Method for preparing sodium stannate from ultrasonic enhanced tin oxide sheet at low temperature

By using ultrasonic enhanced oxidation technology in the preparation of sodium stannate, ultrasonic waves generate free radicals with stronger oxidation performance under low temperature conditions, optimize the addition method of hydrogen peroxide, solve the problem of low dissolution efficiency of tin sheets, and achieve high efficiency and low energy consumption Sodium stannate is prepared, which significantly improves the utilization rate of hydrogen peroxide and the dissolution rate of tin.

CN119080055AActive Publication Date: 2024-12-06KUNMING UNIV OF SCI & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411267745.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

In the existing sodium stannate preparation process, the dissolution efficiency of tin sheets under low temperature conditions is low, the utilization rate of hydrogen peroxide is low, and the high temperature reaction leads to equipment corrosion, high energy consumption and serious environmental pollution.

Method used

Using ultrasonic enhanced oxidation technology, strictly control the temperature between 20 and 30℃, and use ultrasonic waves to generate free radicals with stronger oxidation performance. By optimizing the addition of hydrogen peroxide, the oxidation efficiency of hydrogen peroxide is improved, the dissolution of tin sheets is promoted, and the amount of hydrogen peroxide is reduced, and the amount of hydrogen peroxide is avoided. High temperature decomposition.

Benefits of technology

A highly efficient oxidation reaction at low temperatures was achieved, and the dissolution rate of tin reached more than 99%, which significantly shortened the reaction time, improved the utilization rate of hydrogen peroxide, and reduced energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005037652900000011
    Figure HDA0005037652900000011
  • Figure HDA0005037652900000021
    Figure HDA0005037652900000021
  • Figure HDA0005037652900000022
    Figure HDA0005037652900000022
Patent Text Reader

Abstract

The invention relates to a method for preparing sodium stannate at low temperature by using an ultrasonic enhanced tin oxide sheet, and belongs to the technical field of sodium stannate preparation. The method comprises the following steps: adding a high-purity tin sheet into a sodium hydroxide solution, controlling the temperature of the sodium hydroxide solution to be 20-30 DEG C under an ultrasonic condition, slowly adding hydrogen peroxide to 20-30% of a preset total addition amount, and continuing ultrasonic enhanced oxidation reaction for 7-10 minutes; hydrogen peroxide is slowly added multiple times, then the ultrasonic enhanced oxidation reaction continues, the adding amount of hydrogen peroxide every time is 10-15% of the preset total adding amount, and the ultrasonic enhanced oxidation reaction is conducted for 4-8 min after hydrogen peroxide is added every time; after hydrogen peroxide is completely added according to the preset total addition amount, the ultrasonic enhanced oxidation reaction continues until tin sheets are completely dissolved, and a sodium stannate solution is obtained; and sequentially filtering, concentrating, separating, washing and drying the sodium stannate solution to obtain a sodium stannate product. The oxidation reaction temperature is strictly controlled to be 20-30 DEG C, volatilization of hydrogen peroxide is reduced, the oxidation effect of hydrogen peroxide is enhanced through ultrasound, and the tin dissolving effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, and belongs to the technical field of sodium stannate preparation. Background Art

[0002] Sodium stannate is an important chemical raw material, and plays an important role in the fields of electroplating, textile, anti-corrosion, and organic synthesis catalyst. The production of sodium stannate mainly includes detinning, alkali fusion, and alkaline hydrolysis. Detinning method The detinning method is mainly used to recover secondary tin resources such as tinplate and tin-plating slag. It has problems such as low product purity, large amount of wastewater, unstable source of tin-containing waste, and is not conducive to stable industrial production. The alkali fusion method refers to a method in which cassiterite concentrate is used as a raw material, and a high-temperature melting reaction with sodium hydroxide is performed to generate a sodium stannate melt, and the sodium stannate product is obtained after cooling, leaching, impurity removal, filtration, crystallization, etc. However, it has problems such as strong corrosion to equipment, high cost, and complicated process.

[0003] Alkali hydrolysis is one of the most widely used and most mature methods in China. Its principle is to use refined tin (zero-valent tin) as raw material. The type of refined tin may be small-sized tin flowers or large-sized tin flakes. In a solution mixed with a concentrated sodium hydroxide solution and an oxidant, redox reactions and hydrothermal reactions occur to convert it into sodium stannate. Patent CN101544397 reports a method for producing sodium stannate using tin. The oxidant used is sodium nitrate, but the process must maintain a high temperature reaction (300°C-600°C), produce harmful gas ammonia, high energy consumption, serious environmental pollution, and hidden dangers in operation safety. Taninouchi et al. compared the effects of 13 oxidants on the conversion effect of tin in alkaline solution, among which iodate ions have the best effect, but how to achieve the separation of tin and iodate is one of the issues to be considered in subsequent treatment. At this time, oxidants such as oxygen and hydrogen peroxide without the introduction of impurity ions are more concerned by everyone. Due to the limited oxidizing capacity of oxygen, high pressure and high temperature oxygen pressure treatment is required to obtain satisfactory results. However, the oxygen pressure method still has problems such as unsafe operation, high cost and strict requirements on equipment. Hydrogen peroxide has become the main oxidant used in the production of sodium stannate due to its high oxidizing capacity and environmental protection.

[0004] The existing patent CN201210313074.1 provides a method of using tin flower, hydrogen peroxide and sodium hydroxide as raw materials, reacting at a reaction temperature of 60-100°C for 1-6h, then filtering, concentrating the filtrate under reduced pressure, filtering and drying the filter cake to obtain sodium stannate, and the yield of sodium stannate is as high as 99.5%; the invention has the characteristics of simple preparation process, no generation of harmful gases such as ammonia, no use of high temperature or high pressure, energy saving and environmental protection, and can be used for industrial production. Patent CN201911190579.1 discloses a method for preparing sodium stannate with low free alkali and low aqueous solution turbidity, wherein the preparation step of the sodium stannate solution is to react the metal tin flower with sodium hydroxide solution and hydrogen peroxide at 75-85°C for 3.5-4.5h and then filter to obtain the filtrate sodium stannate solution. However, hydrogen peroxide is relatively stable below 30°C and begins to decompose into water and oxygen above 30°C. The amount of oxygen produced by the decomposition of 30% hydrogen peroxide at different temperatures was tested, and it was found that the oxygen volumes measured at 30°C, 40°C, 50°C, 60°C, 70°C, 80°C and 90°C were 0, 4.9, 10, 20, 49, 89 and 125 (mL), respectively. This shows that hydrogen peroxide is unstable as the temperature increases, and the decomposition rate will accelerate. Tin itself has a high density and is easy to sink to the bottom of the solution in the reaction system. Compared with small-sized tin flowers, large-sized tin flakes are significantly more difficult to dissolve. During high-temperature reactions, a large amount of hydrogen peroxide at a higher position of the liquid surface is converted into water and oxygen and then dissipated into the air, and the oxidizability of the solution is reduced, resulting in poor tin flake dissolution effect, long dissolution time, low hydrogen peroxide utilization rate, and high hydrogen peroxide consumption. However, under low temperature conditions, the kinetic energy of the reactants will decrease, the average speed of the molecules will also slow down, the collision frequency and energy between the reactant molecules will decrease, and the reaction rate will decrease, resulting in poor tin flake dissolution effect. Therefore, how to achieve rapid oxidation under low temperature conditions, improve tin oxidation efficiency, reduce oxidant consumption, and accelerate tin dissolution is the key issue that needs to be solved urgently. Summary of the invention

[0005] In view of the problems of low dissolution efficiency and the like in the existing sodium stannate preparation, the present invention provides a method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets. The present invention strictly controls the oxidation reaction temperature to 20-30°C, utilizes ultrasonic cavitation to promote hydrogen peroxide to generate free radicals (·OH) with stronger oxidation performance, utilizes microjets and shock waves (mechanical action) generated by ultrasound to strengthen the diffusion of hydrogen peroxide and free radicals in the solution, optimizes the addition method of hydrogen peroxide, thereby improving the effective utilization of hydrogen peroxide, strengthening the tin dissolution effect, reducing the amount of hydrogen peroxide, and avoiding the problems of easy decomposition of hydrogen peroxide at high temperature and high energy consumption heating.

[0006] A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, the specific steps are as follows:

[0007] (1) adding a high-purity tin sheet to a sodium hydroxide solution, controlling the temperature of the sodium hydroxide solution to 20 to 30° C. under ultrasonic conditions, slowly adding hydrogen peroxide to 20 to 30% of the preset total addition amount, and then continuing the ultrasonic enhanced oxidation reaction for 7 to 10 minutes;

[0008] (2) under ultrasonic conditions and at a solution system temperature of 20 to 30° C., slowly adding hydrogen peroxide in multiple times and then continuing the ultrasonic enhanced oxidation reaction, wherein the amount of hydrogen peroxide added each time is 10 to 15% of the preset total amount, and the ultrasonic enhanced oxidation reaction is continued for 4 to 8 minutes after each addition of hydrogen peroxide; after the hydrogen peroxide is completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction is continued until the tin sheet is completely dissolved to obtain a sodium stannate solution;

[0009] (3) The sodium stannate solution is filtered, concentrated, separated, washed and dried in sequence to obtain a sodium stannate product.

[0010] The concentration of the sodium hydroxide solution in step (1) is 3-6 mol / L, and the solid-liquid ratio (g:mL) of the high-purity tin flakes to the sodium hydroxide solution is 1:4-8.

[0011] The mass concentration of the hydrogen peroxide is 15-30%, and the preset total addition amount of the hydrogen peroxide is 1.2-2 times the molar amount of the high-purity tin flakes.

[0012] The ultrasonic power is 180-300W, and the frequency is 20-40kHz.

[0013] The addition rate of hydrogen peroxide in step (1) is 2-4 mL / min.

[0014] The addition rate of hydrogen peroxide in step (2) is 1 to 4 mL / min.

[0015] The principle of preparing sodium stannate by ultrasonically strengthening tin oxide sheets at low temperature in the present invention is: under low temperature (20-30°C), while reducing the volatilization of hydrogen peroxide, ultrasonic strengthening is used to promote hydrogen peroxide to produce free radicals with stronger oxidizing performance, thereby improving the oxidation efficiency of hydrogen peroxide and achieving the effect of strengthening the dissolution of tin at low temperature (such as Figure 1 ); The micro jet generated by ultrasound scours and destroys the surface of the tin sheet, making the tin sheet thinner and forming many holes and scouring cracks on its surface (such as Figure 2 and Figure 3 ), increase the specific surface area of ​​the tin flakes, promote the contact of the tin flakes with sodium hydroxide and oxidants, and thus improve the dissolution effect of tin, such as Figure 2 , 3 , as shown in Figure 4.

[0016] The beneficial effects of the present invention are:

[0017] (1) The present invention utilizes ultrasound to promote the generation of more oxidative hydroxyl radicals at a temperature of 20 to 30° C. in hydrogen peroxide, and optimizes the method of adding hydrogen peroxide to effectively enhance the oxidation potential of the solution, strengthen the oxidation of zero-valent tin to tetravalent tin, and improve the utilization rate of hydrogen peroxide;

[0018] (2) The present invention realizes efficient oxidation reaction at low temperature (temperature of 20-30° C.), and the dissolution rate of tin can reach more than 99%, realizing low energy consumption and high efficiency conversion of tin;

[0019] (3) The present invention greatly improves the utilization rate of hydrogen peroxide, reduces the amount of hydrogen peroxide used, and significantly shortens the reaction time. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is the dissolution rate of tin under ultrasonic enhancement and conventional (without ultrasound) at different temperatures;

[0021] Figure 2 The microscopic morphology scanning electron microscope (SEM) images of the tin flake raw material, the remaining tin flake after conventional (no ultrasound at 20°C) treatment for 60 minutes, and the remaining tin flake after ultrasound enhanced treatment at 20°C for 10 minutes;

[0022] Figure 3 This is a scanning electron microscope (SEM) image of the surface microstructure of the remaining tin sheet after conventional treatment (without ultrasound at 20°C) for 60 minutes;

[0023] Figure 4 This is a scanning electron microscope (SEM) image of the surface microstructure of the remaining tin sheet after ultrasonic strengthening treatment at 20°C for 10 minutes. DETAILED DESCRIPTION

[0024] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.

[0025] Example 1: A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, the specific steps are as follows:

[0026] (1) adding a high-purity tin flake to a sodium hydroxide solution with a concentration of 4 mol / L, controlling the temperature of the sodium hydroxide solution to 20°C under ultrasonic conditions (ultrasonic power of 240 W, frequency of 24 kHz), slowly adding hydrogen peroxide at a rate of 3 mL / min to 25% of the preset total addition amount, and then continuing the ultrasonic enhanced oxidation reaction for 10 minutes; the mass concentration of the hydrogen peroxide is 30%, and the preset total addition amount of the hydrogen peroxide is 1.5 times the molar amount of the high-purity tin flake; the solid-liquid ratio of the high-purity tin flake to the sodium hydroxide solution is g:mL 1:6;

[0027] (2) Under ultrasonic conditions (ultrasonic power of 240 W, frequency of 24 kHz) and a solution system temperature of 20° C., hydrogen peroxide was slowly added in batches (each at a rate of 2 mL / min) and then the ultrasonic enhanced oxidation reaction was continued for 7 minutes, wherein the amount of hydrogen peroxide added each time was 15% of the preset total amount, and the ultrasonic enhanced oxidation reaction was continued for 7 minutes after each addition of hydrogen peroxide; after the hydrogen peroxide was completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction was continued until the tin sheet was completely dissolved to obtain a sodium stannate solution; the total time of the hydrogen peroxide oxidation reaction in this embodiment was 60 minutes;

[0028] (3) the sodium stannate solution is filtered to remove impurities, concentrated under reduced pressure to crystallize, centrifuged, washed, and dried to obtain a sodium stannate product;

[0029] In this embodiment, the total oxidation reaction time of hydrogen peroxide at a temperature of 20° C. is 60 minutes, and the dissolution rate of the tin sheet reaches 100%.

[0030] Comparative Example 1: The difference between this comparative example and Example 1 is that: no ultrasonic wave is introduced, the entire reaction time is 100 min; the dissolution rate of the tin flake is only 72.3%, while the dissolution rate of tin in Example 1 is increased by 27.7% compared with this comparative example; Figure 2-4 As shown in the figure, ultrasonic cavitation is used to promote hydrogen peroxide to produce free radicals (·OH) with stronger oxidizing properties, and ultrasonic mechanical action is used to produce a strong impact on the tin sheet, which breaks and perforates the tin sheet, increases the reaction contact surface, and promotes the reaction. Under the same reaction conditions, the tin sheet becomes significantly thinner after ultrasonic treatment and many cracks and holes appear on the surface, while the tin sheet is still thicker and has a denser surface after conventional treatment.

[0031] Comparative Example 2: The only difference between this comparative example and Example 1 is that the hydrogen peroxide is added to the solution all at once, and the tin oxide sheet is ultrasonically strengthened for 80 minutes;

[0032] In this comparative example, the dissolution rate of the tin flakes is 79.3%. In Example 1, the dissolution rate of the tin can be increased by 20.7% by optimizing the addition method of hydrogen peroxide.

[0033] Comparative Example 3: A method for preparing sodium stannate from tin oxide sheets at low temperature, the specific steps are as follows:

[0034] The high-purity tin flakes were added to a sodium hydroxide solution with a concentration of 4 mol / L. Under ultrasonic conditions (ultrasonic power of 240 W, frequency of 24 kHz), the temperature of the sodium hydroxide solution was controlled to be 20°C, hydrogen peroxide was slowly added at a rate of 3 mL / min, and the ultrasonic enhanced oxidation reaction was continued for 80 minutes. The mass concentration of the hydrogen peroxide was 30%, and the preset total addition amount of the hydrogen peroxide was 1.5 times the molar amount of the high-purity tin flakes. The solid-liquid ratio of the high-purity tin flakes to the sodium hydroxide solution was 1:6 in g:mL.

[0035] The dissolution rate of the tin flakes in this comparative example is 82.9%. The dissolution rate of the tin in Example 1 can be increased by 17.1% by optimizing the addition method of hydrogen peroxide.

[0036] Comparative Example 4: The difference between this comparative example and Example 1 is that: no ultrasonic wave is introduced, and hydrogen peroxide is slowly added at a rate of 2 mL / min at a temperature of 60° C. until the tin sheet is completely dissolved;

[0037] The total time of the hydrogen peroxide oxidation reaction in this comparative example reaches 130 minutes, and the total consumption of hydrogen peroxide is 2.21 times that of the total consumption of hydrogen peroxide in Example 1; therefore, Example 1 can significantly shorten the time and reduce the amount of hydrogen peroxide at low temperature (20° C.).

[0038] Example 2: A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, the specific steps are as follows:

[0039] (1) adding a high-purity tin flake to a sodium hydroxide solution with a concentration of 3 mol / L, controlling the temperature of the sodium hydroxide solution to 25°C under ultrasonic conditions (ultrasonic power of 200 W, frequency of 20 kHz), slowly adding hydrogen peroxide at a rate of 3 mL / min to 20% of the preset total addition amount, and then continuing the ultrasonic enhanced oxidation reaction for 10 minutes; the mass concentration of the hydrogen peroxide is 15%, and the preset total addition amount of the hydrogen peroxide is twice the molar amount of the high-purity tin flake; the solid-liquid ratio of the high-purity tin flake to the sodium hydroxide solution is g:mL 1:8;

[0040] (2) under ultrasonic conditions (ultrasonic power of 200 W, frequency of 20 kHz) and a solution system temperature of 25° C., hydrogen peroxide was slowly added in batches (each at a rate of 1 mL / min) and then the ultrasonic enhanced oxidation reaction was continued for 5 min, wherein the amount of hydrogen peroxide added each time was 10% of the preset total amount, and the ultrasonic enhanced oxidation reaction was continued for 5 min after each addition of hydrogen peroxide; after the hydrogen peroxide was completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction was continued until the tin sheet was completely dissolved to obtain a sodium stannate solution; in this embodiment, the total time of the hydrogen peroxide oxidation reaction was 80 min, and the total reaction time was 95 min;

[0041] (3) The sodium stannate solution is filtered to remove impurities, concentrated under reduced pressure to crystallize, centrifuged, washed, and dried to obtain a sodium stannate product; in this embodiment, the total time of the hydrogen peroxide oxidation reaction at a temperature of 25° C. is 80 minutes, and the dissolution rate of the tin flakes reaches 100%.

[0042] Example 3: A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, the specific steps are as follows:

[0043] (1) adding a high-purity tin flake to a sodium hydroxide solution with a concentration of 4 mol / L, controlling the temperature of the sodium hydroxide solution to 25°C under ultrasonic conditions (ultrasonic power of 400 W, frequency of 24 kHz), slowly adding hydrogen peroxide at a rate of 3 mL / min to 26% of the preset total addition amount, and then continuing the ultrasonic enhanced oxidation reaction for 20 minutes; the mass concentration of the hydrogen peroxide is 30%, and the preset total addition amount of the hydrogen peroxide is 1.8 times the molar amount of the high-purity tin flake; the solid-liquid ratio of the high-purity tin flake to the sodium hydroxide solution is g:mL 1:5;

[0044] (2) Under ultrasonic conditions (ultrasonic power of 400 W, frequency of 24 kHz) and a solution system temperature of 25° C., hydrogen peroxide was slowly added in batches (each at a rate of 2 mL / min) and then the ultrasonic enhanced oxidation reaction was continued, wherein the amount of hydrogen peroxide added each time was 12% of the preset total amount, and the ultrasonic enhanced oxidation reaction was continued for 5 minutes after each addition of hydrogen peroxide; after the hydrogen peroxide was completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction was continued until the tin sheet was completely dissolved to obtain a sodium stannate solution; the total time of the hydrogen peroxide oxidation reaction in this embodiment was 58 minutes, and the total reaction time was 83 minutes;

[0045] (3) the sodium stannate solution is filtered to remove impurities, concentrated under reduced pressure to crystallize, centrifuged, washed, and dried to obtain a sodium stannate product;

[0046] The dissolution rate of the tin sheet in this embodiment is 100%.

[0047] Example 4: A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, the specific steps are as follows:

[0048] (1) adding a high-purity tin flake to a sodium hydroxide solution with a concentration of 4 mol / L, controlling the temperature of the sodium hydroxide solution to 30°C under ultrasonic conditions (ultrasonic power of 300 W, frequency of 24 kHz), slowly adding hydrogen peroxide to 30% of the preset total addition amount at a rate of 3 mL / min, and continuing the ultrasonic enhanced oxidation reaction for 8 min; the mass concentration of the hydrogen peroxide is 30%, and the preset total addition amount of the hydrogen peroxide is 1.5 times the molar amount of the high-purity tin flake; the solid-liquid ratio of the high-purity tin flake to the sodium hydroxide solution is g:mL 1:5;

[0049] (2) Under ultrasonic conditions (ultrasonic power of 300 W, frequency of 24 kHz) and a solution system temperature of 30° C., hydrogen peroxide was slowly added in batches (each at a rate of 2 mL / min) and then the ultrasonic enhanced oxidation reaction was continued, wherein the amount of hydrogen peroxide added each time was 10% of the preset total amount, and the ultrasonic enhanced oxidation reaction was continued for 8 minutes after each addition of hydrogen peroxide; after the hydrogen peroxide was completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction was continued until the tin sheet was completely dissolved to obtain a sodium stannate solution; the total time of the hydrogen peroxide oxidation reaction in this embodiment was 55 minutes, and the total reaction time was 71 minutes;

[0050] (3) the sodium stannate solution is filtered to remove impurities, concentrated under reduced pressure to crystallize, centrifuged, washed, and dried to obtain a sodium stannate product;

[0051] The dissolution rate of the tin sheet in this embodiment is 100%.

[0052] The specific implementation modes of the present invention are described in detail above, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets, characterized in that: The specific steps are as follows: (1) adding a high-purity tin sheet to a sodium hydroxide solution, controlling the temperature of the sodium hydroxide solution to 20 to 30° C. under ultrasonic conditions, slowly adding hydrogen peroxide to 20 to 30% of the preset total addition amount, and then continuing the ultrasonic enhanced oxidation reaction for 7 to 10 minutes; (2) under ultrasonic conditions and at a solution system temperature of 20 to 30° C., slowly adding hydrogen peroxide in multiple times and then continuing the ultrasonic enhanced oxidation reaction, wherein the amount of hydrogen peroxide added each time is 10 to 15% of the preset total amount, and the ultrasonic enhanced oxidation reaction is continued for 4 to 8 minutes after each addition of hydrogen peroxide; after the hydrogen peroxide is completely added according to the preset total amount, the ultrasonic enhanced oxidation reaction is continued until the tin sheet is completely dissolved to obtain a sodium stannate solution; (3) The sodium stannate solution is filtered, concentrated, separated, washed and dried in sequence to obtain a sodium stannate product.

2. The method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets according to claim 1, characterized in that: The concentration of the sodium hydroxide solution in step (1) is 3-6 mol / L, and the solid-liquid ratio (g:mL) of the high-purity tin sheet to the sodium hydroxide solution is 1:4-8.

3. The method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets according to claim 1, characterized in that: The mass concentration of hydrogen peroxide is 15-30%, and the preset total addition amount of hydrogen peroxide is 1.2-2 times of the molar amount of the high-purity tin flakes.

4. The method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets according to claim 1, characterized in that: The ultrasonic power is 180~300W and the frequency is 20~40kHz.

5. The method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets according to claim 1, characterized in that: The addition rate of hydrogen peroxide in step (1) is 2-4 mL / min.

6. The method for preparing sodium stannate at low temperature by ultrasonically strengthening tin oxide sheets according to claim 1, characterized in that: The addition rate of hydrogen peroxide in step (2) is 1 to 4 mL / min.

Citation Information

Patent Citations

  • Method for preparing sodium stannate

    CN102863015A

  • Method for preparing low-free-alkali low-water-solution turbidity sodium stannate

    CN110817940A

  • Ultrasound Assisted Heavy Metal Recovery

    US20090250408A1