Method for preparing graphene by pulse liquid phase discharge method, prepared graphene and application
Preparation of graphene in inorganic salt solution by pulse liquid phase discharge method solves the problems of high cost of graphene preparation and low reproducibility in the prior art, and achieves efficient and green graphene macro-quantitative production, with excellent electrical Chemical properties and environmentally friendly process characteristics.
Patent Information
- Application Number
- CN202411200284.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing graphene preparation methods have problems such as high cost, complex process, low reproducibility, and irreversible damage to the crystal structure, making it difficult to achieve large-scale, green and economical high-quality graphene mass production.
The pulse liquid phase discharge method is used to pulse peel off the graphite sheet in the inorganic salt solution through a pulse power supply, and the expansion and dissolution of the graphite sheet is promoted by using high concentrations of oxygen-containing free radicals and bubbles, and the carbon-oxygen ratio is low and the number of layers is small. Graphene with large specific surface area and excellent electrochemical properties.
It has achieved efficient preparation of graphene with excellent electrochemical properties in inorganic salt solution. It has simple process, convenient operation, synthesis at room temperature and pressure, environment friendly, high peeling efficiency, and is suitable for macro-quantitative production.
Smart Images

Figure CN119079986A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphene materials, and in particular to a pulse liquid phase discharge method for preparing graphene, the prepared graphene and its application. Background Art
[0002] Graphene is a new type of two-dimensional carbon material that has attracted much attention in the 21st century. It has unique physical and chemical properties, mainly reflected in high specific surface area, excellent conductivity, fast two-dimensional planar transfer characteristics, small stacking density, high chemical stability, high mechanical strength and oxidation resistance. It has a wide range of applications in supercapacitors, lithium-ion batteries, flexible sensors and other fields. At present, graphene can be prepared by a variety of processes, mainly including chemical vapor deposition, epitaxial growth, redox method, mechanical exfoliation, liquid phase exfoliation, etc. Chemical vapor deposition often has high preparation costs and complex processes; while epitaxial growth method is difficult to control the thickness of graphene growth and has randomness; mechanical exfoliation method cannot be implemented on a large scale due to low reproducibility and can only be used for basic research and basic research; redox method has high yield but harsh reduction process and irreversibly destroys the crystal structure; liquid phase exfoliation method has few defects but low exfoliation yield and high cost of using organic solvents / ionic solutions. In order to realize the large-scale application of graphene and adapt to the update and development of energy storage needs of emerging products, it is urgent to develop a simple, green and economical method to mass produce high-quality graphene. See Banszerus L, et al. Science Advances, 2015, 1 (6): 1-6. Huang Q, et al. The Journal of Physical Chemistry C, 2011, 115 (42): 20538-20545. Agarwal V. Chemical Engineering Journal, 2020.12 (2): 126-130. Yi M, Shen Z. Journal of Materials Chemistry A, 2015, 3(22): 11700-11715. Yang S, et al. Advanced Materials, 2013.25, 2452–2456.
[0003] Electrochemical exfoliation is a common method for preparing graphene. It has a simple process, fast production, and is generally environmentally friendly. It is a large-scale preparation method for graphene with commercial potential. Usually, a voltage is applied between two electrodes, and different electrolytes are used for exfoliation, mainly including water systems, ionic liquid systems, and composite systems. However, non-aqueous electrolytes are expensive and sensitive to oxygen and water, which greatly limits their practical applications. See Khaled Parvez, et al. J. Am. Chem. Soc. 2014, 136, 6083-6091. Parvez K, et al. Journal of the American Chemical Society, 2014, 136 (16): 6083-6091. Ambrosi A, et al. Chemistry: A European journal, 2016 (1): 22. Summary of the invention
[0004] The technical problem to be solved by the present invention is how to provide a new method for preparing graphene with excellent electrochemical performance.
[0005] The present invention solves the above technical problems through the following technical means:
[0006] The first aspect of the present invention provides a method for preparing graphene by a pulsed liquid phase discharge method, comprising the following steps: the anode of a pulse power supply is connected in parallel to a plurality of graphite sheet target materials, the cathode is a graphite sheet, the cathode is completely immersed in an inorganic salt solution, and the anode is placed above the inorganic salt solution; the pulse power supply is started, pulse stripping is performed, and then graphene is obtained by solid-liquid separation.
[0007] Beneficial effects: The present invention adopts a pulse liquid phase discharge method to prepare graphene, and performs macro-synthesis of graphene in an inorganic salt solution. Microsecond-level pulse discharge forms high voltage in an instant, and a high concentration of oxygen-containing free radicals are generated at the interface between the anode graphite sheet and the inorganic salt solution, opening the edge interlayer spacing, and anions move to the graphite sheet opened by the anode and intercalate. A large number of bubbles generated by the pulse discharge at the solid-liquid interface further promote the expansion and dissolution of the graphite sheet target material, so that the prepared graphene has the characteristics of low carbon-oxygen ratio, small number of layers, large specific surface area, excellent electrochemical performance, etc.
[0008] Preferably, the anode is connected in parallel with 2 to 6 graphite sheet targets, and the thickness of the graphite sheet targets is 1 to 2 mm.
[0009] Preferably, the cathode graphite sheet has a thickness of 2 to 5 mm.
[0010] Preferably, the inorganic salt solution is sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution or sodium chloride solution.
[0011] Preferably, the volume of the inorganic salt solution is 300 ml, and the concentration of the inorganic salt solution is 0.1-0.5M.
[0012] Preferably, the anode is 1.3 to 1.7 cm away from the inorganic salt solution.
[0013] Preferably, the current of the pulse power supply is 2-7A, the discharge machining pulse working period ranges from 100-300 μs, the pulse rest period ranges from 100-300 μs, and the discharge gap is set to 25-75 μm.
[0014] Preferably, the pulse stripping time is 10 to 30 minutes.
[0015] The second aspect of the present invention provides a method for preparing graphene using the above-mentioned pulsed liquid phase discharge method to prepare graphene.
[0016] The third aspect of the present invention provides the use of graphene prepared by the method for preparing graphene by the pulsed liquid phase discharge method in supercapacitor electrodes.
[0017] The advantages of the present invention are:
[0018] The present invention uses a pulsed liquid phase discharge method to obtain graphene with excellent capacitance performance in a variety of inorganic salt solutions, and achieves excellent stripping efficiency in a very short time. Compared with the traditional electrochemical stripping preparation of graphene, the present invention is not limited to the use of constant voltage power supplies or scientific research equipment in electrochemical workstations in a laboratory environment. It uses a pulse power supply for macro-quantitative clean preparation. The process is simple, easy to operate, and easy to control. It belongs to normal temperature and pressure synthesis, and does not use toxic reaction raw materials. It is an environmentally friendly green synthesis process. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 Schematic diagram of the method for preparing graphene by pulse liquid phase discharge in an embodiment; in the figure, three graphite sheet targets are connected in parallel to the anode, the cathode graphite sheet is completely immersed in an inorganic salt solution, and a large number of bubbles are generated at the solid-liquid interface by pulse discharge;
[0020] Figure 2 The morphological characterizations of graphene obtained in different inorganic salt solutions of the embodiments; (a) and (e) are morphological characterizations of graphene obtained in embodiment 1; (b) and (f) are morphological characterizations of graphene obtained in embodiment 2; (c) and (g) are morphological characterizations of graphene obtained in embodiment 3; (d) and (h) are morphological characterizations of graphene obtained in embodiment 4;
[0021] Figure 3The microscopic morphology and layer number characterization of the graphene obtained in different inorganic salt solutions of the embodiments; (a) and (e) are the microscopic morphology and layer number characterization of the graphene obtained in Example 1; (b) and (f) are the microscopic morphology and layer number characterization of the graphene obtained in Example 2; (c) and (g) are the microscopic morphology and layer number characterization of the graphene obtained in Example 3; (d) and (h) are the microscopic morphology and layer number characterization of the graphene obtained in Example 4;
[0022] Figure 4 It is a structural characterization of graphene obtained in different inorganic salt solutions in the examples; (a) is the XRD spectrum of graphene obtained in Examples 1-4; (b) is the adsorption-desorption curve of graphene obtained in Examples 1-4; (c) is the Raman spectrum of graphene obtained in Examples 1-4; (d) is the XPS full spectrum of graphene obtained in Examples 1-4; (eh) is the XPS carbon spectrum of graphene obtained in Examples 1-4;
[0023] Figure 5 The electrochemical properties of the graphene obtained in different inorganic salt solutions of the embodiments; (a) is the cyclic voltammetry curve of the graphene obtained in embodiments 1-4; (b) is the cyclic voltammetry curve of the graphene obtained in embodiment 1 at different scan rates; (c) is the charge and discharge curve of the graphene obtained in embodiments 1-4; (d) is the charge and discharge curve of the graphene obtained in embodiment 1 at different current densities; (e) is the EIS curve of the graphene obtained in embodiments 1-4; (f) is the stability test of the graphene obtained in embodiments 1-2;
[0024] Figure 6 The figures show the microscopic morphology and electrochemical properties of graphene obtained in pure water in the comparative example: (a) and (b) are the microscopic morphology characterizations of the graphene obtained in the comparative example; (c) is the cyclic voltammetry curve of the graphene obtained in the comparative example at different scan rates; (d) is the charge and discharge curve of the graphene obtained in the comparative example at different current densities. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0027] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0028] The present invention provides a method for preparing graphene by a pulsed liquid phase discharge method and the prepared graphene, comprising the following steps:
[0029] (1) Connect 2 to 6 graphite sheet targets in parallel to the anode of the pulse power supply, the thickness of the graphite sheet targets is 1 to 2 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 2 to 5 mm. The thickness of the cathode graphite sheet is selected to be thicker to prevent the cathode graphite sheet from breaking due to excessively long pulse stripping time.
[0030] (2) Then completely immerse the cathode graphite sheet in the inorganic salt solution, place the anode target material above the inorganic salt solution, 1.3 to 1.7 cm from the inorganic salt liquid surface, and control the distance between the target material and the liquid surface to ensure that the pulse discharge stripping continues to occur. Figure 1 shown.
[0031] (3) The salt-free solution is a sodium sulfate solution, a sodium perchlorate solution, a sodium carbonate solution or a sodium chloride solution, with a volume of 300 ml and a concentration of 0.1 to 0.5 M.
[0032] (4) Start the pulse power supply to perform pulse stripping for 10 to 30 minutes. The current of the pulse power supply is 2 to 7A, the discharge machining pulse working cycle ranges from 100 to 300 μs, the pulse rest cycle ranges from 100 to 300 μs, and the discharge gap is set to 25 to 75 μm.
[0033] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 20 to 30 minutes, washed with deionized water 2 to 3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product. The present invention ultrasonically disperses the graphene solution, washes it multiple times, and filters it to wash away inorganic salts on the surface of the graphene, so as to obtain a pure graphene product.
[0034] Example 1
[0035] This embodiment provides a method for preparing graphene by pulsed liquid phase discharge method and the obtained graphene, comprising the following steps:
[0036] (1) The anode of the pulse power supply is connected in parallel to three graphite target sheets, the thickness of the graphite target sheet is 1 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 2 mm.
[0037] (2) Then, the cathode graphite sheet is completely immersed in the sodium sulfate solution, and the anode is placed above the sodium sulfate solution, 1.5 cm away from the sodium sulfate liquid surface. The volume of the sodium sulfate solution is 300 ml and the concentration is 0.1 M.
[0038] (4) Start the pulse power supply to perform pulse stripping for 10 minutes. The current of the pulse power supply is 5A, the discharge machining pulse working period is 200 μs, the pulse rest period is 200 μs, and the discharge gap is set to 50 μm.
[0039] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 20 minutes, washed with deionized water 2-3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product.
[0040] Example 2
[0041] This embodiment provides a method for preparing graphene by pulsed liquid phase discharge method and the obtained graphene, comprising the following steps:
[0042] (1) The anode of the pulse power supply is connected in parallel to three graphite sheet targets, the thickness of the graphite sheet targets is 2 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 3 mm.
[0043] (2) Then, the cathode graphite sheet is completely immersed in the sodium perchlorate solution, and the anode target is placed above the sodium perchlorate solution, 1.5 cm away from the sodium perchlorate liquid surface. The volume of the sodium perchlorate solution is 300 ml, and the concentration is 0.2 M.
[0044] (4) Start the pulse power supply to perform pulse stripping for 20 minutes. The current of the pulse power supply is 5A, the discharge machining pulse working period is 200 μs, the pulse rest period is 200 μs, and the discharge gap is set to 50 μm.
[0045] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 30 minutes, washed with deionized water 2-3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product.
[0046] Example 3
[0047] This embodiment provides a method for preparing graphene by pulsed liquid phase discharge method and the obtained graphene, comprising the following steps:
[0048] (1) The anode of the pulse power supply is connected in parallel to three graphite sheet targets, the thickness of the graphite sheet targets is 1 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 4 mm.
[0049] (2) Then, the cathode graphite sheet is completely immersed in the sodium carbonate solution, and the anode target is placed above the sodium carbonate solution, 1.5 cm away from the sodium carbonate liquid surface. The volume of the sodium carbonate solution is 300 ml, and the concentration is 0.3 M.
[0050] (4) Start the pulse power supply to perform pulse stripping for 30 minutes. The current of the pulse power supply is 5A, the discharge machining pulse working period is 200 μs, the pulse rest period is 200 μs, and the discharge gap is set to 50 μm.
[0051] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 30 minutes, washed with deionized water 2 to 3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product.
[0052] Example 4
[0053] This embodiment provides a method for preparing graphene by pulsed liquid phase discharge method and the obtained graphene, comprising the following steps:
[0054] (1) The anode of the pulse power supply is connected in parallel to three graphite sheet targets, the thickness of the graphite sheet targets is 1 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 5 mm.
[0055] (2) Then, the cathode graphite sheet is completely immersed in the sodium carbonate solution, and the anode target is placed above the sodium carbonate solution, 1.5 cm away from the sodium carbonate liquid surface. The volume of the sodium carbonate solution is 300 ml, and the concentration is 0.4 M.
[0056] (4) Start the pulse power supply to perform pulse stripping for 25 minutes. The current of the pulse power supply is 5A, the discharge machining pulse working period is 200 μs, the pulse rest period is 200 μs, and the discharge gap is set to 50 μm.
[0057] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 20 minutes, washed with deionized water 2-3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product.
[0058] Comparative Example 1
[0059] This embodiment provides a method for preparing graphene by pulsed liquid phase discharge method and the obtained graphene, comprising the following steps:
[0060] (1) The anode of the pulse power supply is connected in parallel to three graphite target sheets, the thickness of the graphite target sheet is 1 mm, and the cathode is a graphite sheet, the thickness of the cathode graphite sheet is 2 mm.
[0061] (2) Then, the cathode graphite sheet is completely immersed in pure water, and the anode target is placed above the pure water, 1.5 cm away from the pure water.
[0062] (4) Start the pulse power supply to perform pulse stripping for 10 minutes. The current of the pulse power supply is 5A, the discharge machining pulse working period is 200 μs, the pulse rest period is 200 μs, and the discharge gap is set to 50 μm.
[0063] (5) After the pulse action, a black graphene solution is obtained, which is ultrasonically dispersed for 20 minutes, washed with deionized water 2-3 times, and then filtered with a 0.22 μm water filter membrane and freeze-dried to obtain a graphene product.
[0064] according to Figure 2 It can be seen that the graphene products obtained in different inorganic salt solutions all present a micron-sized graphene thin layer state with a wrinkled texture. The graphene obtained in the sodium sulfate solution presents different lamellae structure stacking morphology, the edges of the lamellae are transparent and light, the graphene obtained in the sodium perchlorate solution has a larger lateral scale and thinner lamellae, and the graphene lamellae obtained in the sodium carbonate solution and the sodium chloride solution are found to be thicker and the degree of exfoliation is not complete.
[0065] according to Figure 3 It can be seen that the microscopic morphology and number of layers of graphene produced in different inorganic salt solutions can be seen through a transmission electron microscope. It can be found that the number of graphene layers produced in sodium sulfate solution is about 2 layers, the number of graphene layers produced in sodium perchlorate solution is 3 to 5 layers, the number of graphene layers produced in sodium carbonate solution is about 5 layers, and the number of graphene layers produced in sodium chloride solution reaches 10 layers.
[0066] according to Figure 4 It can be seen that (a) shows that the graphene prepared in different inorganic salt solutions all have graphene phase; (b) is the nitrogen adsorption-desorption curve, which shows that the specific surface areas of graphene prepared in sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution, and sodium chloride solution are 430 m 2 / g, 217m 2 / g, 167m 2 / g, 109m 2 / g, the graphene prepared in sodium sulfate solution has the highest specific surface area; (c) is the Raman spectrum, the ratio of the D peak and the G peak intensity can reflect the degree of defects in graphene, and the graphene prepared in sodium sulfate solution has the smallest ID / IG ratio, indicating the least defects and the best quality; (d) is the XPS full spectrum of graphene prepared in different inorganic salt solutions, through which the carbon-oxygen atomic ratio of each sample can be obtained. The carbon-oxygen atomic ratios of the graphene samples prepared in sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution, and sodium chloride solution are: 5. 25, 3.04, 2.29, 4.65, it can be concluded that the graphene prepared in sodium sulfate solution has the lowest oxygen content; (eh) Figure is the carbon spectrum of graphene prepared in different inorganic salt solutions. The carbon atom bonding conditions of different samples are obtained by fitting the C1s peak. The four binding energy positions at 284.5eV, 285.45eV, 386.65eV, and 288.4eV correspond to C=C bond, CC bond, CO bond, and C=O bond, respectively. By fitting the peak area, the four bonding area proportions shown in Table 1 can be obtained.
[0067] Table 1 Carbon atom bonding peak area ratio (%) of C1s spectra of four samples
[0068]
[0069] according to Figure 5 It can be seen that (a) shows that the CV background current of the graphene sample obtained in the sodium sulfate solution is the highest, and (c) shows that at 1 mA / cm 2 At a current density of 2.5 Å, the capacitance values of graphene prepared in sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution, and sodium chloride solution were 257 mF / cm 2 、160mF / cm 2 , 107mF / cm 2 、28mF / cm 2 , proving that the graphene sample obtained in sodium sulfate solution has the highest capacitance value. Figure (e) shows that the electrochemical impedance values of graphene samples obtained in sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution, and sodium chloride solution are 0.36149Ω, 0.56436Ω, 0.62464Ω, and 0.97891Ω, respectively, and the solution resistance is 1.043Ω, 1.057Ω, 1.54Ω, and 2.087Ω, indicating that the graphene obtained in sodium sulfate solution has the lowest resistance value and exhibits the best conductivity. Figure (f) shows that after 10,000 cycles of charge and discharge, the capacitance retention rate of graphene obtained in sodium sulfate solution is more than 90%, while the capacitance retention rate of graphene obtained in sodium perchlorate solution decays to less than 80%.
[0070] according to Figure 6It can be seen that the graphene peeled in pure water presents a larger unpeeled graphite block morphology. By performing voltammetric and cyclic voltammetric tests on the samples, it can be found that the capacitance value of the graphene peeled in pure water at 5mV / s is 18mF / cm 2 , the overall capacitance is low, and with the increase of scanning speed, the capacitance decreases rapidly, and the capacitance retention rate is 66.67%. In the comparative example, there are many graphite agglomerates on the surface of the graphene obtained by pure water stripping, which are not fully separated, and the stacking structure of these agglomerates is relatively dense. Compared with the preparation of graphene by stripping with inorganic salt solution, the graphene obtained in the comparative example shows obvious disadvantages in terms of electrochemical performance.
[0071] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing graphene by pulsed liquid phase discharge, characterized in that: The following steps are involved: The anode of the pulse power supply is connected in parallel with multiple graphite sheet targets, and the cathode is a graphite sheet. The cathode is completely immersed in an inorganic salt solution, and the anode target is placed above the inorganic salt solution; the pulse power supply is started, pulse stripping is performed, and then graphene is obtained through solid-liquid separation.
2. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The anode is connected in parallel with 2 to 6 graphite sheet targets, and the thickness of the graphite sheet targets is 1 to 2 mm.
3. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The thickness of the cathode graphite sheet is 2-5 mm.
4. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The inorganic salt solution is sodium sulfate solution, sodium perchlorate solution, sodium carbonate solution or sodium chloride solution.
5. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The volume of the inorganic salt solution is 300 ml, and the concentration of the inorganic salt solution is 0.1-0.5M.
6. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The anode target is 1.3-1.7 cm away from the inorganic salt solution.
7. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The current of the pulse power supply is 2-7A, the discharge machining pulse working cycle ranges from 100-300μs, the pulse rest cycle ranges from 100-300μs, and the discharge gap is set to 25-75μm.
8. The method for preparing graphene by pulsed liquid phase discharge method according to claim 1, characterized in that: The pulse stripping time is 10 to 30 minutes.
9. Graphene is obtained by the method for preparing graphene by pulsed liquid phase discharge method as described in any one of claims 1 to 8.
10. Use of graphene prepared by the method for preparing graphene by pulsed liquid phase discharge method according to any one of claims 1 to 8 in supercapacitor electrodes.
Citation Information
Patent Citations
Graphene preparation method, and graphene prepared through using method
CN102815694A
Preparation method of high specific surface area graphene
CN105347330A
Method and device for electrochemically preparing graphene oxide
CN111032568A
Method for preparing high-quality graphene through double-pulse electrochemical technology
CN112978721A
Preparation method of graphene and graphene
CN113249741A