Method for removing impurities from lithium-containing material
Through anhydrous ethanol dissolution method and blended solution distillation technology, the efficiency and purity of potassium and sodium impurities removal in lithium battery materials in the prior art were solved, and high-purity and high yield lithium salt products were achieved, and the process was simplified. And reduce costs.
Patent Information
- Application Number
- CN202411199849.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
The prior art has problems such as low purity, high cost, complex process and low efficiency when removing potassium and sodium ions from lithium battery materials. Especially in the development of high-nickel ternary materials, it is difficult to effectively remove monovalent lithium. Potassium and sodium impurities in chemicals.
The impurities are initially removed by anhydrous ethanol dissolution method, and then by forming a blended solution and adjusting the distillation end point, the organic solvent-water solubility difference of lithiate and sodium/potassium impurity salts in different proportions can be achieved efficiently remove impurities and reduce lithium salts. Loss and distillation losses.
The acquisition of high-purity lithium salt products has been achieved, with high yield, small losses and low distillation losses, which simplifies the process flow and reduces production costs.
Smart Images

Figure CN119080032A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of battery materials, and in particular to a method for removing impurities from lithium-containing materials. Background Art
[0002] With the vigorous development of new energy vehicles, the lithium battery positive electrode material market has gradually shifted from lithium iron phosphate to ternary composite materials, especially the development of high-nickel ternary materials, which has prompted the lithium salt market demand to gradually shift from lithium carbonate to lithium hydroxide / lithium chloride. Therefore, it is of great significance to study and prepare high-quality lithium hydroxide / lithium chloride products. From the perspective of lithium extraction technology, whether it is lithium extraction from ore or brine, the current main technology is the wet process, that is, lithium and other elements enter the solution together, and lithium is subsequently extracted from the solution. Among them, since potassium, sodium and other ions are monovalent and belong to the same group of elements as lithium ions, and their properties are similar, it is more difficult to remove potassium and sodium ions.
[0003] There are several traditional methods for removing potassium and sodium from monovalent lithium compounds: ① Lithium sulfate freezing method: add sodium hydroxide to the lithium concentrate after roasting, acidification, pulping, and leaching to obtain a preliminary concentrated lithium sulfate solution, cool and freeze to 5°C to 10°C, and precipitate sodium sulfate to obtain lithium hydroxide monohydrate. However, Na is not completely removed, and a large amount of Na2SO4 will remain in the solution, reducing the purity of lithium hydroxide. ② Electrolysis method: brine or lithium sulfate, lithium carbonate is used as raw materials, and lithium hydroxide is obtained by ion migration under the action of an electric field. Prior art A method for removing sodium and potassium from a lithium sodium potassium solution, the steps of which include: subjecting the lithium sodium potassium solution to electrodialysis, wherein the sodium and potassium ions migrate under the action of an electric field, thereby removing sodium and potassium, and obtaining a lithium-containing solution, and then obtaining lithium hydroxide through other treatments. The cost of the permeable membrane in this method is relatively high, and the instability requires frequent replacement, which increases costs. ③ Adding a sodium removal agent to the lithium product: In the prior art, according to Na + A special refining agent is added to a concentration of 5wt% to obtain a refined liquid. However, this method depends on the refining agent, which increases the cost of the refining agent and the complexity of the refining process. ④ Multiple recrystallization method: The prior art evaporates and concentrates the lithium hydroxide aqueous solution to a slurry solid content of 5wt% to 10wt%, then cools and cools to 30°C to 40°C, precipitates lithium hydroxide monohydrate crystals, separates the slurry solid-liquid, and washes the crystals to obtain lithium hydroxide monohydrate wet crystals. The obtained lithium hydroxide monohydrate product is not pure enough, and the recrystallization production process is repeated until lithium hydroxide monohydrate crystals with qualified product quality are obtained. Although this method is simple, it has the problems of unstable product quality, repeated production operations, and low production efficiency. Therefore, a new simple method for removing sodium and potassium ions from a solid or solution (lithium-containing material) containing lithium ions, sodium ions and potassium ions is needed. Summary of the invention
[0004] In view of this, the present application provides a method for removing impurities from a lithium-containing material. First, the lithium-containing material is dissolved in anhydrous ethanol, insoluble impurities are removed by filtration, and then an appropriate amount of water is added to the ethanol solution of high-concentration lithium salt to form a blended solution. The blended solution is distilled and crystallized, and the ethanol concentration in the mother liquor at the end point of the distillation is coordinated and controlled, so that a high-purity lithium salt product can be precipitated, and the lithium salt loss is small, the yield is high, and the distillation loss is low.
[0005] In a first aspect, the present application provides a method for removing impurities from a lithium-containing material, wherein the lithium-containing material contains a lithium compound and impurities, wherein the lithium compound includes at least one of LiCl and LiOH, and the impurities include at least one of NaCl and KCl, and optionally at least one of NaOH and KOH.
[0006] The method comprises at least the following steps:
[0007] S1, obtain lithium-containing material, add anhydrous ethanol to dissolve the lithium-containing material, filter, obtain crude lithium-containing filtrate and filter residue, the filter residue contains at least one impurity, S2, add water to the crude lithium-containing filtrate to obtain a blended solution, and then distill the blended solution to obtain a solid-liquid mixture containing solids and mother liquor, S3, filter the solid-liquid mixture, and then wash and dry the solid to obtain a high-purity lithium compound. The mother liquor includes unremoved impurities and a composite solvent, the unremoved impurities are dissolved in the composite solvent, the composite solvent includes water and ethanol, and the mass percentage of the ethanol is n wt% based on the mass of the composite solvent, and the value range of n is 50≤n≤70.
[0008] Both monovalent lithium compounds and sodium / potassium impurity salts have high solubility in water. The prior art uses pure water to remove sodium / potassium impurity salts from lithium-containing materials, which will result in a large loss of lithium, reduce the yield of lithium salts, and require multiple recrystallizations, increase the experimental process, and increase costs. In view of the miscibility of water and some organic solvents, this application first uses an ethanol solution to remove most of the impurities in the lithium-containing material, and then adds water for distillation and crystallization. The solubility difference of lithium compounds and sodium / potassium impurity salts in organic solvent-water blended solutions at different proportions is used to dissolve the lithium compounds as little as possible in the mixed solvent, while the sodium / potassium impurity salts are guaranteed to dissolve as much as possible, thereby achieving efficient removal of sodium / potassium impurity salts from lithium-containing materials.
[0009] The present application first dissolves the lithium-containing material (solid) in anhydrous ethanol, removes insoluble impurities by filtering to obtain an ethanol solution of high-concentration lithium salt (crude lithium-containing filtrate), and then adds a certain proportion of water to the ethanol solution of high-concentration lithium salt to form a mixed solution, and then the lithium salt product can be precipitated by distillation, crystallization and regulation of the distillation end point. In this way, on the one hand, the present application regulates the composite solvent in the mother liquor at the end point of the distillation so that the ethanol content is within the range of 50≤n≤70, which can ensure that the impurities are completely dissolved in the solvent at the end point of the distillation, the loss of lithium salt is minimized, and the direct yield is improved. On the other hand, the solvent is evaporated and collected in the form of an azeotrope (ethanol-water), which can reduce the boiling point of the solution, reduce distillation losses, and improve efficiency.
[0010] In some embodiments, in step S1, the amount of anhydrous ethanol added is m 醇 The method for determining the mass of the lithium compound in the lithium-containing material is as follows: S1-a, obtaining the mass of the lithium compound in the lithium-containing material, denoted as m 锂 , S1-b, according to the mass m of the lithium compound 锂 And the solubility S of the lithium compound in anhydrous ethanol 锂 , determine the amount of anhydrous ethanol added m 醇 , unit: g. The lithium compound is LiCl, and the solubility of LiCl in anhydrous ethanol ranges from 115 g / L to 125 g / L. The lithium compound is LiOH, and the solubility of LiOH in anhydrous ethanol ranges from 1.3 g / 100 g to 1.4 g / 100 g.
[0011] In some embodiments, step S1-b includes: step S1-b1, according to the mass m of the lithium compound 锂 And the solubility S of the lithium compound in anhydrous ethanol 锂 , determine the theoretical addition amount m of the anhydrous ethanol 理 Step S1-b2: according to the theoretical amount of anhydrous ethanol added m 理 , through formula Ⅰ, the amount of anhydrous ethanol added m can be obtained 醇 ;
[0012] m 理 ≤m 醇 ≤m 理 ╳k1 Formula Ⅰ
[0013] Among them, the value range of k1 is 1.0≤k1≤1.5.
[0014] In the present application, the solubility range of LiCl in anhydrous ethanol is selected as 115g / L to 125g / L, and the solubility range of LiOH in anhydrous ethanol is selected as 1.3g / 100g to 1.4g / 100g. According to the type and mass of the lithium compound and the corresponding solubility in anhydrous ethanol, the theoretical amount of anhydrous ethanol added can be determined, and then the actual amount of anhydrous ethanol added in the present application (m 醇 ), in this way, most of the impurities can be removed after dissolving and filtering the lithium-containing material, and the obtained crude lithium-containing filtrate is an ethanol solution of high-concentration lithium salt, and the loss of lithium salt in the lithium-containing material is small, which is beneficial to improve the yield of the lithium salt product.
[0015] In the present application, the solubility of the lithium compound in ethanol fluctuates slightly due to the influence of the actual physical and chemical environment, so the solubility of the lithium compound in ethanol can take any value within the above range.
[0016] Exemplarily, the dissolution conditions include: dissolution temperature: 55°C to 65°C, and dissolution time: 1h to 2h.
[0017] In some embodiments, in step S2, the amount of water added is m 水 Methods for determining include:
[0018] S2-a, pre-obtaining the mass m of the composite solvent used to dissolve the impurities not removed 复 ;
[0019] The impurities not removed refer to the other substances except the lithium compound in the crude lithium-containing filtrate after the lithium-containing material is dissolved and filtered with anhydrous ethanol in step S1, and the lithium compound and the other substances are dissolved in the crude lithium-containing filtrate;
[0020] S2-b, according to the mass m of the composite solvent 复 The content of ethanol in the composite solvent is n'wt%, and the mass of ethanol in the composite solvent is m 醇1 ;
[0021] Wherein, n' is selected from any value in the value range of n;
[0022] S2-c, according to the mass m of ethanol in the composite solvent 醇1 And the amount of anhydrous ethanol added in step S1 is m 醇 , through formula II, we can get the mass m of ethanol distilled during the distillation process 醇2 ;
[0023] m 醇2 =m 醇 -m 醇1 Formula II
[0024] S2-d, according to the mass m of distilled ethanol 醇2 , through formula III, we can get the mass m of water distilled during the distillation process 水2 ;
[0025]
[0026] Wherein, in formula III, the range of k2 is 0.95≤k2≤1.05;
[0027] S2-e, according to the mass m of the distilled water 水2 and the mass m of water in the composite solvent 水1 , through formula Ⅳ, the water addition amount m can be obtained 水 ;
[0028] m 水 =m 水2 +m 水1 Formula IV.
[0029] In some embodiments, step S2-a includes:
[0030] S2-a1, obtaining the mass m of the impurities not removed in the crude lithium-containing filtrate by detection 杂 ;
[0031] Wherein, the mass of the impurities not removed is m 杂 Measured by the mass of the target impurity, the target impurity is the chloride salt with the largest mass among NaCl and KCl;
[0032] S2-a2, obtaining the solubility S of the target impurity in the composite solvent 杂 , unit: g / 100g;
[0033] Wherein, the ethanol content in the composite solvent is n'wt%;
[0034] S2-a3, according to the mass m 杂 and solubility S 杂 , the mass m of the composite solvent used to dissolve the impurities not removed can be obtained in advance 复 .
[0035] In some embodiments, step S2-a3 comprises:
[0036] When the mass of the impurities not removed m 杂 When the impurities are greater than 0.5 g, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance according to formula V-1. 复 ;
[0037]
[0038] Among them, the value range of k3 is 1.0≤k3≤1.5.
[0039] When the mass of impurities not removed is large (m 杂 >0.5g), the mass of the composite solvent in the mother liquor needs to be controlled within the above range, so that it is conducive to better dissolving the impurities that have not been removed and precipitating the lithium salt product, and the lithium salt product has high purity and good yield.
[0040] When the mass of the impurities not removed m 杂 ≤0.5g, according to formula V-2, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance 复 ;
[0041]
[0042] Among them, the value range of p1 is 2≤p1≤10, and the value range of p2 is 12≤p2≤18.
[0043] When the mass of impurities not removed is less (m 杂 ≤0.5g), the mass of the composite solvent in the mother liquor needs to be appropriately increased and within the above range. Otherwise, if the amount of the composite solvent is too small, the solid-liquid mixture will be more viscous, resulting in the inability to filter and obtain the lithium salt product subsequently.
[0044] The present application obtains a blended solution by adding an appropriate amount of water in step S2. The blended solution can make as much solid phase of the lithium compound as possible precipitate by regulating the ethanol concentration of the composite solvent in the mother liquor during the negative pressure distillation process, and the sodium and potassium impurities are dissolved in the mother liquor as much as possible, so that the crude lithium-containing filtrate after dissolution and filtration with anhydrous ethanol can further remove the sodium and potassium impurities, thereby achieving high purity and high yield of the lithium compound. Too much water content in the blended solution will lead to excessive loss of lithium salts, which is not conducive to taking into account the high yield of the lithium compound, while too little water content in the blended solution is not conducive to removing the sodium and potassium impurities in the crude lithium-containing filtrate, which is not conducive to taking into account the high purity of the lithium compound. It can be seen that the blended solution prepared by the above-mentioned calculated amount of water addition and the ethanol concentration n of the composite solvent in the mother liquor after negative pressure distillation are also suitable, which can take into account the high purity and high yield of the lithium compound.
[0045] Exemplarily, the conditions for negative pressure distillation include: vacuum degree: -0.06MPa to -0.04MPa, distillation temperature: 85°C to 90°C.
[0046] Specifically, in the present application, ethanol + water are distilled and separated according to a mass ratio of about 95.6:4.4, so that the lithium compound dissolved in the fraction is precipitated, and the amount of water added is adjusted to make the ethanol content in the remaining mother liquor within 50wt% to 70wt%, and the sodium potassium impurities are dissolved in the mother liquor as much as possible, so that the sodium potassium impurities not removed in the first step are separated from the lithium compound. In a composite solvent with an ethanol content of 50wt% to 70wt%, the solubility of the lithium compound and the sodium potassium impurities is quite different, the sodium potassium impurities have a higher solubility in the composite solvent, and the lithium compound (LiCl, LiOH) has a lower solubility in the composite solvent. By utilizing the solubility difference, the precipitation of sodium potassium impurities is avoided as much as possible, the purity of the lithium compound is improved, and the lithium compound is precipitated in large quantities, thereby ensuring the yield of the lithium compound.
[0047] In some embodiments, the lithium-containing material is a solid lithium-containing material, or the lithium-containing material is a solid lithium-containing material obtained by negative pressure evaporation of a liquid lithium-containing material. Based on the mass of the lithium-containing material, the mass percentage of the lithium compound is W1 wt%, W1≥30, and the mass percentage of the impurities is W2wt%, 10≤W2≤70. Preferably, at least one of the following conditions is met: (1) 60≤n≤65; (2) 55≤W1≤75; (3) 30≤W2≤45. The present application further regulates the state, parameters and conditions of the distillation end point of the lithium-containing material within the above range, which is more conducive to the removal of impurities from the lithium-containing material, especially the removal of potassium, sodium and other ions that are monovalent and in the same group as lithium ions, while taking into account the improvement of the yield of lithium salt products.
[0048] In some embodiments, in step S3, the filtered mother liquor is returned to the lithium-containing material in step S1 after negative pressure operation. + This is because LiCl and LiOH also have a certain solubility in the composite solvent of ethanol and water. The mother liquor is converted into a solid lithium-containing material through negative pressure operation and then circulated, which further improves the yield of the lithium salt product.
[0049] In some embodiments, in step S3, during the solid washing process, the detergent contains ethanol and water, the mass content of ethanol in the detergent is nwt%, and the washing times are 2 to 3 times. Preferably, the detergent (containing Li + ), and after negative pressure operation, returns to the lithium-containing material in step S1. The detergent after washing contains Li + , which is converted into a solid lithium-containing material through negative pressure operation and then circulated, which is beneficial to improving the yield of lithium salt products.
[0050] In some embodiments, the vacuum drying conditions include: vacuum temperature: 145° C. to 155° C., vacuum time: 1 h to 3 h.
[0051] The present application first dissolves the lithium-containing material in anhydrous ethanol to remove most of the impurities, and adds an appropriate amount of water to the ethanol solution of the obtained high-concentration lithium salt to form a mixed solution. During the negative pressure distillation process, the mixed solution can make the lithium compound precipitate in the solid phase with a high yield by regulating the ethanol concentration of the composite solvent in the mother liquor, and the impurities that have not been removed are dissolved in the mother liquor to a large extent, especially at the end point of the distillation, the impurities are almost completely dissolved in the mother liquor, and the loss of the lithium salt product is small and the purity is high. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0053] Figure 1 This is a schematic diagram of the process flow of the method for removing impurities from lithium-containing materials in this application. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0055] The inventive concept of this process is: sodium and potassium impurities in the lithium compound are removed in two steps. In the first step, most of the impurities with low solubility in the lithium compound are removed by using anhydrous ethanol (precipitated in the form of precipitation) to obtain an ethanol solution of high-concentration lithium salt. Then, in the second step, water is added to the obtained ethanol solution of high-concentration lithium salt, and the lithium compound is precipitated in the solid phase by negative pressure distillation and regulating the concentration of ethanol in the mother liquor, while the sodium and potassium impurities are dissolved in the mother liquor as much as possible, and the sodium and potassium impurities are further removed. This process takes into account both the purity and yield of the lithium compound.
[0056] Method for removing impurities from lithium-containing materials
[0057] The lithium-containing material contains lithium compounds and impurities, wherein the lithium compounds include at least one of LiCl and LiOH, and the impurities include at least one of NaCl and KCl, and optionally at least one of NaOH and KOH.
[0058] See also Figure 1 , including the following steps:
[0059] S1. Obtain a lithium-containing material, add anhydrous ethanol to dissolve the lithium-containing material, and filter to obtain a crude lithium-containing filtrate and a filter residue, wherein the filter residue contains at least one impurity;
[0060] S2, adding water to the crude lithium-containing filtrate to obtain a blended solution, and then distilling the blended solution to obtain a solid-liquid mixture containing solids and mother liquor;
[0061] S3, filtering the solid-liquid mixture, and then washing and drying (vacuum drying) the solid (high-purity lithium-containing solid) to obtain a high-purity lithium compound (lithium salt product);
[0062] The mother liquor includes unremoved impurities and a composite solvent, the unremoved impurities are dissolved in the composite solvent, the composite solvent includes water and ethanol, and based on the mass of the composite solvent, the mass percentage of ethanol is nwt%, and the value range of n is 50≤n≤70.
[0063] The method of the present application mainly includes two steps, the first step is to dissolve the solid lithium-containing material in anhydrous ethanol, remove insoluble impurities by dissolving and filtering, and obtain an ethanol solution of high-concentration lithium salt (coarse lithium-containing filtrate), the first step can remove most of the insoluble impurities in the lithium-containing material, including NaCl, KCl, NaOH, KOH or other impurities, the second step is to add an appropriate amount of water to the ethanol solution of high-concentration lithium salt to form a blended solution, the addition of water in the second step is very critical, the addition of water is too little, resulting in the lithium compound cannot be efficiently precipitated, and the mother liquor is too viscous, and the subsequent lithium compound product cannot be obtained at a high rate, and the addition of water is too much, the lithium salt loss is large (cannot be efficiently precipitated), and the yield is low. At the same time, the blended solution needs to coordinate the ethanol concentration of the composite solvent in the mother liquor during the distillation and crystallization process to make the lithium compound precipitate as much as possible while dissolving as much impurities as possible, which is beneficial to improve the direct yield and purity, and the solvent is evaporated and collected in the form of an azeotrope (ethanol-water), which can reduce the boiling point of the solution, reduce distillation losses, and improve efficiency.
[0064] In the present application, the mass content of ethanol in the composite solvent is 50wt% to 70wt%. At this time, the solubility of the lithium compound and the solubility of the impurities are greatly different, about 1:4, so the lithium compound can be effectively precipitated in the solid phase and the impurities can be dissolved in the liquid phase as much as possible.
[0065] In this process, the mass content of ethanol in the composite solvent is 50wt% to 70wt%, which can be determined by any suitable method according to the teachings of this application by those skilled in the art. A possible method is described below:
[0066] Step S100, using the mass ratio of the organic solvent in the mixed solvent as the horizontal coordinate and the solubility of the target impurity as the vertical coordinate, fitting and determining the corresponding relationship curve y1=f1 between the solubility of the target impurity and the mass ratio of the organic solvent in the mixed solvent 1 (n) , f 1 (n) is a quadratic function of n;
[0067] Step S200, using the mass ratio of the organic solvent in the mixed solvent as the horizontal coordinate and the solubility of lithium hydroxide and / or lithium chloride as the vertical coordinate, fitting and determining the corresponding relationship curve y2=f between the solubility of the lithium compound and the mass ratio of the organic solvent in the mixed solvent 2 (n) , f 2 (n) is a quadratic function of n;
[0068] Step S300, according to y1=f 1 (n) and y2 = f 2 (n) , determine the range of n values, including:
[0069] According to formula I, two real roots n1 and n2 are determined, and n1<n2;
[0070] f 1 (n) / f 2 (n) ≥Q Formula I
[0071] Among them, the value range of Q is 3≤Q≤4.5;
[0072] The value range of n is n1≤n≤n2.
[0073] <Method for determining the amount of anhydrous ethanol added>
[0074] S1-a, obtain the mass of lithium compound in the lithium-containing material, denoted as m 锂 ;
[0075] S1-b, according to the mass m of the lithium compound 锂 And the solubility S of lithium compounds in anhydrous ethanol 锂 , determine the amount of anhydrous ethanol added m 醇 , unit: g.
[0076] Wherein, step S1-b includes: step S1-b1, according to the mass m of the lithium compound 锂 And the solubility S of the lithium compound in anhydrous ethanol 锂 , determine the theoretical addition amount m of the anhydrous ethanol 理 ; Step S1-b2, according to the theoretical amount of anhydrous ethanol added m 理 , through formula Ⅰ, the amount of anhydrous ethanol added m can be obtained 醇 ;
[0077] m 理 ≤m 醇 ≤m 理 ╳k1 Formula Ⅰ
[0078] Among them, the value range of k1 is 1.0≤k1≤1.5.
[0079] In the present application, the solubility of LiCl in anhydrous ethanol ranges from 115 g / L to 125 g / L, and the solubility of LiOH in anhydrous ethanol ranges from 1.3 g / 100 g to 1.4 g / 100 g.
[0080] <Method for determining the amount of water added>
[0081] S2-a, pre-obtaining the mass m of the composite solvent used to dissolve the impurities not removed 复 .
[0082] Step S2-a includes:
[0083] S2-a1, obtaining the mass m of the impurities not removed in the crude lithium-containing filtrate by detection 杂 ;
[0084] Wherein, the mass of the impurities not removed is m 杂 Measured by the mass of the target impurity, the target impurity is the chloride salt with the largest mass among NaCl and KCl;
[0085] S2-a2, obtaining the solubility S of the target impurity in the composite solvent 杂 , unit: g / 100g; wherein the ethanol content in the composite solvent is n'wt%;
[0086] In this process, the solubility S of the target impurity in the composite solvent is 杂 The method for obtaining the solubility S of the target impurity can be obtained by those skilled in the art according to actual needs, for example, a composite solvent with an ethanol content of n'wt% is directly prepared, and the target impurity is slowly added to obtain its solubility S 杂 Of course, you can also configure composite solvents with different ethanol proportions of n'wt%, obtain the solubility of the corresponding target impurities therein, and then draw a corresponding relationship curve. According to the corresponding relationship curve, calculate the solubility of the target impurity when the ethanol content is n'wt%.
[0087] S2-a3, according to the mass m 杂 and solubility S 杂 , the mass m of the composite solvent used to dissolve the impurities not removed can be obtained in advance 复 .
[0088] Wherein, when the mass of the impurities not removed m 杂 When the impurities are greater than 0.5 g, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance according to formula V-1. 复 ;
[0089]
[0090] Wherein, the value range of k3 is 1.0≤k3≤1.5; or,
[0091] When the mass of the impurities not removed m 杂 ≤0.5g, according to formula V-2, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance 复 ;
[0092]
[0093] Among them, the value range of p1 is 2≤p1≤10, and the value range of p2 is 12≤p2≤18.
[0094] S2-b, according to the mass m of the composite solvent 复 The content of ethanol in the composite solvent is n'wt%, and the mass of ethanol in the composite solvent is m 醇1 ;
[0095] Wherein, n' is selected from any value in the value range of n.
[0096] S2-c, according to the mass m of ethanol in the composite solvent 醇1 And the amount of anhydrous ethanol added in step S1 is m 醇 , through formula II, we can get the mass m of ethanol distilled during the distillation process 醇2 ;
[0097] m 醇2 =m 醇 -m 醇1 Formula II.
[0098] S2-d, according to the mass m of distilled ethanol 醇2 , through formula III, we can get the mass m of water distilled during the distillation process 水2 ;
[0099]
[0100] Wherein, in formula III, the range of k2 is 0.95≤k2≤1.05.
[0101] S2-e, according to the mass m of the distilled water 水2 and the mass m of water in the composite solvent 水1 , through formula Ⅳ, the water addition amount m can be obtained 水 ;
[0102] m 水 =m 水2 +m 水1 Formula IV.
[0103] The following are possible implementations
[0104] The main process of the technical solution proposed in this application may include the following five main steps: 1. obtaining lithium salt material (lithium-containing material), which is in solid form; 2. dissolving, filtering and removing impurities with ethanol solution (anhydrous ethanol); 3. adding water to prepare a certain proportion of mixed lithium salt solution (blended solution), and crystallizing lithium salt by negative pressure distillation; 4. filtering and washing to obtain lithium salt solid; 5. vacuum drying to obtain high-purity lithium salt. The product of this process is a high-purity lithium salt product.
[0105] The raw material to be purified (solid or solution in OH - , Cl - 、SO4 2- Anion) is obtained by a series of operations such as negative pressure distillation to obtain high-purity lithium salt solid.
[0106] In this process, the purity of lithium salt in the lithium-containing material is greater than or equal to 30wt%, and the main impurities are NaCl, KCl, NaOH, KOH, etc. (content 10-70wt%, and a small amount of other impurities content 0-2wt%).
[0107] First, the solid material enters the ethanol dissolution, filtration and impurity removal stage. The amount of ethanol required is calculated based on the solubility of lithium salt in ethanol in the material, and the amount used is 1-1.5 times the theoretical amount corresponding to the saturated solubility of lithium salt. After dissolution, the solid impurities insoluble in ethanol are filtered out to initially obtain a high-concentration lithium salt ethanol solution.
[0108] A certain proportion of water is added to the ethanol solution of lithium salt, and the water content is ensured to ensure that ethanol: water is distilled and separated according to a mass ratio of 95.6:4.4 during the distillation operation, and the ethanol in the remaining mother liquor accounts for 50wt% to 70wt% of the composite solvent (for example, 64.16wt%), ensuring that the impurities are completely dissolved in the solution and the lithium salt is dissolved as little as possible. Then the mixed solution is concentrated by negative pressure distillation to obtain a solid-liquid mixture, which is filtered and washed to obtain a lithium salt solid.
[0109] The filtrate containing sodium and potassium impurity ions and lithium salt solids are removed by filtering and washing, and the filter membrane is a 0.22μm organic filter membrane. The filtrate (mainly containing Na+, Li+, K cations, Cl-, OH-, SO4 2- The main anion is one of the main anions) and then returned to the first process to extract lithium salts, and the fractions are processed and recycled. The vacuum degree is -0.06MPa to -0.04MPa.
[0110] The washing liquid is selected to be a solution with the same mass ratio of ethanol: water as that in the mother liquor for elution, and the washing is performed three times and the elution liquid is recovered and returned to the first process together with the filtrate for cyclic extraction of lithium salt.
[0111] Finally, the filtered solid is vacuum dried to obtain a high-purity lithium salt product. The vacuum drying temperature is controlled at 100°C-190°C, and the drying time is 1-4 hours. The evaporation and drying process is conducive to controlling CO3 2- , reducing the Li element to exist in the form of Li2CO3.
[0112] Hereinafter, examples and comparative examples are given to more specifically illustrate the embodiments of the present application. Unless otherwise stated, the parts, percentages and ratios listed are all based on mass.
[0113] Example 1
[0114] Step S1: Take 20 g of lithium salt solid (mainly composed of LiCl, NaCl and KCl, of which LiCl accounts for 56%, KCl accounts for 19%, and NaCl accounts for 25%) as the initial raw material (lithium-containing material), add 100 mL (about 79 g) of anhydrous ethanol according to the solubility of LiCl of 120 g / L (test data, NaCl in the solution is about 1.1 g, KCl is about 0.2 g), stir at 60° C. for 1 h, and then perform solid-liquid separation operation to remove most of the insoluble impurities NaCl (about 3.9 g) and KCl (about 3.6 g);
[0115] Step S2: add 13.55g (including 10.8g water in the mother liquor + 2.75g distilled water) of water to the ethanol solution of LiCl (crude lithium-containing filtrate), mix and stir for 0.5h, distill the mixed solution under negative pressure at 85°C (vacuum degree is -0.06MPa to -0.04MPa), stop distillation when the fraction mass is 62.55g (59.8g ethanol + 2.75 water), and obtain 30g of composite solvent containing 64wt% ethanol-water (theoretically soluble NaCl is 1.2g, soluble KCl is 0.37g), and perform solid-liquid separation operation when naturally cooled to room temperature, and wash the solid with 5mL×3 of 64wt% ethanol-water detergent;
[0116] Step S3: The collected solid was dried in a vacuum drying oven at 150° C. for 2 h to obtain 10.23 g of a high-purity LiCl product with a purity of 99.1% and a yield of 91.3%.
[0117] Specifically:
[0118] 1. The calculation process of the amount of anhydrous ethanol added is as follows:
[0119] Step S1-a: The mass of LiCl is 11.2 g, i.e., m 锂 11.2g;
[0120] Step S1-b: Theoretical addition amount of anhydrous ethanol m 理 for:
[0121] Step S1-b1, 11.2 g / m 理 =12g / (0.789g / mlⅹ100ml), m 理 =73.64g;
[0122] The amount of anhydrous ethanol added 醇 for:
[0123] Step S1-b2, m 理 ≤m 醇 ≤m 理 ⅹk1, when k1=1.1, 73.64≤m 醇 ≤81g, choose m 醇 =79g.
[0124] 2. The amount of water added m 水 The calculation of is as follows:
[0125] Step S2-a: Pre-obtaining the mass m of the composite solvent used to dissolve the impurities not removed 复 ;
[0126] Step S2-a1: Detect and obtain the mass m of the target impurity NaCl 杂 =1.1g;
[0127] Step S2-a2: Take the content of ethanol in the composite solvent used to dissolve the impurities not removed as n'wt% = 64wt%; obtain the solubility S of NaCl in the composite solvent containing 64wt% ethanol 杂 =4g / 100g;
[0128] Step S2-a3: According to the mass m of the target impurity NaCl 杂 =1.1g (>0.5g), the mass m of the composite solvent is obtained 复 for:
[0129] 1.1gⅹ100g / 4g≤m 复 ≤k3ⅹ1.1gⅹ100g / 4g
[0130] When k3=1.1, 27.5g≤m 复 ≤30.25g, take m 复 =30g.
[0131] Step S2-b: obtaining the masses of ethanol and water in the composite solvent;
[0132] The mass of ethanol in the composite solvent m 醇1 =30 x 64 wt% = 19.2 g,
[0133] The mass of water in the composite solvent is m 水1 =30 x 36 wt% = 10.8 g;
[0134] Step S2-c: Obtaining the mass m of ethanol distilled during the distillation process 醇2 ;
[0135] The mass of ethanol distilled is m 醇2 =79g-19.2g=59.8g;
[0136] Step S2-d: Obtain the mass m of water distilled during the distillation process 水2 ;
[0137] The mass of distilled water m 水2 for:
[0138] 59.8 / m 水2 =95.6 / 4.4ⅹk2, when k2=1, m 水2 =2.75g;
[0139] Step S2-e: Obtaining the amount of water added m 水
[0140] Water addition amount m 水 =10.8+2.75=13.55g.
[0141] Example 2
[0142] Step S1: Take 10 g of lithium salt solid (mainly composed of LiOH, NaCl and NaOH, of which LiOH accounts for 70%, NaCl accounts for 23%, and NaOH accounts for 7%) as the initial raw material (lithium-containing material), add 600 g of anhydrous ethanol according to the solubility of LiOH of 1.33 g / 100 g (test data, NaCl in the solution is about 0.2 g, NaOH is about 0.5 g), stir at 60 ° C for 2 h, and then perform solid-liquid separation operation to remove most of the insoluble impurities NaCl (about 2.1 g) and a small amount of NaOH (about 0.2 g);
[0143] Step S2: add 50g (including 24g water in the mother liquor + 26g distilled water) water to the ethanol solution of LiOH (crude lithium-containing filtrate) and mix and stir for 0.5h, distill the mixed solution under negative pressure at 90°C (vacuum degree is -0.06MPa~-0.04MPa), and stop distilling when the fraction mass is 590g (564g ethanol + 26g water). The mother liquor is 60g of a mixed solution of 60wt% ethanol and water (if there is too little liquid phase in the mother liquor, it is relatively viscous, which affects the subsequent filtering effect), the theoretically soluble NaCl is 0.2ⅹ15g, and the dissolved NaOH is greater than 0.5g. When it is naturally cooled to room temperature, a solid-liquid separation operation is performed, and the solid is washed with 10mLⅹ3 of a detergent of 60wt% ethanol and water;
[0144] Step S3: The collected solid was dried in a vacuum drying oven at 150° C. for 2 h to obtain 6.09 g of high-purity LiOH product with a purity of 99.8% and a yield of 87%.
[0145] Specifically:
[0146] 1. The calculation process of the amount of anhydrous ethanol added is as follows:
[0147] Step S1-a: The mass of LiOH is 7 g, i.e., m 锂 7g;
[0148] Step S1-b1, theoretical amount of anhydrous ethanol added m 理 :7g / m 理 =1.33g / 100g, m 理 =526g;
[0149] Step S1-b2, the amount of anhydrous ethanol added m 醇 For: m 理 ≤m 醇 ≤m 理 ⅹk1,
[0150] When k1=1.2, 526≤m 醇 ≤631g, choose m 醇 =600g.
[0151] 2. The amount of water added m 水 The calculation of is as follows:
[0152] Step S2-a: Pre-obtaining the mass m of the composite solvent used to dissolve the impurities not removed 复 ;
[0153] Step S2-a1: Detect and obtain the mass m of the target impurity NaCl 杂 =0.2g;
[0154] Step S2-a2: taking the content of ethanol in the composite solvent used to dissolve the impurities not removed to n'wt%=60wt%;
[0155] Obtain the solubility S of NaCl in the composite solvent containing 60 wt% ethanol 杂 =5g / 100g;
[0156] Step S2-a3: According to the mass m of the target impurity NaCl 杂 =0.2g (≤0.5g), and the mass m of the composite solvent is obtained. 复 for:
[0157] p1×100×0.2 / 5≤m 母≤p2×100×0.2 / 5, take p1=10, p2=15, then 40g≤m 复 ≤60g,
[0158] Select m 复 = 60 g of composite solvent to dissolve the impurities that have not been removed;
[0159] Step S2-b: obtaining the masses of ethanol and water in the composite solvent;
[0160] The mass of ethanol in the composite solvent m 醇1 =60 x 60 wt% = 36 g;
[0161] The mass of water in the composite solvent is m 水1 =60 x 40 wt% = 24 g;
[0162] Step S2-c: Obtaining the mass m of ethanol distilled during the distillation process 醇2 ;
[0163] The mass of ethanol distilled is m 醇2 =600g-36g=564g;
[0164] Step S2-d: Obtain the mass m of water distilled during the distillation process 水2 ;
[0165] The mass of distilled water m 水2 for:
[0166] 564 / m 水2 =95.6 / 4.4ⅹk2, when k2=1, m 水2 =26g;
[0167] Step S2-e: Obtaining the amount of water added m 水
[0168] Water addition amount m 水 =24+26=50g.
[0169] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for removing impurities from a lithium-containing material, characterized in that: The lithium-containing material contains lithium compounds and impurities; The lithium compound includes at least one of LiCl and LiOH; The impurities include at least one of NaCl and KCl, and optionally at least one of NaOH and KOH; The method comprises at least the following steps: S1. Obtain a lithium-containing material, add anhydrous ethanol to dissolve the lithium-containing material, and filter to obtain a crude lithium-containing filtrate and a filter residue, wherein the filter residue contains at least one of the impurities; S2, adding water to the crude lithium-containing filtrate to obtain a blended solution, and then distilling the blended solution to obtain a solid-liquid mixture containing solids and mother liquor; S3, filtering the solid-liquid mixture, and then washing and drying the solid to obtain a high-purity lithium compound; Wherein, the mother liquor comprises unremoved impurities and a composite solvent, and the unremoved impurities are dissolved in the composite solvent; The composite solvent comprises water and ethanol. Based on the mass of the composite solvent, the mass percentage of the ethanol is n wt%, and the value range of n is 50≤n≤70.
2. The method according to claim 1, characterized in that In step S1, the amount of anhydrous ethanol added is m 醇 Methods for determining include: S1-a, obtaining the mass of the lithium compound in the lithium-containing material, denoted as m 锂 ; S1-b, according to the mass m of the lithium compound 锂 And the solubility S of the lithium compound in anhydrous ethanol 锂 , determine the amount of anhydrous ethanol added m 醇 , unit: g; Wherein, the lithium compound is LiCl, and the solubility of LiCl in anhydrous ethanol ranges from 115 g / L to 125 g / L; The lithium compound is LiOH, and the solubility of LiOH in anhydrous ethanol ranges from 1.3 g / 100 g to 1.4 g / 100 g.
3. The method according to claim 2, characterized in that Step S1-b includes: Step S1-b1, according to the mass m of the lithium compound 锂 And the solubility S of the lithium compound in anhydrous ethanol 锂 , determine the theoretical addition amount m of the anhydrous ethanol 理 ; Step S1-b2: according to the theoretical amount of anhydrous ethanol added m 理 , through formula Ⅰ, the amount of anhydrous ethanol added m can be obtained 醇 ; m 理 ≤m 醇 ≤m 理 ╳k1 Formula Ⅰ Among them, the value range of k1 is 1.0≤k1≤1.
5.
4. The method according to claim 1, characterized in that: In step S2, the amount of water added is m 水 Methods for determining include: S2-a, pre-obtaining the mass m of the composite solvent used to dissolve the impurities not removed 复 ; S2-b, according to the mass m of the composite solvent 复 The content of ethanol in the composite solvent is n'wt%, and the mass of ethanol in the composite solvent is m 醇1 ; Wherein, n' is selected from any value in the value range of n; S2-c, according to the mass m of ethanol in the composite solvent 醇1 And the amount of anhydrous ethanol added in step S1 is m 醇 , through formula II, we can get the mass m of ethanol distilled during the distillation process 醇2 ; m 醇2 =m 醇 -m 醇1 Formula II S2-d, according to the mass m of distilled ethanol 醇2 , through formula III, we can get the mass m of water distilled during the distillation process 水2 ; Wherein, in formula III, the range of k2 is 0.95≤k2≤1.05; S2-e, according to the mass m of the distilled water 水2 and the mass m of water in the composite solvent 水1 , through formula Ⅳ, the water addition amount m can be obtained 水 ; m 水 =m 水2 +m 水1 Formula IV.
5. The method according to claim 4, characterized in that Step S2-a includes: S2-a1, obtaining the mass m of the impurities not removed in the crude lithium-containing filtrate by detection 杂 ; Wherein, the mass of the impurities not removed is m 杂 Measured by the mass of the target impurity, the target impurity is the chloride salt with the largest mass among NaCl and KCl; S2-a2, obtaining the solubility S of the target impurity in the composite solvent 杂 , unit: g / 100g; Wherein, the ethanol content in the composite solvent is n'wt%; S2-a3, according to the mass m 杂 and solubility S 杂 , the mass m of the composite solvent used to dissolve the impurities not removed can be obtained in advance 复 .
6. The method according to claim 5, characterized in that Step S2-a3 includes: When the mass of the impurities not removed m 杂 When the impurities are greater than 0.5 g, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance according to formula V-1. 复 ; Wherein, the value range of k3 is 1.0≤k3≤1.5; or, When the mass of the impurities not removed m 杂 ≤0.5g, according to formula V-2, the mass m of the composite solvent used to dissolve the impurities not removed is obtained in advance 复 ; Among them, the value range of p1 is 2≤p1≤10, and the value range of p2 is 12≤p2≤18.
7. The method according to claim 1, characterized in that The lithium-containing material is a solid lithium-containing material, or the lithium-containing material is a solid lithium-containing material obtained by evaporating a liquid lithium-containing material under negative pressure; Preferably, based on the mass of the lithium-containing material, the mass percentage of the lithium compound is W1 wt%, W1≥30, and the mass percentage of the impurities is W2 wt%, 10≤W2≤70.
8. The method according to claim 7, characterized in that At least one of the following conditions is met: (1) 60≤n≤65; (2) 55≤W1≤75; (3)30≤W2≤45。 9. The method according to claim 1, characterized in that: In step S3, the filtered mother liquor is returned to the lithium-containing material in step S1 after negative pressure operation.
10. The method according to claim 1, characterized in that In step S3, during the solid washing process, the detergent contains ethanol and water, the mass content of the ethanol in the detergent is nwt%, and the number of washings is 2 to 3 times; Preferably, the detergent after washing is returned to the lithium-containing material in step S1 after negative pressure operation.
Citation Information
Patent Citations
Technology for extracting high-purity lithium chloride from lithium ore
CN106365180A
Method for purifying lithium salts
CN114728805A
Process method for preparing battery-grade lithium carbonate by recovering lithium chloride from organic reaction wastewater
CN116462212A
Method for extracting lithium chloride by using organic solvent
CN118324166A
Method for producing battery grade lithium hydroxide monohydrate
WO2021228936A1