High-aluminum pyrolusite synthesized sodium ion battery positive electrode active material and preparation method thereof

The synthesis of a sodium ion battery active material from high-aluminum pyrolusite with specific molar ratios and additives enhances structural stability and electrochemical performance, addressing the limitations of existing cathode materials in sodium-ion batteries.

CN119080068APending Publication Date: 2024-12-06JIANGXI ANCHI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411086467.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The performance of cathode materials in sodium-ion batteries, including transition metal oxide systems and Prussian blue systems, requires improvement for enhanced electrochemical capacity and cycle stability.

Method used

A method involving the synthesis of a sodium ion battery positive electrode active material using high-aluminum pyrolusite, mixed with an iron and sodium source, followed by grinding, spray drying, and a solid phase reaction, with specific molar ratios and additives like sodium hydroxide and chromium trioxide, to enhance structural stability and electrochemical performance.

Benefits of technology

The method improves the structural stability and electrochemical performance of sodium ion batteries by promoting active Na occupation in the triangular prism structure and stabilizing the crystal phase, resulting in improved cycle performance and capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004985315540000051
    Figure BDA0004985315540000051
Patent Text Reader

Abstract

The invention discloses a sodium ion battery positive electrode active material synthesized from high-aluminum pyrolusite and a preparation method thereof, and relates to the field of sodium ion batteries, first pyrolusite, an iron source and a sodium source are mixed and ground to 40-60 nm to obtain a mixture, then the mixture is subjected to spray drying, and finally a solid-phase reaction is performed to prepare the sodium ion battery positive electrode active material. The sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of (1-2): (8-9); wherein the aluminum content of the pyrolusite is 2 to 5 weight percent. Aluminum-containing pyrolusite is used as a manganese source and reacts with an iron source and a sodium source to obtain the sodium-ion battery positive electrode active material, sodium hydroxide is added into the sodium source, the sodium hydroxide reacts with aluminum oxide in the pyrolusite in the grinding process to generate aluminum hydroxide, the aluminum hydroxide is mixed into the mixture, more Na elements can be promoted to be converted into active Na through doped Al, and the sodium-ion battery positive electrode active material is obtained. In other words, active Na occupies gaps of the triangular prism structure formed by O, the structural stability of the active material is improved, and therefore the performance of the sodium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of sodium ion batteries, and in particular to a sodium ion battery positive electrode active material synthesized from high-aluminum pyrolusite and a preparation method thereof. Background Art

[0002] Sodium-ion batteries have wide applications and market prospects in electric vehicles and other energy storage fields due to their low cost. Their working principle is to utilize the reversible insertion and extraction of sodium ions between the positive and negative electrodes to achieve energy storage and release.

[0003] At present, the cathode materials used in sodium-ion batteries mainly include transition metal oxide systems, polyanion compounds and Prussian blue systems. However, the performance of these cathode active materials still has room for improvement. Summary of the invention

[0004] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a high-aluminum pyrolusite-synthesized sodium ion battery positive electrode active material and a preparation method thereof.

[0005] The technical solution of the present invention is as follows:

[0006] A method for preparing a positive electrode active material for a sodium ion battery synthesized from high-aluminum pyrolusite, comprising first mixing pyrolusite with an iron source and a sodium source, grinding the mixture to 40-60 nm to obtain a mixture, then spray drying the mixture, and finally performing a solid phase reaction to obtain the material; the sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of 1-2:8-9;

[0007] Wherein, the aluminum content of the pyrolusite is 2-5wt%.

[0008] As a preferred embodiment of the present invention, the pyrolusite, iron source and sodium source are added according to the molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:1 to obtain the O3 structure: 0.88MnO2+0.02Al(OH)3+0.1FeCO3+NaCO3=NaMn 0.88 Al 0.02 Fe 0.1 O2.

[0009] As a preferred embodiment of the present invention, the pyrolusite, iron source and sodium source are added according to the molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:0.7 to obtain the P2 structure: 0.88MnO2+0.02Al(OH)3+0.1FeCO3+0.7NaCO3=Na 0.7 Mn 0.88 Al 0.02 Fe 0.1 O2.

[0010] As a preferred embodiment of the present invention, the pyrolusite, iron source and sodium source are added according to the molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:0.9 to obtain a mixture of O3 structure and P2 structure:

[0011] 0.88MnO2+0.02Al(OH)3+0.1FeCO3+0.9NaCO3=Na 0.9 Mn 0.88 Al 0.02 Fe 0.1 O2.

[0012] As a preferred embodiment of the present invention, chromium trioxide is also added to the solid phase reaction to obtain 0.88MnO2+0.02Al(OH)3+0.1FeCO3+0.01Cr2O3+NaCO3=NaMn 0.88 Al 0.02 Fe 0.1 Cr 0.02 O2.

[0013] As a preferred embodiment of the present invention, the content of aluminum hydroxide in the mixture is 0.8-1.2 wt %.

[0014] As a preferred embodiment of the present invention, the solid phase reaction is specifically as follows: heating to 800-1000°C at a rate of 3-6°C / min, calcining for 6-10h, and cooling to obtain the product.

[0015] As a preferred embodiment of the present invention, the cooling rate is 4-6°C / min.

[0016] The invention also discloses a sodium ion battery positive electrode active material synthesized from high-aluminum pyrolusite, which is prepared by any of the above preparation methods.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention uses aluminum-containing pyrolusite as a manganese source, reacts it with an iron source and a sodium source to obtain a positive electrode active material for a sodium ion battery, and adds sodium hydroxide to the sodium source so that it reacts with aluminum oxide in the pyrolusite during grinding to generate aluminum hydroxide, which is then mixed into the mixture. The doped aluminum hydroxide can promote more Na elements to be converted into active Na, that is, active Na is more likely to occupy the gaps in the triangular prism structure formed by O, thereby improving the structural stability of the active material and thus improving the performance of the sodium ion battery.

[0019] In addition, by adjusting the amount of manganese ions, iron ions and sodium ions, active materials with different crystal phase structures were obtained, among which P2 has excellent electrochemical capacity; while O3 is easy to transform into O2, the electrochemical capacity is easy to deteriorate, but the cycle performance is excellent. Therefore, by adjusting the amount of raw materials added, the P2 and O3 structures can be mixed, thereby improving the electrochemical performance.

[0020] (2) The present invention further adds chromium trioxide inorganic oxide, which has a more stable structure after synthesis and can effectively improve the cycle performance. DETAILED DESCRIPTION

[0021] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used that do not specify the manufacturer are all conventional products that can be obtained commercially.

[0022] Example 1

[0023] A method for preparing a positive electrode active material for a sodium ion battery comprises the following steps: firstly mixing pyrolusite with an iron source and a sodium source, grinding the mixture to 50 nm to obtain a mixture, then spray drying the mixture, and finally performing a solid phase reaction to obtain the positive electrode active material; the sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of 1:9; and the iron source is iron carbonate.

[0024] The aluminum content of the pyrolusite is 3wt%, and the aluminum hydroxide content in the mixture is 1wt%;

[0025] Pyrolusite, iron source and sodium carbonate were added in a molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:1 to carry out solid phase reaction to obtain NaMn 0.88 Al 0.02 Fe 0.1 O2;

[0026] The solid phase reaction is specifically as follows: heating to 950° C. at a rate of 4° C. / min for calcination for 8 hours, and cooling at a rate of 5° C. / min to obtain the product.

[0027] Example 2

[0028] A method for preparing a positive electrode active material for a sodium ion battery comprises the following steps: firstly mixing pyrolusite with an iron source and a sodium source, grinding the mixture to 50 nm to obtain a mixture, then spray drying the mixture, and finally performing a solid phase reaction to obtain the positive electrode active material; the sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of 1:9; and the iron source is iron carbonate.

[0029] The aluminum content of the pyrolusite is 3wt%, and the aluminum hydroxide content in the mixture is 1wt%;

[0030] Pyrolusite, iron source and sodium carbonate were added in a molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:0.7 to carry out solid phase reaction to prepare Na 0.7 Mn 0.88 Al 0.02 Fe 0.1 O2;

[0031] The solid phase reaction is specifically as follows: heating to 950° C. at a rate of 4° C. / min for calcination for 8 hours, and cooling at a rate of 5° C. / min to obtain the product.

[0032] Example 3

[0033] A method for preparing a positive electrode active material for a sodium ion battery comprises the following steps: firstly mixing pyrolusite with an iron source and a sodium source, grinding the mixture to 50 nm to obtain a mixture, then spray drying the mixture, and finally performing a solid phase reaction to obtain the positive electrode active material; the sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of 1:9; and the iron source is iron carbonate.

[0034] The aluminum content of the pyrolusite is 3wt%, and the aluminum hydroxide content in the mixture is 1wt%;

[0035] Pyrolusite, iron source and sodium carbonate were added in a molar ratio of manganese ion: aluminum ion: iron ion: sodium ion of 0.88:0.02:0.1:0.9, and a solid phase reaction was performed to obtain Na 0.9 Mn 0.88 Al 0.02 Fe 0.1 O2;

[0036] The solid phase reaction is specifically as follows: heating to 950° C. at a rate of 4° C. / min for calcination for 8 hours, and cooling at a rate of 5° C. / min to obtain the product.

[0037] Example 4

[0038] This embodiment is an improvement on the basis of embodiment 3. Specifically, chromium trioxide is further added in the solid phase reaction. Pyrolusite, iron source, sodium source and chromium trioxide are added in a molar ratio of manganese ion: aluminum ion, iron ion: sodium ion: chromium ion of 0.88:0.02:0.1:1:0.02 to carry out solid phase reaction to obtain Na Mn 0.88 Al 0.02 Fe 0.1 Cr 0.02 O2.

[0039] Comparative Example 1 (without sodium hydroxide)

[0040] A method for preparing a positive electrode active material for a sodium ion battery comprises mixing sodium carbonate, an iron source and pyrolusite, grinding the mixture to a size of 50 nm, and conducting a solid phase reaction to obtain the positive electrode active material, wherein the iron source is iron carbonate;

[0041] Pyrolusite, iron source and sodium carbonate were added in a molar ratio of manganese ion: iron ion: sodium ion of 0.9:0.1:1, and a solid phase reaction was carried out to obtain NaMn 0.9 Fe 0.1 O2; wherein the aluminum content of the pyrolusite is 3wt%.

[0042] The solid phase reaction is specifically as follows: heating to 950° C. at a rate of 4° C. / min for calcination for 8 hours, and cooling at a rate of 5° C. / min to obtain the product.

[0043] Comparative Example 2 (pyrolusite with low aluminum content)

[0044] A method for preparing a positive electrode active material for a sodium ion battery comprises mixing sodium carbonate, an iron source and pyrolusite, grinding the mixture to a size of 50 nm, and conducting a solid phase reaction to obtain the positive electrode active material, wherein the iron source is iron carbonate;

[0045] Pyrolusite, iron source and sodium carbonate were added in a molar ratio of manganese ion: iron ion: sodium ion of 0.9:0.1:1, and a solid phase reaction was carried out to obtain NaMn 0.9 Fe 0.1 O2; wherein the aluminum content of the pyrolusite is 0.003wt%.

[0046] The solid phase reaction is specifically as follows: heating to 950° C. at a rate of 4° C. / min for calcination for 8 hours, and cooling at a rate of 5° C. / min to obtain the product.

[0047] The sodium ion battery (finished battery) prepared by the positive electrode active material of the above embodiment was subjected to gram capacity and 1000 cycle tests. The test results are shown in Table 1.

[0048] Table 1 Performance test results of embodiments and comparative examples

[0049]

[0050] As can be seen from the above table, the performance of the embodiment is better than that of the comparative example. The analysis of comparative examples 1 and 2 shows that the performance of the high aluminum-containing pyrolusite and the pyrolusite with very little aluminum is not treated with sodium hydroxide, which is worse than that of the embodiment. The reason may be that the embodiment uses aluminum-containing pyrolusite as a manganese source, reacts it with an iron source and a sodium source to obtain a positive active material for a sodium ion battery, and by adding sodium hydroxide to the sodium source, it reacts with aluminum trioxide in the pyrolusite during the grinding process to form aluminum hydroxide, which is mixed into the mixture. The doped aluminum hydroxide can promote more Na elements to be converted into active Na, that is, active Na is more likely to occupy the gaps in the triangular prism structure composed of O, thereby improving the structural stability of the active material, thereby improving the performance of the sodium ion battery. In addition, Example 2 obtains a P2 structure with excellent gram capacity, and Example 1 obtains an O3 crystal with ultra-high discharge electrochemical capacity. O3 is easy to transform to O2, resulting in capacity loss in electrochemistry, which causes electrochemical deterioration, but the cycle performance is better. Therefore, by adjusting the amount of raw materials added, a P2 and O3 structure mixture (Example 3) can be obtained, and a mixed structure with excellent comprehensive performance is obtained. In addition, the performance of Example 4 is further optimized because chromium trioxide is also added in the embodiment, and the synthesis has a more stable structure, which can effectively improve the cycle performance. The production process of the present invention is simple, practical, and can be used for production.

[0051] The above-mentioned embodiments only express the preferred implementation modes of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the present invention. It should be pointed out that, for ordinary technicians in this field, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all these changes and deformations should fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a positive electrode active material for a sodium ion battery by synthesizing high-aluminum pyrolusite, characterized in that: First, pyrolusite, an iron source and a sodium source are mixed, ground to 40-60 nm to obtain a mixture, then the mixture is spray-dried, and finally a solid phase reaction is performed to obtain the product; the sodium source comprises sodium hydroxide and sodium carbonate in a molar ratio of 1-2:8-9; Wherein, the aluminum content of the pyrolusite is 2-5wt%.

2. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The pyrolusite, iron source and sodium source are added in a molar ratio of manganese ion:aluminum ion:iron ion:sodium ion of 0.88:0.02:0.1:

1.

3. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The pyrolusite, iron source and sodium source are added in a molar ratio of manganese ion:aluminum ion:iron ion:sodium ion of 0.88:0.02:0.1:0.

7.

4. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The pyrolusite, iron source and sodium source are added in a molar ratio of manganese ion:aluminum ion:iron ion:sodium ion of 0.88:0.02:0.1:0.

9.

5. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The iron source includes iron carbonate and / or ferrous carbonate.

6. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: During the solid phase reaction, chromium trioxide is also added.

7. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The content of aluminum hydroxide in the mixture is 0.8-1.2 wt %.

8. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 1, characterized in that: The solid phase reaction is specifically as follows: heating to 800-1000° C. at a rate of 3-6° C. / min, calcining for 6-10 hours, and cooling to obtain the product.

9. The method for preparing a positive electrode active material for a sodium ion battery from high-aluminum pyrolusite according to claim 8, characterized in that: The cooling rate is 4-6°C / min.

10. A sodium ion battery positive electrode active material synthesized from high-aluminum pyrolusite, characterized in that: The method is prepared by any one of claims 1 to 9.