Grouting material for gypsum / mirabilite karst foundation as well as preparation method and application of grouting material

By melting blast furnace slag powder and steel slag powder in the grouting material at high temperature and forming ettringite, the dissolution problem of gypsum/Glauber's salt karkarst foundation is solved, the foundation stability and dissolution resistance are improved, the construction cost is reduced, and the processing process is simplified .

CN119080409AActive Publication Date: 2024-12-06SOUTHWESTERN ARCHITECTURAL DESIGN INST
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411264985.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

The gene dissolution of gypsum/Glauber's salt karst causes unstable foundations. The traditional treatment methods are expensive and complex in construction, and lack effective dissolution blocking materials.

Method used

Provide a grouting material, including 70 to 92 parts of blast furnace slag powder, 8 to 30 parts of steel slag powder and 250 to 350 parts of water, through high temperature melting and rapid cooling, forming a dense structure, combining alkaline exciter, expansion hardener and stable The agent is used to form ettringite to adhere gypsum/Glauber’s salt interlayer to block dissolution.

Benefits of technology

It improves the stability and dissolution resistance of gypsum/Glaubert salkarst foundation, reduces construction costs, simplifies the treatment process, and achieves long-term stability and bearing capacity improvement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080409A_ABST
    Figure CN119080409A_ABST
Patent Text Reader

Abstract

The invention provides a grouting material for a gypsum / mirabilite karst foundation as well as a preparation method and application of the grouting material. The grouting material for the gypsum / mirabilite karst foundation comprises the following components in parts by mass: 70-92 parts of blast furnace slag powder, 8-30 parts of steel slag powder and 250-350 parts of water. The blast furnace slag powder and the steel slag powder of the grouting material provided by the invention are subjected to high-temperature melting and rapid cooling in the forming process, so that the structures of the grouting material are relatively compact and stable, and hydration reaction with water is avoided due to the structural stability; when the grouting material reaches an environment with gypsum / mirabilite, calcium oxide and aluminum oxide in the blast furnace slag powder and the steel slag powder can generate ettringite with sulfate ions in the gypsum / mirabilite, and the ettringite is attached to a gypsum / mirabilite interlayer, so that the effect of blocking corrosion is achieved, and the stability of a gypsum / mirabilite karst foundation is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of grouting materials, and in particular to a grouting material for a gypsum / glauber's salt karst foundation, and a preparation method and application thereof. Background Art

[0002] Gypsum and mirabilite, as the main representatives of sulfate rocks, are widely distributed in many regions around the world, especially in southwest China, where a large number of thin layers of mirabilite / gypsum mines have been found in strata such as Sichuan Province. Due to their soluble properties, these rocks are prone to dissolution under the action of groundwater and other erosive flowing water, forming complex karst landforms, including caves, karst grooves, and karst funnels. These karst phenomena not only affect the quality of groundwater, but also seriously threaten the safety of engineering construction. Problems such as unstable foundations, collapse, water inrush, and leakage frequently occur, bringing huge challenges to engineering construction.

[0003] With the continuous development of modern engineering technology, especially in the construction of large-scale infrastructure such as high-rise buildings, bridges, tunnels and other projects, the requirements for foundation stability and bearing capacity are increasing. However, the dissolution of gypsum / glauber's salt karst foundation has become a major obstacle to the smooth implementation of these projects. Traditional foundation treatment methods, such as grouting reinforcement and pile foundation reinforcement, can improve the bearing capacity of the foundation to a certain extent, but they have limited effect on blocking the dissolution of gypsum / glauber's salt, and are often costly and complex to construct.

[0004] Therefore, it is particularly important to urgently need a gypsum / glauber's salt karst foundation dissolution blocking material. Summary of the invention

[0005] The purpose of the present invention is to solve the technical problem of unstable foundation caused by the dissolution phenomenon of existing gypsum / glauber's salt karst base.

[0006] To solve the above technical problems, the present invention first provides a grouting material for gypsum / glauber's salt karst foundation, which at least includes the following components in parts by mass: 70-92 parts of blast furnace slag powder, 8-30 parts of steel slag powder, and 250-350 parts of water.

[0007] Preferably, the granulation grade of blast furnace slag powder is ≥ S75, and the density of blast furnace slag powder is ≥ 2.8 g / cm 3 , specific surface area ≥300m 2 / kg.

[0008] Preferably, the granulation grade of the steel slag powder is ≥ grade II, and the fineness of the steel slag powder is not less than 1200 mesh.

[0009] Preferably, the grouting material also includes 5 to 10 parts of an alkaline activator.

[0010] Preferably, the alkaline activator is at least one of water glass, sodium hydroxide and quicklime.

[0011] Preferably, the grouting material also includes 3 to 5 parts of an expansion hardener and 1 to 2 parts of a stabilizer.

[0012] Preferably, the expansion hardener is magnesium oxide, and the stabilizer is cellulose ether compound or polyvinyl alcohol.

[0013] Accordingly, the present invention also provides a method for preparing a grouting material for a gypsum / glauber's salt karst foundation as described above, the method comprising: S10, mixing blast furnace slag powder and steel slag powder and grinding them to obtain a powder material; S20, mixing the powder material with water and stirring to obtain a grouting material.

[0014] Accordingly, in step S20, the stirring temperature of the stirring treatment is 20° C. to 30° C., and the stirring time of the stirring treatment is 2 to 4 min.

[0015] Correspondingly, the present invention further provides a grouting material for gypsum / glauber's salt karst foundation as described above and / or a preparation method of a grouting material for gypsum / glauber's salt karst foundation as described above, and its application in gypsum / glauber's salt karst foundation reinforcement engineering.

[0016] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides a grouting material for gypsum / glauber's salt karst foundation and its preparation method and application, wherein the grouting material for gypsum / glauber's salt karst foundation comprises at least the following components by mass: 70-92 parts of blast furnace slag powder, 8-30 parts of steel slag powder, and 250-350 parts of water. The blast furnace slag powder and steel slag powder of the grouting material provided by the present invention undergo high-temperature melting and rapid cooling during the formation process, making their structures relatively dense and stable, and this structural stability avoids hydration reaction with water; when the grouting material reaches an environment with gypsum / glauber's salt, the calcium oxide and aluminum oxide in the blast furnace slag powder and the steel slag powder can react with the sulfate ions in the gypsum / glauber's salt to generate calcium sulfonate and adhere to the gypsum / glauber's salt interlayer, thereby achieving the effect of blocking dissolution, thereby improving the stability of the gypsum / glauber's salt karst foundation. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 A flow chart of a method for preparing a grouting material for a gypsum / glauber's salt karst foundation provided by an embodiment of the present invention; Figure 2 Schematic diagram of gypsum / glauber's salt sandwich core sample provided for multiple embodiments of the present invention; Figure 3aA schematic diagram of a core sample after the grouting material provided in some embodiments of the present invention is injected into a dynamic water test chamber in which a gypsum / glauber's salt sandwich core sample is placed and then taken out after 72 hours; Figure 3b Schematic diagram of the core sample taken out after 72 hours after the grouting material provided in Comparative Example 2 of the present invention is injected into a dynamic water test chamber in which a gypsum / glauber's salt sandwich core sample is placed; Figure 4a A schematic diagram of an apparatus used for performing a dynamic water flushing test on the test pieces provided in Examples 1 to 6 of the present invention and Comparative Examples 1 to 2; Figure 4b A schematic diagram of a core sample of a test piece provided in Example 3 of the present invention after a 14-day dynamic water scouring test; Figure 4c A schematic diagram of a core sample of a specimen provided in Comparative Example 1 of the present invention after a 14-day dynamic water scouring test; Figure 4d A schematic diagram of a core sample of a specimen provided in comparative example 2 of the present invention after a 14-day dynamic water scouring test; Figure 4e A schematic diagram of a core sample of a test piece provided in Example 3 of the present invention after a 22-day dynamic water scouring test; Figure 4f Schematic diagram of the core sample of the specimen provided in Control Example 2 of the present invention after 22 days of dynamic water scouring test. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] In view of the technical problem that the existing gypsum / glauber's salt karst foundation has an unstable foundation due to the dissolution phenomenon, the present invention provides a grouting material for gypsum / glauber's salt karst foundation and a preparation method and application thereof. The material has the advantages of good flow permeability, no hydration ability in the absence of gypsum / glauber's salt, targeted blocking of the dissolution of gypsum / glauber's salt and low price.

[0020] In order to achieve the above technical objectives, this application adopts the following technical solutions: In a first aspect, the present invention first provides a grouting material for gypsum / glauber's salt karst foundation, comprising at least the following components in parts by weight: 70 to 92 parts of blast furnace slag powder, 8 to 30 parts of steel slag powder, and 250 to 350 parts of water.

[0021] In the embodiment of the present invention, blast furnace slag powder is a potential hydraulic cementitious material. Experimental studies have shown that its activity changes with the change of its grinding fineness (specific surface area). When the specific surface area of ​​the grinding reaches 300m 2 / kg or above, the effect is better, which can significantly improve the early strength and the later strength can exceed that of silicate cement.

[0022] Specifically, the blast furnace slag powder adopts S75 pure slag powder that meets the standard of GB / T18046-2008 "Slag powder for cement and concrete" for slag powder in cement and concrete. The density of blast furnace slag powder is ≥2.8g / cm 3 , specific surface area ≥300m 2 / kg.

[0023] Preferably, the blast furnace slag powder includes the following components in parts by mass: 30-40 parts of SiO2, 10-20 parts of Al2O3, 30-45 parts of CaO, 5-15 parts of MgO, and 1-5 parts of Fe2O3.

[0024] Steel slag powder is hot smoldering slag. The open-hearth steelmaking process melts the charge into two mutually insoluble liquid phases at high temperature, separates the steel and other impurities, and forms steel slag powder. The activity of free calcium oxide in steel slag powder increases with the decrease of the grinding fineness of steel slag powder. Steel slag powder has a certain micro-expansion, which improves the shrinkage of cementitious materials. Specifically, the granulation grade of the steel slag powder is ≥ grade II, and the fineness of the steel slag powder is not less than 1200 meshes.

[0025] Preferably, the steel slag powder comprises the following components in parts by mass: 10-30 parts of SiO2, 2-10 parts of Al2O3, 30-50 parts of CaO, 5-15 parts of MgO, and 10-30 parts of Fe2O3.

[0026] In the embodiment of the present invention, since the fineness of the steel slag powder is relatively low and the glass structure of the blast furnace slag powder is more stable than that of the steel slag powder, this structural stability makes it easier for the steel slag powder to react with the sulfate ions in the gypsum / glauber's salt karst foundation to generate calcium sulfonate; therefore, by adding a certain proportion of steel slag powder to the grouting material, it is beneficial to accelerate the formation of calcium sulfonate on the gypsum / glauber's salt interlayer, thereby achieving the effect of targeted blocking of the dissolution of gypsum / glauber's salt and improving its anti-corrosion performance.

[0027] Specifically, when the steel slag powder in the grouting material is greater than 30 parts, the formation rate of calcium sulfonate on the gypsum / glauber's salt interlayer is too fast. The rapid formation of calcium sulfonate will have many effects on the performance of the grouting material. On the one hand, the too fast formation rate may make the crystal structure of calcium sulfonate not stable enough, making it difficult to form an effective barrier layer on the gypsum / glauber's salt interlayer. On the other hand, too fast reaction may lead to uneven local reaction, affecting the stability and durability of the entire grouting material system.

[0028] Specifically, when the steel slag powder in the grouting material is less than 8 parts, the speed of forming calcium sulfonate on the gypsum / glauber's salt interlayer is slow. When the steel slag powder content is too low, the substances participating in the reaction are relatively reduced, and the driving force of the reaction is insufficient, which slows down the speed of forming calcium sulfonate on the gypsum / glauber's salt interlayer. The slow formation of calcium sulfonate will bring a series of problems. First, an effective protective layer cannot be formed on the interlayer in time, and the dissolution of gypsum and Glauber's salt cannot be blocked in time, which may cause the damage to the structure to gradually increase. Secondly, the slow reaction speed may affect the progress and efficiency of the entire grouting project and extend the construction time.

[0029] In the embodiment of the present invention, the grouting material further includes 5 to 10 parts of an alkaline activator, wherein the alkaline activator mainly promotes the reaction of active components in the material by providing an alkaline environment. Under alkaline conditions, elements such as silicon and aluminum in the material can react chemically with alkali metal ions to form a gelling product.

[0030] Specifically, the alkaline activator can promote the dissolution of silicon-calcium-aluminum substances in blast furnace slag powder and steel slag powder, thereby accelerating the reaction of silicon-calcium-aluminum substances with sulfate ions in gypsum / glauber's salt karst foundation to form ettringite.

[0031] Preferably, the alkaline activator is at least one of water glass, sodium hydroxide and quicklime.

[0032] In an embodiment of the present invention, the grouting material also includes 3 to 5 parts of an expansion hardener and 1 to 2 parts of a stabilizer; wherein the expansion hardener can fill the tiny gaps and cracks between the grouting material and the injected structure, improve the overall density, and enhance the waterproof and anti-seepage properties; the stabilizer can prevent the grouting material from undergoing performance changes during storage, transportation and use, such as precipitation, stratification, deterioration, etc., to ensure that the grouting material always maintains good working performance.

[0033] Preferably, the expansion hardener is magnesium oxide, and the stabilizer is cellulose ether compound or polyvinyl alcohol.

[0034] See also Figure 1 , Figure 1 A flow chart of a method for preparing a grouting material for a gypsum / glauber's salt karst foundation provided in an embodiment of the present invention; wherein the method comprises: S10, mixing blast furnace slag powder and steel slag powder and grinding them to obtain a powder material; S20, mixing the powder material with water and stirring to obtain a grouting material.

[0035] Specifically, in step S10, a mixer is used to evenly mix blast furnace slag powder and steel slag powder, and a ball mill is used to grind the mixture.

[0036] In step S20, the stirring temperature of the stirring treatment is 20°C to 30°C, and the stirring time of the stirring treatment is 2 to 4 minutes.

[0037] Accordingly, the present invention further provides a grouting material for gypsum / glauber's salt karst foundation as described above and / or a preparation method for a grouting material for gypsum / glauber's salt karst foundation as described above for use in a gypsum / glauber's salt karst foundation reinforcement project; wherein the mechanism by which the grouting material can have good anti-corrosion performance in a gypsum / glauber's salt karst environment is as follows: Since both blast furnace slag powder and steel slag powder contain CaO and Al2O3, and although blast furnace slag powder and steel slag powder have certain potential activity, they basically do not react to hydration reaction in water alone. Therefore, in the absence of gypsum / glauber's salt, the material can diffuse with the water flow, and the effective components will not be reduced due to hydration reaction.

[0038] When the above grouting material reaches the environment with gypsum / glauber's salt, calcium sulfonate can be generated and attached to the gypsum / glauber's salt interlayer. The specific reaction is as follows: 6CaO+Al2O3+3CaSO4+61H2O=3CaO·Al2O3·3CaSO4·32H2O+29H2O.

[0039] Since ettringite is CaO, Al2O3 and SO4 2- The reaction generates SO4 in the environment 2- It will not corrode the newly formed calcium sulfide, thus achieving the effect of blocking dissolution. The technical solution of the present invention is now further described in conjunction with specific embodiments.

[0040] 1. Test methods of various embodiments and comparative examples Embodiment 1: This embodiment 1 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by weight: 95 parts of blast furnace slag powder, 5 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0041] Embodiment 2: This embodiment 2 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by mass: 92 parts of blast furnace slag powder, 8 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0042] Embodiment 3: This embodiment 3 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by mass: 90 parts of blast furnace slag powder, 10 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0043] Embodiment 4: This embodiment 4 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by mass: 85 parts of blast furnace slag powder, 15 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0044] Embodiment 5: This embodiment 5 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by mass: 80 parts of blast furnace slag powder, 20 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0045] Embodiment 6: This embodiment 6 provides a grouting material for gypsum / glauber's salt karst foundation, comprising the following components in parts by mass: 75 parts of blast furnace slag powder, 25 parts of steel slag powder, and 300 parts of water; wherein the blast furnace slag powder is 800 mesh S95 grade granulated blast furnace slag, and the steel slag powder is 1200 mesh II grade steel slag powder.

[0046] Comparative Example 1: Comparative Example 1 provides a grouting material for a gypsum / glauber's salt karst foundation, comprising 400 parts by mass of clean water.

[0047] Comparative Example 2: Comparative Example 2 provides a grouting material for gypsum / glauber's salt karst foundation, including 400 parts by mass of PO42.5 cement paste (water-cement ratio 1:1), wherein the PO42.5 cement paste is a slurry formed by mixing PO42.5 ordinary Portland cement and water.

[0048] II. Analysis of test results of various embodiments and comparative examples The grouting materials prepared in Examples 1 to 6 and Comparative Examples 1 to 2 were injected into a dynamic water test box containing a gypsum / glauber's salt sandwich core sample for 4 hours. Afterwards, the SO4 content of each test box was tested at intervals of 24 hours. 2- concentration, conductivity; until SO4 in all examples 2- After the temperature is 0, Examples 1 to 6 and Comparative Example 2 are cleaned.

[0049] See also Figure 2 , Figure 3a as well as Figure 3b , Figure 2 Schematic diagram of gypsum / glauber's salt sandwich core sample provided for multiple embodiments of the present invention; Figure 3a A schematic diagram of a core sample after the grouting material provided in some embodiments of the present invention is injected into a dynamic water test chamber in which a gypsum / glauber's salt sandwich core sample is placed and then taken out after 72 hours; Figure 3b A schematic diagram of a core sample taken out after 72 hours after the grouting material provided in Comparative Example 2 of the present invention is injected into a dynamic water test box in which a gypsum / glauber's salt sandwich core sample is placed; Figure 3a as well as Figure 3b It can be seen that the core samples of Examples 1 to 6 are all covered with a thick layer of gypsum / glauber's salt karst foundation dissolution blocking material (ettringite), while the cement slurry of Control Example 2 completely fills the entire test box, and Control Example 2 is processed into a cylindrical core sample.

[0050] See also Figure 4a , Figure 4a Schematic diagram of the equipment used for the dynamic water flushing test of the test pieces provided in Examples 1 to 6 of the present invention and Comparative Examples 1 to 2; the same SO4 as in Comparative Example 1 is used 2- The cylindrical core samples formed by the tests in the dynamic water test chamber of Examples 1 to 6 and Control Example 2 were subjected to a dynamic water scouring test with a concentration solution, and the respective dissolution amounts were recorded every 24 hours. After 24 hours, the dissolution amount of Control Example 1 was no longer tested, and the state of the specimens was observed. Figure 4b to Figure 4f As shown, Figure 4b A schematic diagram of a core sample of a test piece provided in Example 3 of the present invention after a 14-day dynamic water scouring test; Figure 4c A schematic diagram of a core sample of a specimen provided in Comparative Example 1 of the present invention after a 14-day dynamic water scouring test; Figure 4d A schematic diagram of a core sample of a specimen provided in comparative example 2 of the present invention after a 14-day dynamic water scouring test; Figure 4e A schematic diagram of a core sample of a test piece provided in Example 3 of the present invention after a 22-day dynamic water scouring test; Figure 4f Schematic diagram of the core sample of the specimen provided in Control Example 2 of the present invention after 22 days of dynamic water scouring test.

[0051] Specifically, by Figure 4b to Figure 4f It can be seen that the cylindrical core samples of the test pieces provided in Example 3 of the present invention were covered with a thick layer of gypsum / glauber's salt karst foundation dissolution blocking material after the 14d and 22d dynamic water scouring tests, and no dissolution occurred. The test pieces provided in Control Example 1 of the present invention all showed obvious dissolution after the 14d dynamic water scouring test.

[0052] Please refer to the following Table 1, which shows the dissolution results of the test pieces provided in Examples 1 to 6 of the present invention and Comparative Examples 1 to 2 after the dynamic water scouring test: Table 1

[0053] Specifically, it can be seen from Table 1 that the dissolution amount of the cylindrical core sample of Control Example 1 after the dynamic water scouring test after 24 hours of dynamic water scouring is 23%, indicating that obvious dissolution occurs; the cylindrical core samples of Examples 1 to 6 after the dynamic water scouring test are all covered with a thick layer of gypsum / glauber's salt karst foundation dissolution blocking material, and the dissolution amount after 24 hours of dynamic water scouring is 0, and the structure of the cylindrical core samples after the dynamic water scouring test is stable, indicating that they all have good dissolution performance, can remain stable for a long time in the groundwater environment, and effectively prevent the dissolution and migration of gypsum and Glauber's salt.

[0054] Furthermore, it can be seen from Table 1 that the cylindrical core samples formed by injecting PO42.5 cement slurry with a water-cement ratio of 1:1 into the control example 2 and placing the gypsum / glauber's salt interlayer showed a dissolution amount of 0 after a 24-hour dynamic water scouring test, indicating that the control example 2 also has a certain dissolution performance on the gypsum / glauber's salt interlayer. This is mainly because the main components in the PO42.5 cement, such as tricalcium silicate, dicalcium silicate, and tricalcium aluminate, will undergo hydration reactions in a water environment. When sulfate ions are present in the environment, the sulfate ions will react with the calcium hydroxide in the cement to form calcium sulfate, and the calcium sulfate may further react with the tricalcium aluminate in the cement to form calcium sulfonate. However, the formation of calcium sulfonate will cause the volume expansion of the cement, causing cracking and damage to the cylindrical core sample, which is not conducive to the foundation stability of the gypsum / glauber's salt interlayer. Figure 4d as well as Figure 4f shown.

[0055] The grouting material for gypsum / glauber's salt karst foundation provided by the embodiment of the present invention has good anti-corrosion performance, can maintain stability for a long time in the groundwater environment, effectively prevents the dissolution and migration of gypsum and Glauber's salt to block the dissolution of gypsum and Glauber's salt, and improves the stability and bearing capacity of the karst foundation. At the same time, the material should also have good construction performance, be easy to use in the complex and changeable karst foundation environment, and have reasonable cost and economic feasibility.

[0056] The grouting material for gypsum / glauber's salt karst foundation provided by the embodiment of the present invention has good flow permeability, has no hydration ability in the absence of gypsum / glauber's salt, and only has 2- The hydration reaction can only occur in an environment with high temperature, which can block the dissolution of gypsum / saltwater and has the advantages of low price. At the same time, the main materials of the grouting material are solid powders. Before use, you only need to add water and mix evenly to get the required grouting material. There is no need to prepare the activator solution in advance. It has the advantages of simple process and convenient construction.

[0057] Compared with other existing methods, the gain effects of the present invention include: (1) Compared with the existing barrier method, the design is more difficult and requires regular maintenance. However, the corrosion blocking treatment using the present invention is simple and easy to perform, has good durability, excellent corrosion resistance, and does not require regular maintenance.

[0058] (2) The pile-repairing method requires the pile to pass through the gypsum layer, which has a high processing cost. However, the present invention can react the gypsum interlayer in the rock layer and block the dissolution process, so the cost is low.

[0059] (3) Compared with the existing treatment technology, the present invention has the characteristics of low cost, targeted treatment, and green environmental protection. It can effectively and economically block the dissolution reaction and fundamentally solve the dissolution problem of gypsum interlayer.

[0060] In summary, different from the prior art, the present invention provides a grouting material for gypsum / glauber's salt karst foundation and its preparation method and application, the grouting material for gypsum / glauber's salt karst foundation comprises at least the following components by mass: 70-92 parts of blast furnace slag powder, 8-30 parts of steel slag powder, and 250-350 parts of water. The blast furnace slag powder and steel slag powder of the grouting material provided by the present invention undergo high-temperature melting and rapid cooling during the formation process, making its structure relatively dense and stable, and this structural stability avoids hydration reaction with water; when the above grouting material reaches an environment with gypsum / glauber's salt, the calcium oxide and aluminum oxide in the blast furnace slag powder and the steel slag powder can react with the sulfate ions in the gypsum / glauber's salt to generate calcium sulfonate and adhere to the gypsum / glauber's salt interlayer, thereby achieving the effect of blocking dissolution, thereby improving the stability of the gypsum / glauber's salt karst foundation.

[0061] It should be noted that the above embodiments all belong to the same inventive concept, and the description of each embodiment has its own focus. For matters that are not described in detail in some embodiments, reference may be made to the description in other embodiments.

[0062] The above embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A grouting material for gypsum / glauber's salt karst foundation, characterized in that: The invention comprises the following components in parts by weight: 70 to 92 parts of blast furnace slag powder, 8 to 30 parts of steel slag powder and 250 to 350 parts of water.

2. The grouting material for gypsum / glauber's salt karst foundation according to claim 1, characterized in that: The granulation grade of the blast furnace slag powder is ≥ S75, and the density of the blast furnace slag powder is ≥ 2.8 g / cm 3 , specific surface area ≥300m 2 / kg.

3. The grouting material for gypsum / glauber's salt karst foundation according to claim 1, characterized in that: The granulation grade of the steel slag powder is ≥ grade II, and the fineness of the steel slag powder is not less than 1200 meshes.

4. The grouting material for gypsum / glauber's salt karst foundation according to claim 1, characterized in that: The grouting material also includes 5 to 10 parts of an alkaline activator.

5. The grouting material for gypsum / glauber's salt karst foundation according to claim 1, characterized in that: The alkaline activator is at least one of water glass, sodium hydroxide and quicklime.

6. The grouting material for gypsum / glauber's salt karst foundation according to claim 1, characterized in that: The grouting material also includes 3 to 5 parts of an expansion hardener and 1 to 2 parts of a stabilizer.

7. The grouting material for gypsum / glauber's salt karst foundation according to claim 6, characterized in that: The expansion hardener is magnesium oxide, and the stabilizer is cellulose ether compound or polyvinyl alcohol.

8. A method for preparing a grouting material for gypsum / glauber's salt karst foundation according to any one of claims 1 to 7, characterized in that: The method comprises: S10, mixing blast furnace slag powder and steel slag powder and grinding them to obtain a powder material; S20, mixing the powder material with water and stirring to obtain a grouting material.

9. The method for preparing a grouting material for gypsum / glauber's salt karst foundation according to claim 8, characterized in that: In the step S20, the stirring temperature of the stirring treatment is 20°C to 30°C, and the stirring time of the stirring treatment is 2 to 4 minutes.

10. Use of a grouting material for gypsum / glauber's salt karst foundation according to any one of claims 1 to 7 and / or a preparation method of a grouting material for gypsum / glauber's salt karst foundation according to any one of claims 8 to 9 in a gypsum / glauber's salt karst foundation reinforcement project.

Citation Information

Patent Citations

  • Dispersion-resistant and high-impermeability grouting material under flowing water condition as well as preparation method and application thereof

    CN115504747A