a quartz boat respectively with the catalyst powder, and placing the quartz boat on the right side of a dual-temperature zone high-temperature vacuum sliding tube furnace, and placing the porcelain boat on the left side, setting the furnace to heat at a rate of 20°C / min, and introducing inert gas at a flow rate of 300 sccm to exclude air; (3) Raise the temperature to 300°C to 400°C on the left side and 700°C to 800°C on the right side, then adjust the inert gas flow rate to continuously introduce it at a flow rate of 100 sccm for 25 to 45 minutes; then cool down and adjust the inert gas flow rate to 300 sccm until the temperature on one side of the waste rubber reaches room temperature, then stop the ventilation, and single-walled carbon nanotubes are obtained.
2. The method according to claim 1, characterized in that The mass ratio of the porous magnesium oxide to the cobalt nitrate hexahydrate is 2:0.
7.
3. The method according to claim 1, characterized in that The preparation steps of the porous magnesium oxide are as follows: calcining basic magnesium carbonate at 400° C. to 500° C. for 90 minutes to obtain the porous magnesium oxide.
4. The method according to claim 1, characterized in that: The mass ratio of the catalyst to the waste rubber particles is 1:
1.
5. The method according to claim 1, characterized in that The waste rubber is waste rubber produced from any one or several rubber products including natural rubber, nitrile rubber, hydrogenated nitrile rubber, butadiene rubber, polyurethane rubber and isoprene rubber.
6. The method according to claim 1, characterized in that The inert gas includes argon and nitrogen.
7. The method according to claim 1, characterized in that In the step (1), the immersion time is 4 hours and the drying temperature is 120°C.
8. The method according to claim 1, characterized in that In the step (3), the left pyrolysis zone is heated to 300°C to 400°C and stabilized, and the right heating zone is heated to 700°C to 800°C and stabilized, and then the inert gas is adjusted to continuously flow at a flow rate of 100 sccm, and the reaction temperature and gas flow rate are maintained for 35 minutes.
Citation Information
Patent Citations
Processes for production of carbon nanotubes from natural rubber
CN111465579A
Method for preparing single-walled carbon nanotube from pyrolytic plastic and nano electronic device
CN113683081A