Hydraulic composition, tackifier and additive thereof
By using the combination of hydroxyalkyl alkyl cellulose and specific polyethylene glycol derivatives in the hydraulic composition, the problem of increasing the amount of air and defoaming agents affecting the resistance to freezing damage is solved, and improvement is achieved Frost damage resistance, fluidity and ooze effect.
Patent Information
- Application Number
- CN202410719808.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-06
- Filing Date
- 2024-06-05
- Publication Date
- 2024-12-06
AI Technical Summary
The existing water-soluble cellulose ether increases the amount of air in concrete, resulting in a decrease in compressive strength, and the defoamer affects the frost damage resistance after removing the fine bubbles.
Using the combination of hydroxyalkyl alkyl cellulose and specific polyethylene glycol (PEG) derivatives, the hydraulic composition is improved by adjusting the IOB value and weight average molecular weight of the PEG derivative, combining water repellent and defoaming agents. Resistant to frost damage, fluidity and ooze.
The freezing damage resistance, fluidity and ooze properties of the hydraulic composition are significantly improved, ensuring the strength and stability of the concrete.
Smart Images

Figure BDA0004876722730000231 
Figure BDA0004876722730000241 
Figure BDA0004876722730000281
Abstract
Description
Technical Field
[0001] The present invention relates to a tackifier, a tackifier and an additive thereof. Background Art
[0002] Water-soluble cellulose ethers represented by hydroxyalkyl alkyl cellulose are widely used as thickeners for reducing exudation without losing fluidity. However, water-soluble cellulose ethers have air introduction ability, and there is a risk that the amount of air in the hydraulic composition or concrete increases to exceed the standard (4.5±1.5%), thereby reducing the compressive strength of the concrete. Therefore, one method is to add a defoaming agent to remove air bubbles to reduce the amount of air. However, this method causes deterioration of freezing resistance because fine air bubbles effective for freezing resistance are also removed at the same time.
[0003] A hydraulic composition using a water-soluble cellulose ether and also having frost damage resistance is known from Patent Document 1, which discloses a concrete composition comprising a concrete mixture consisting of a cement binder, aggregate, water, a water reducing agent and an air entraining (AE) agent, wherein 0.02 to 0.5% by weight (relative to the cement binder) of an alkali metal salt of sulfoethylcellulose and a nonionic water-soluble cellulose ether are added to the concrete mixture.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: JP-A H05-085791
[0007] Non-patent literature
[0008] Non-patent document 1: "Methods of emulsion formulation design, pages 2-9", Nihon Emulsion Co., Ltd., "What is emulsion formulation design based on organic concept map?" [January 10, 2023], URL <https: / / www.nihon-emulsion.co.jp / tech / organic.html> Summary of the invention
[0009] Although the sulfoethyl cellulose used in Patent Document 1 has low air incorporation, it has the disadvantage of increased fluidity. In addition, sulfoethyl cellulose is expensive and therefore is not preferred from an economical point of view. There is still room for improvement.
[0010] The present invention aims to provide a thickener for hydraulic compositions which can effectively formulate hydraulic compositions having satisfactory frost resistance, improved fluidity and reduced seepage; an additive for hydraulic compositions containing the thickener; and a hydraulic composition.
[0011] The present inventors have found that the use of a water-soluble cellulose ether in combination with a polyethylene glycol (PEG) derivative having a specific chemical structure can overcome the outstanding problems of hydraulic compositions including freeze damage, fluidity and exudation.
[0012] In one aspect, the present invention provides a thickener for a hydraulic composition, comprising: (A) hydroxyalkyl alkyl cellulose, and (B) a polyethylene glycol derivative, wherein the polyethylene glycol derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw measured by gel permeation chromatography relative to a polystyrene standard of 300 to 2500, and the polyethylene glycol derivative has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0013] In a preferred embodiment, the component (B) is at least one of the polyethylene glycol derivatives represented by the general formula (B1) and (B2):
[0014] RCOO-(C2H4O) n -H (B1)
[0015] (RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (B2)
[0016] Wherein, R and n are as defined above, R 1 A residue obtained by removing hydroxyl groups from a polyol having 2 to 5 hydroxyl groups, wherein the residue is a 2- to 5-valent C2-C5 straight-chain or branched hydrocarbon group, t and u are each integers of 1 to 4, the sum of t and u is an integer of 2 to 5, n1 and n2 are each an integer greater than 0, and n1×t+n2×u is an integer of 3 to 30.
[0017] Specifically, the hydroxyalkyl alkyl cellulose as the component (A) is hydroxypropyl methyl cellulose or hydroxyethyl methyl cellulose.
[0018] In a preferred embodiment, the viscosity of a 2 wt % aqueous solution of the hydroxyalkyl alkyl cellulose as the component (A) at 20° C. is 15 to 450,000 mPa·s.
[0019] The tackifier further includes a water repellent.
[0020] In another aspect, the present invention provides a viscosity-enhancing agent-containing additive for a hydraulic composition, comprising: the viscosity-enhancing agent defined above and (C) water and / or a liquid water-reducing agent.
[0021] In yet another aspect, the present invention provides a hydraulic composition comprising: the above-defined viscosity-enhancing agent-containing additive, a hydraulic substance, and water;
[0022] The hydraulic composition comprises: a viscosity enhancer as defined above, a hydraulic substance, and water and / or a liquid water reducing agent;
[0023] The hydraulic composition comprises: (A) hydroxyalkyl alkyl cellulose; (B) a polyethylene glycol derivative, wherein the polyethylene glycol derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw of 300 to 2500 measured by gel permeation chromatography relative to a polystyrene standard, and the polyethylene glycol derivative has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group; a hydraulic substance; and water and / or a liquid water reducing agent.
[0024] The hydraulic composition further comprises a water repellent.
[0025] In a preferred embodiment, the hydraulic composition is a concrete composition further comprising fine aggregate, coarse aggregate and a water reducing agent, wherein the slump of the concrete composition measured by the method of JIS A 1101 is 8 to 21 cm, and the compressive strength measured by the method of JIS A 1108 at 28 days is 18 to 45 N / mm 2 .
[0026] Advantageous Effects of the Invention
[0027] The use of a thickener for a hydraulic composition and a thickener-containing additive for a hydraulic composition can improve freezing resistance, fluidity, and oozing reduction in the hydraulic composition. DETAILED DESCRIPTION
[0028] <Thickening agent for hydraulic composition>
[0029] As used herein, Mw means weight average molecular weight, GPC means gel permeation chromatography, DS means “degree of substitution”, and MS means “molar substitution.” The notation (Cn-Cm) indicates a group containing n to m carbon atoms per group.
[0030] <Thickener>
[0031] One embodiment of the present invention is a thickener for a hydraulic composition. The thickener is defined as follows: comprising (A) hydroxyalkyl alkyl cellulose; and (B) a polyethylene glycol (PEG) derivative, wherein the PEG derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw measured by GPC relative to a polystyrene standard of 300 to 2500, and the polyethylene glycol derivative has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0032] Another embodiment of the present invention is a thickener-containing additive for a hydraulic composition, which contains (C) water and / or a liquid water reducing agent in addition to the thickener, ie, components (A) and (B).
[0033] In order to overcome the three prominent problems of freeze damage, fluidity and exudation of hydraulic compositions, the present inventors focused on the structure of polyethylene glycol (PEG) derivatives.
[0034] The present inventors have conducted the following research. In hydraulic compositions, it is believed that the structure of PEG affects the diameter of bubbles and defoaming properties that are easy to remove when it functions as a defoamer (considering frost resistance). In addition, it is believed that the monovalent hydrocarbon group at the end of the PEG derivative affects the dispersibility of cement particles (considering fluidity). Furthermore, it is believed that the size of the Mw of the PEG derivative affects the film thickness of water when water is adsorbed on cement particles (considering reduced exudation). Hydroxyalkyl alkyl cellulose plays a role in not hindering the effect produced by the PEG derivative from appearing or further enhancing the effect.
[0035] Through the above studies, the present inventors have found that PEG derivatives having a specific structure are advantageous. By combining hydroxyalkyl alkyl cellulose with a PEG derivative as a thickener for a hydraulic composition, significant improvements in freezing resistance, fluidity, and exudation reduction can be achieved.
[0036] One embodiment of the present invention is a thickener for a hydraulic composition, comprising: (A) hydroxyalkyl alkyl cellulose, and (B) a PEG derivative, wherein the PEG derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, a weight average molecular weight Mw measured by GPC relative to a polystyrene standard of 300 to 2500, and the PEG derivative has at least one RCOO (C2H4O) in the molecule. n -, wherein R is a linear or branched monovalent hydrocarbon group having 10 to 24 carbon atoms, n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
[0037] ((A) Hydroxyalkyl alkyl cellulose)
[0038] The hydroxyalkyl alkyl cellulose as the component (A) is a nonionic water-soluble cellulose ether. Examples thereof include hydroxypropyl methyl cellulose, hydroxyethyl methyl cellulose and hydroxyethyl ethyl cellulose. Among them, hydroxypropyl methyl cellulose (hereinafter also referred to as "HPMC") and hydroxyethyl methyl cellulose (hereinafter also referred to as "HEMC") are preferred from the perspective of both fluidity and reduced bleeding.
[0039] As the hydroxyalkyl alkyl cellulose, commercially available cellulose or cellulose produced by a known method can be used. The hydroxyalkyl alkyl cellulose can be used alone or in combination of two or more, depending on the purpose.
[0040] Among hydroxyalkyl alkyl celluloses, the DS of the methoxyl groups in hydroxypropyl methyl cellulose (HPMC) is preferably 1.00 to 2.20, more preferably 1.30 to 1.90, and the MS of the hydroxypropoxyl groups is preferably 0.10 to 0.60, more preferably 0.10 to 0.50. The DS of the methoxyl groups in hydroxyethyl methyl cellulose (HEMC) is preferably 1.00 to 2.20, more preferably 1.30 to 1.90, and the MS of the hydroxyethoxyl groups is preferably 0.10 to 0.60, more preferably 0.20 to 0.40. The DS of the ethoxyl groups in hydroxyethyl ethyl cellulose (HEEC) is preferably 1.00 to 2.20, more preferably 1.20 to 2.00, and the MS of the hydroxyethoxyl groups is preferably 0.05 to 0.60, more preferably 0.10 to 0.50.
[0041] It should be noted that the degree of substitution (DS) refers to the average number of alkoxy groups per unit of anhydrous glucose. The molar substitution (MS) refers to the average number of moles of hydroxyalkoxy groups per mole of anhydrous glucose. The DS of the alkoxy groups and the MS of the hydroxyalkoxy groups in the hydroxyalkyl alkylcellulose are determined by converting the values that can be measured by the analysis of the DS of hydroxypropylmethylcellulose (hydroxypropyl methylcellulose) described in the Japanese Pharmacopoeia (18th edition).
[0042] From the perspective of imparting a desired viscosity to the hydraulic composition, the viscosity of a 2 wt % aqueous solution of hydroxyalkyl alkyl cellulose at 20° C. is preferably 15 to 450,000 mPa·s, more preferably 50 to 370,000 mPa·s, and even more preferably 80 to 350,000 mPa·s. The viscosity of a 2 wt % aqueous solution of a water-soluble cellulose ether at 20° C. is measured using a single cylinder type rotational viscometer in accordance with the viscosity determination method of the general test method described in the Japanese Pharmacopoeia (18th edition) when the viscosity is 600 mPa·s or more. When the viscosity is less than 600 mPa·s, it is measured using an Ubbelohde viscometer in accordance with the capillary viscometer method of the viscosity determination method of the general test method described in the Japanese Pharmacopoeia (18th edition).
[0043] In the case of low-fluidity concrete such as ordinary concrete, cellulose ethers with low molecular weight or low viscosity are preferred from the perspective of reduced fluidity. In the case of high-fluidity concrete in which no reduction in fluidity occurs, cellulose ethers with high molecular weight or high viscosity are preferred from the perspective of cost. Specifically, for use in ordinary concrete, the viscosity of a 2 wt % aqueous solution of hydroxyalkyl alkyl cellulose at 20° C. is preferably 15 to 80,000 mPa·s, more preferably 50 to 50,000 mPa·s, and further preferably 80 to 35,000 mPa·s. For use in high-fluidity concrete, the viscosity of a 2 wt % aqueous solution of hydroxyalkyl alkyl cellulose at 20° C. is preferably 50,000 to 450,000 mPa·s, more preferably 60,000 to 370,000 mPa·s, and further preferably 70,000 to 350,000 mPa·s.
[0044] ((B) Polyethylene glycol derivatives)
[0045] The PEG derivative as component (B) should have an IOB value of 0.3 to 1.8 in the organic concept diagram, an Mw of 300 to 2500 measured by gel permeation chromatography relative to a polystyrene standard, and at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a terminal functional group.
[0046] [IOB value]
[0047] The IOB value of the PEG derivative in the organic concept diagram should be 0.3 to 1.8, preferably 0.7 to 1.2. If the IOB value is less than 0.3, the water solubility of the PEG derivative is poor. If the IOB value exceeds 1.8, the PEG derivative has a stronger surfactant effect and a poor defoaming effect, and cannot impart frost damage resistance to the hydraulic composition.
[0048] As the fluidity of the hydraulic composition decreases, more air is easily introduced during the mixing step, and thus a stronger defoaming ability is required. In this sense, the fluidity of the hydraulic composition is related to the IOB value of the PEG derivative in the organic concept diagram.
[0049] Specifically, in the case of a hydraulic composition having a slump of 8 to 21 cm obtained by the method in JIS A 1101, the IOB value of the PEG derivative in the organic concept diagram is preferably 0.3 to 1.4, more preferably 0.7 to 1.4, and further preferably 0.7 to 1.2. In the case of medium-flow concrete having a slump of 35 to 50 cm as specified in the East / Central / West Japan Expressway Tunnel Construction Management Guidelines and in the case of high-flow concrete having a slump of 55 to 75 cm as specified in the Construction Code of Concrete Standard Specification 2017, the IOB value of the PEG derivative in the organic concept diagram should preferably be 0.9 to 1.8, and more preferably 0.9 to 1.6.
[0050] It should be noted that IOB (Inorganic Organic Balance) in the organic concept diagram is the ratio of the inorganic value (IV) to the organic value (OV) determined based on the organic concept diagram. That is, IOB = IV / OV (the same below). The OV and IV of a compound are determined by adding the predetermined values of the groups or sites of the compound in the entire molecule. For IOB, reference should be made to "Methods for Emulsification Formula Design Pages 2-9", Japan Emulsion Co., Ltd., "What is the Emulsification Formula Design of the Organic Concept Diagram?" (Non-Patent Document 1).
[0051] Depending on the specific purpose, the PEG derivatives can be used alone or in combination of two or more. When two or more PEG derivatives are used as the (B) component, the IOB value of each PEG derivative in the organic concept diagram is 0.3 to 1.8.
[0052] [Weight average molecular weight]
[0053] The Mw of the PEG derivative measured by GPC relative to a polystyrene standard should be 300 to 2500, preferably 500 to 1300, and more preferably 500 to 1200. If the Mw is less than 300, the PEG derivative has poor dispersibility in water. If the Mw exceeds 2500, the PEG derivative cannot reduce the exudation of the hydraulic composition.
[0054] The Mw of PEG derivatives can be measured by GPC using tetrahydrofuran (THF) as a developing solvent relative to a polystyrene standard. Specifically, the test solution is injected into a high performance liquid chromatography device using a size exclusion column, the dissolution time is measured, and the Mw (hereinafter the same) is determined by comparing the measured value with a calibration curve of a standard solution.
[0055] In the PEG derivative, since the average number of added moles n of ethyleneoxy groups (-C2H4O-, EO) that affect the molecular weight is related to the IOB value, Mw is related to the fluidity of the hydraulic composition in the same manner as the IOB value. Specifically, in the case of a hydraulic composition having a slump of 8 to 21 cm measured by the method in JIS A1101, the Mw of the PEG derivative is preferably 300 to 1300, more preferably 500 to 1300, and further preferably 500 to 1200. In the case of medium-flowing concrete with a slump of 35 to 50 cm as specified in the East / Central / West Japan Expressway Tunnel Construction Management Guidelines and in the case of high-flowing concrete with a slump of 55 to 75 cm as specified in the Construction Code of Concrete Standard Specification 2017, the Mw of the PEG derivative is preferably 700 to 2500, and more preferably 700 to 1700.
[0056] [Structure of PEG derivatives]
[0057] PEG derivatives are asymmetric linear or branched structures with at least one RCOO (C2H4O) n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group (ie, has no functional group other than -OH group at the terminal).
[0058] In PEG derivatives, RCOO(C2H4O) in the molecule n The number of - is at least 1, preferably 1 to 4, and more preferably 1.
[0059] From the perspective of improving the fluidity and frost resistance of the hydraulic composition and the dispersibility of the PEG derivative in water, R is C 10 To C 24 , preferably C 16 To C 22A linear or branched monovalent hydrocarbon group. Examples of the monovalent hydrocarbon group R include linear alkyl groups such as lauryl, cetyl, stearyl, behenyl, undecyl, pentadecyl, heptadecyl, and heneicosyl; branched alkyl groups such as isostearyl, octyldodecyl, decyltetradecyl, isoheptadecyl, 16-methylhexadecyl, 2-octylundecyl, and 2-decyltridecyl; and linear alkenyl groups such as oleyl. From the perspective of the availability and handling of the compound, R is preferably a linear or branched alkyl group such as heptadecyl and isoheptadecyl.
[0060] From the viewpoint of improving the freezing resistance of the hydraulic composition, the PEG derivative has an ester bond (—COO—).
[0061] From the perspective of reducing the bleeding of the hydraulic composition, improving the frost resistance and preventing foaming, the average added molar number n of the ethyleneoxy group (-C2H4O-) is an integer of 3 to 40, preferably 5 to 30, and more preferably an integer of 5 to 20.
[0062] The PEG derivative as component (B) is preferably at least one of the compounds represented by general formulae (B1) and (B2). The compound having formula (B1) and the compound having formula (B2) are referred to as compounds B1 and B2, respectively.
[0063] RCOO-(C2H4O) n -H (B1)
[0064] (RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (B2)
[0065] In formula (B1) and (B2), R is independently C 10 ~C 24 A linear or branched monovalent hydrocarbon group, R 1 The residue is a residue obtained by removing a hydroxyl group from a polyol having 2 to 5 hydroxyl groups, the residue being a C2 to C5 straight-chain or branched hydrocarbon group having a valence of 2 to 5, the average number of moles of ethyleneoxy (-C2H4O-) added n being an integer of 3 to 40, t and u being each an integer of 1 to 4, and the sum of t and u being an integer of 2 to 5 (equivalent to the number of moles of R obtained therefrom) 1 The number of hydroxyl groups in the polyol), n1 and n2 are each an integer greater than 0 (equivalent to the average number of moles of ethylene oxide (-C2H4O-) added), and n1×t+n2×u is an integer from 3 to 30.]
[0066] [Compound B1]
[0067] Compound B1 is a compound of formula (B1) having an IOB value of 0.3 to 1.8 in an organic concept diagram and an Mw of 300 to 2500 as measured by GPC relative to a polystyrene standard.
[0068] In formula (B1), from the perspective of improving fluidity and freezing resistance and the solubility of the PEG derivative in water, R is as defined above and each independently is C 10 ~C 24 , preferably C 16 ~C 22 Examples of the monovalent hydrocarbon group R are as exemplified above.
[0069] In the formula (B1), from the viewpoint of improving the freezing resistance of the hydraulic composition, an ester bond (—COO—) is present, and n is as defined above.
[0070] Examples of compound B1 include polyethylene glycol monostearate (the average number of added moles of ethylene oxide (-C2H4O-) is 5, 10, 20, 30), polyethylene glycol monoisostearate (the average number of added moles of ethylene oxide (-C2H4O-) is 6, 8, 10, 12, 16), and polyethylene glycol monooleate (the average number of added moles of ethylene oxide (-C2H4O-) is 6, 10).
[0071] When the melting point of compound B1 is above 40°C, it can be crushed and used as a powder. When the melting point of compound B1 is less than 40°C, it becomes a liquid or a waxy solid that is difficult to crush at room temperature (20°C±15°C), so it is difficult to use in powder form. When the average number of added moles of ethyleneoxy (-C2H4O-) in formula (B1) is less than 15, the compound is a ductile solid, so it is difficult to crush even if the melting point is above 40°C.
[0072] When the compound B1 is used in the form of a powder, the average particle size of the powder measured by a dry laser method is preferably 10 to 280 μm, more preferably 10 to 200 μm, and further preferably 10 to 150 μm, from the perspective of preventing the concrete composition from losing fluidity due to poor dissolution. In addition, the proportion of particles having a particle size of 300 μm or more is preferably 0 to 10% by volume, and more preferably 0 to 3% by volume.
[0073] As used herein, the average particle size (D50 or median diameter) of the powder and the volume fraction of particles with a particle size of 300 μm or more are determined by the following interference laser diffraction method: using a Master Sizer 3000 manufactured by Malvern Panalytical plc of the United Kingdom or a HELOS device manufactured by Sympatec GmbH of Germany, the powder sample is sprayed with compressed air, irradiated with laser radiation, the diffraction intensity is measured, and the volume-based average particle size (the same below) is calculated thereby.
[0074] [Compound B2]
[0075] Compound B2 is a compound of formula (B2) having an IOB value in an organic concept diagram of 0.3 to 1.8 and an Mw of 300 to 2500 as measured by GPC relative to a polystyrene standard.
[0076] In formula (B2), from the perspective of improving the fluidity and frost resistance of the hydraulic composition and the solubility of the PEG derivative in water, R is as defined above and each independently is C 10 ~C 24 , preferably C 16 ~C 22 Examples of the monovalent hydrocarbon group R are as exemplified above.
[0077] In the formula (B2), from the viewpoint of improving the freezing resistance of the hydraulic composition, an ester bond (—COO—) is present.
[0078] In formula (B2), R 1 The residue is a residue obtained by removing a hydroxyl group from a polyol preferably having 2 to 5, more preferably 2 or 3 hydroxyl groups, and the residue is preferably a C2 to C5 straight or branched hydrocarbon group having a valence of 2 to 5, more preferably 2 or 3. If the carbon number is less than 2 (i.e., equal to 1), the compound is difficult to synthesize, and if the carbon number is greater than 5, the compound may have high hydrophobicity and be difficult to dissolve or disperse in water.
[0079] Examples of the polyol include dihydric alcohols (having 2 hydroxyl groups) such as 1,2-butanediol and 1,3-butanediol; trihydric alcohols (having 3 hydroxyl groups) such as glycerol and trimethylolpropane; tetrahydric alcohols (having 4 hydroxyl groups) such as diglycerol, erythritol, pentaerythritol, sorbitan and methyl glucoside; pentahydric alcohols (having 5 hydroxyl groups) such as xylitol and triglycerol. Among them, dihydric alcohols and trihydric alcohols are preferred, and 1,2-butanediol and 1,3-butanediol are more preferred from the viewpoint of preventing foaming of the hydraulic composition.
[0080] In formula (B2), t and u are each an integer of 1 to 4, t is preferably 1 from the perspective of reducing bleeding, and u is preferably 1 or 2 from the perspective of preventing foaming of the hydraulic composition. The sum of t and u (i.e., t+u) is an integer of 2 to 5, which is equivalent to obtaining R 1 The sum of (t+u) is more preferably 2 or 3, and most preferably 2, from the perspective of preventing foaming of the hydraulic composition.
[0081] In formula (B2), n1 and n2 are each independently the average added molar number of ethyleneoxy (-C2H4O-), which is an integer greater than 0, and n1×t+n2×u is an integer from 3 to 30, preferably an integer from 5 to 30, more preferably an integer from 8 to 20, and further preferably an integer from 10 to 20.
[0082] Examples of compound B2 include PEG-10BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 10), PEG-15BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 15), PEG-20BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 20), and PEG-25BG isostearate (the total (n1+n2) of the average number of moles of ethyleneoxy (-C2H4O-) added is 25).
[0083] Compound B2 is a liquid or a waxy solid that is difficult to crush at room temperature (20°C ± 15°C), and therefore it is difficult to use it in a powder form.
[0084] The PEG derivative can be used without limitation in the case of solid or liquid. When the melting point of the PEG derivative is less than 40°C or the average number of added moles of ethyleneoxy (-C2H4O-) in formula (B1) is less than 15, the PEG derivative is preferably used as a solution in water and / or a liquid water reducing agent described later.
[0085] In the thickener for a hydraulic composition, the weight ratio of component (A) to component (B), i.e., A:B, is preferably 95:5 to 20:80, more preferably 93:7 to 30:70, and even more preferably 90:10 to 40:60, from the viewpoint of improving frost resistance, fluidity, and reducing oozing out.
[0086] (Other ingredients)
[0087] In addition to component (A) and component (B), the thickener may contain other components such as a water repellent, a gum, and a defoamer. These components may be introduced as contained in the hydraulic composition described later. In particular, when the other components are liquid, they are preferably used as a solution or dispersion in water, which is used to prepare a hydraulic composition or a thickener-containing additive for a hydraulic composition.
[0088] [Water repellent]
[0089] The water repellent used in this article is a substance that can increase the contact angle with water to impart water repellency. As long as it is a water repellent commonly used in the previous hydraulic composition, there is no particular restriction. Examples include, for example, hydrocarbons such as liquid paraffin, squalane, paraffin, and vaseline; waxes such as beeswax, jojoba oil, and carnauba wax; triglycerides such as triisostearate and tricaprylin; ester oils such as myristyl isocetyl and palmitic acid cetyl; higher alcohols such as cetyl alcohol and stearyl alcohol; vegetable oils such as olive oil and castor oil; fatty acids such as stearic acid; and fatty acid salts such as calcium stearate, sodium stearate, magnesium stearate, calcium isostearate, sodium isostearate, and magnesium isostearate. Among them, from the aspect of reducing the amount of addition, fatty acid salts are preferred, and calcium stearate is more preferred. For example, calcium stearate is commercially available from Fujifilm and Kou Pure Chemical Industries, Ltd.
[0090] From the viewpoint of handling, the water repellent is preferably added in the form of powder.
[0091] When used, the amount of the water repellent added is preferably 0.01 to 30% by weight, more preferably 1.8 to 20% by weight relative to the thickener. When the thickener is added to a hydraulic composition (specifically, a concrete composition), from the perspective of imparting water repellency, the amount of the water repellent added is preferably 0.01 to 30% by weight, more preferably 1.8 to 20% by weight. 3 The amount of the water repellent added to the hydraulic composition is preferably 0.05 to 200 g / m 3 , more preferably 10 to 100 g / m 3 .
[0092] [gum]
[0093] The gum used in this article is not particularly limited as long as it is a substance used in the conventional hydraulic composition. Among them, from the aspect of taking into account the fluidity of the hydraulic composition and the reduction of exudation, diutan gum, welan gum, xanthan gum, and gellan gum are preferred. The gums can be used alone or in combination.
[0094] Diutan gum is composed of sugar units of D-glucose, D-glucuronic acid, D-glucose, L-rhamnose, and 2 L-rhamnose, and is commercially available from CP Kelco under the trade name KELCO-CRETE-DG-F, for example. Welan gum is a structure in which L-rhamnose or L-mannose side chains are bound to a backbone in which D-glucose, D-glucuronic acid, and L-rhamnose are bound in a ratio of 2:2:1, and is commercially available from CP Kelco under the trade name CP KELCO K1A-96, for example. Xanthan gum, like cellulose, has a β-1,4-linked D-glucose backbone, and a side chain composed of 2 mannoses and 1 glucuronic acid, and is commercially available from Sanjing Co., Ltd. under the trade name KELZAN, for example. Gellan gum is a heteropolysaccharide composed of four sugars, D-glucose, D-glucuronic acid and L-rhamnose, bonded in a ratio of 2:1:1, as repeating units, and is commercially available from CP Kelco, for example, under the trade name KELCOGELAFT.
[0095] The gum may be added in the form of a powder or an aqueous solution. From the viewpoint of handling, it is preferably added in the form of a powder.
[0096] When used, the amount of the gum added is preferably 0.004 to 15% by weight, more preferably 0.0125 to 12.5% by weight relative to the thickener. When the thickener is added to a hydraulic composition (specifically, a concrete composition), from the perspective of both fluidity and reduced oozing, the amount of the gum added is preferably 0.004 to 15% by weight, more preferably 0.0125 to 12.5% by weight relative to the thickener. 3 The amount of gum added to the hydraulic composition is preferably 5 to 100 g / m 3 , more preferably 5 to 30 g / m 3 , more preferably 10 to 30 g / m 3 .
[0097] [Defoaming agent]
[0098] In order to give the hydraulic composition strength, a defoamer may be added as needed. From the aspect of defoaming performance, suitable defoamers include oxyalkylene-based, silicone-based, alcohol-based, and fatty acid ester-based defoamers. In particular, from the aspect of frost resistance, oxyalkylene-based defoamers are preferred.
[0099] Examples of oxyalkylene defoaming agents include polyoxyalkylenes such as (poly)oxyethylene (poly)oxypropylene adducts; (poly)oxyalkylene alkyl ethers such as diethylene glycol heptyl ether, polyoxyethylene oleyl ether, polyoxypropylene butyl ether, polyoxyethylene polyoxypropylene 2-ethylhexyl ether, and oxyethylene propylene oxide adducts of higher alcohols having 8 or more carbon atoms or secondary alcohols having 12 to 14 carbon atoms; (poly)oxyalkylene (alkyl) aryl ethers such as polyoxypropylene phenyl ether and polyoxyethylene nonyl phenyl ether; oxyalkylenes and acetylene alcohols such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 2,5-dimethyl-3-hexyne-2,5-diol, and 3-methyl-1-butyn-3-ol; (poly)oxyalkylene fatty acid esters such as diethylene glycol oleate, diethylene glycol laurate, and ethylene glycol distearate; (poly)oxyalkylene sorbitan fatty acid esters such as polyoxyethylene sorbitan monolaurate and polyoxyethylene sorbitan trioleate; (poly)oxyalkylene alkyl (aryl) ether sulfates such as sodium polyoxypropylene methyl ether sulfate and sodium polyoxyethylene dodecylphenol ether sulfate; (poly)oxyalkylene alkyl phosphates such as (poly)oxyethylene stearyl phosphate; (poly)oxyalkylene alkylamines such as polyoxyethylene laurylamine; and polyoxyalkylene amides.
[0100] Examples of the silicone-based defoaming agent include dimethyl silicone oil, silicone paste, silicone emulsion, organo-modified polysiloxane (ie, polyorganosiloxane such as dimethyl polysiloxane), and fluorosilicone oil.
[0101] Examples of the alcohol-based defoaming agent include octanol, 2-ethylhexanol, hexadecanol, acetylene alcohols, and glycols.
[0102] Examples of the fatty acid ester-based antifoaming agent include glyceryl monoricinoleate, alkenyl succinic acid derivatives, sorbitan monolaurate, sorbitan trioleate, and natural waxes.
[0103] The defoaming agent can be added in the form of powder or liquid. From the viewpoint of handling, it is preferably added in the form of powder.
[0104] When used, the amount of the defoamer added is preferably 0.0025 to 15% by weight, more preferably 0.008 to 12.5% by weight, relative to the weight of the thickener. When the thickener is added to a hydraulic composition (specifically, a concrete composition), the amount of the defoamer added is preferably 0.0025 to 15% by weight, more preferably 0.008 to 12.5% by weight. 3 The amount of the defoaming agent added to the hydraulic composition is preferably 5 to 100 g / m 3 , more preferably 5 to 30 g / m 3 , more preferably 10 to 30 g / m 3 .
[0105] It should be noted that the total amount of the component (A), the component (B), the water repellent, the gum, and the defoaming agent is 100% by weight.
[0106] <Additives containing thickeners>
[0107] Another embodiment of the present invention is a viscosity-enhancing additive for a hydraulic composition, which comprises the viscosity-enhancing agent defined above, (C) water and / or a liquid water-reducing agent.
[0108] When a thickener is added to a hydraulic composition, a thickener in powder form may be added in this way. When the melting point of component (B) is less than 40°C or the average number of moles of ethylene oxide (-C2H4O-) in formula (B1) is less than 15 and it is difficult to crush (i.e., it is difficult to add the thickener in powder form), it is recommended to dissolve and disperse the thickener or the components constituting the thickener in (C) water and / or a liquid water reducing agent before adding to prepare an additive containing the thickener, and add the obtained additive to the hydraulic composition. The water and / or the liquid water reducing agent may be temperature-controlled when preparing the additive containing the thickener.
[0109] In the component (C), pure water, tap water, and "water other than tap water" shown in JIS A 5308 can be used as water.
[0110] Examples of liquid water reducing agents include lignin, polycarboxylic acids, and melamine-based agents.
[0111] Examples of lignin include lignin sulfonates and derivatives thereof. Examples of polycarboxylic acids include polycarboxylic acid ethers, composites of polycarboxylic acid ethers and crosslinked polymers, composites of polycarboxylic acid ethers and oriented polymers, composites of polycarboxylic acid ethers and highly modified polymers, polyether carboxylic acid polymers, maleic acid copolymers, maleate copolymers, maleic acid derivative copolymers, carboxyl-containing polyethers, polycarboxylic acid group-containing multipolymers having terminal sulfone groups, polycarboxylic acid graft copolymers, polycarboxylic acid compounds, and polycarboxylic acid ether polymers. Examples of melamine include melamine sulfonic acid formalin condensates, melamine sulfonate condensates, and melamine sulfonate polyol condensates.
[0112] The content of component (A) in the thickener-containing additive is preferably 0.005 to 20% by weight, more preferably 0.008 to 10% by weight, and further preferably 0.01 to 5% by weight. The content of component (B) in the thickener-containing additive is preferably 0.005 to 15% by weight, more preferably 0.008 to 10% by weight, and further preferably 0.01 to 5% by weight. The ratio of component (A) to component (B) expressed as a weight ratio (A:B) is preferably 95:5 to 20:80, more preferably 93:7 to 30:70, and further preferably 90:10 to 40:60 from the perspective of improving frost resistance, fluidity, and reducing oozing.
[0113] The content of (C) water and / or liquid water reducing agent is preferably 70.0 to 99.98% by weight, more preferably 85.0 to 99.97% by weight, and still more preferably 90 to 99.96% by weight relative to the additive containing the thickener. The total amount of component (C), components (A) and (B) and other components (described later) is 100% by weight of the additive containing the thickener.
[0114] When other or optional ingredients are added, the content of the water repellent is preferably 0.002 to 8% by weight, more preferably 0.005 to 5% by weight; the content of the gum is preferably 0.001 to 2% by weight, more preferably 0.005 to 1% by weight; the content of the defoaming agent is preferably 0.001 to 5% by weight, more preferably 0.005 to 3% by weight.
[0115] <Hydraulic composition>
[0116] In another aspect, the hydraulic composition according to the present invention relates to the following three embodiments.
[0117] Hydraulic composition (i): comprising a viscosity enhancer, a hydraulic substance (particularly, cement), and water and / or a liquid water reducing agent;
[0118] a hydraulic composition (ii): comprising an additive including a viscosity enhancer, a hydraulic substance (specifically, cement), and water; and
[0119] A hydraulic composition (iii): comprising: (A) hydroxyalkyl alkyl cellulose; (B) a polyethylene glycol derivative, wherein the polyethylene glycol derivative has an IOB value of 0.3 to 1.8 in an organic concept diagram, an Mw of 300 to 2500 measured by GPC relative to a polystyrene standard, and the polyethylene glycol derivative has at least one RCOO (C2H4O) in the molecule n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group; a hydraulic material (specifically, cement); and water and / or a liquid water reducing agent.
[0120] It should be noted that the component (B) may be added in the form of a powder, or may be added in the form of a solution or dispersion after being dissolved or dispersed in water and / or a liquid water reducing agent.
[0121] Exemplary uses of hydraulic compositions include concrete compositions, mortar compositions, and grout compositions.
[0122] The concrete composition comprises fine aggregate (specifically, sand), coarse aggregate (specifically, gravel) and a water reducing agent, and a hydraulic composition. Preferably, the concrete composition has a slump of 8 to 21 cm as measured by the method in JIS A 1101, and a compressive strength of 18 to 45 N / mm at 28 days as measured by the method in JIS A 1108. 2 , more preferably 25 to 40 N / mm 2 .
[0123] Examples of the concrete composition include ordinary concrete, underwater concrete, blown-fill concrete, cold-season concrete, summer-season concrete, mass concrete, lightweight concrete, seawater-exposed concrete, short-fiber reinforced concrete, dam concrete, paving concrete, and prestressed concrete.
[0124] The mortar composition includes fine aggregate (specifically, sand) and a hydraulic composition. Examples of the mortar include tiling mortar, repair mortar, and self-leveling material.
[0125] The grout composition is composed of a hydraulic composition, and examples thereof include adhesives for tile-based inorganic building materials and grouting materials for filling gaps between members.
[0126] From the perspective of fluidity, seepage reduction and frost resistance, per cubic meter (m 3 ) in the hydraulic composition (specifically, the concrete composition), the amount of the thickener in the hydraulic composition (i) or the amount of the thickener-containing additive in the hydraulic composition (ii) is preferably 0.025 to 10.0 kg / m 3 , more preferably 0.05 to 5.0 kg / m 3 .
[0127] From the perspective of both fluidity and leakage reduction of the hydraulic composition, the volume per cubic meter (m 3 The amount of component (A) or hydroxyalkyl alkyl cellulose added to the hydraulic composition (specifically, concrete composition) is preferably 10 to 1500 g / m 3 , more preferably 15 to 1000 g / m 3 .
[0128] From the perspective of fluidity, oozing reduction and frost resistance of hydraulic compositions, 3 The amount of the component (B) added to the hydraulic composition (specifically, the concrete composition) is preferably 10 to 300 g / m 3 , more preferably 10 to 150 g / m 3 .
[0129] Hydraulic material refers to cement and inorganic powder system mixed materials in the ingredients matched when manufacturing hydraulic composition. Cement can be used alone or in combination with mixed materials, as long as the desired strength, durability and other properties can be obtained. Examples of cement include Portland cement (e.g., ordinary Portland cement, early-strength Portland cement, ultra-early-strength Portland cement, medium-heat Portland cement), mixed cement (e.g., blast furnace cement, silica cement, fly ash cement), special cement (e.g., alumina cement). Examples of mixed materials include slag, fly ash, silica fume, and limestone powder.
[0130] When the hydraulic composition is concrete, the amount of the hydraulic substance added to the concrete is preferably 270 to 550 kg / m 3 When the hydraulic composition is mortar, the amount of the hydraulic material added to the mortar is preferably 300 to 900 kg / m 3 When the hydraulic composition is cement paste, the amount of the hydraulic material added to the cement paste is preferably 900 to 1600 kg / m 3 These amounts are preferred from the aspect of strength.
[0131] Examples of water include tap water, and "water other than tap water" shown in JIS A 5308. The unit amount of water in concrete is preferably up to 185 kg / m 3 .
[0132] The water / hydraulic substance ratio in the hydraulic composition is preferably 30 to 70% by weight, more preferably 35 to 65% by weight, in view of preventing separation of the materials.
[0133] The hydraulic composition may further comprise aggregate as required. Suitable aggregates include fine aggregate and coarse aggregate. Examples of fine aggregate include river sand, mountain sand, land sand, crushed sand, silica sand, etc. The particle size (maximum particle size) of fine aggregate is preferably less than 5 mm. Examples of coarse aggregate include river gravel, mountain gravel, land gravel, crushed stone, etc. The particle size (maximum particle size) of coarse aggregate is larger than the particle size of fine aggregate, preferably less than 40 mm, more preferably less than 25 mm.
[0134] When the hydraulic composition is concrete, 3 The content of fine aggregate is preferably 600 to 1100 kg, more preferably 700 to 1000 kg. When the hydraulic composition is mortar, the content of fine aggregate is preferably 600 to 1100 kg, more preferably 700 to 1000 kg. 3 The content of fine aggregate is preferably 900-1600kg, more preferably 1000-1400kg.
[0135] When the hydraulic composition is concrete, the amount of 3The content of coarse aggregate is preferably 600-1000kg, more preferably 650-900kg.
[0136] When the hydraulic composition is concrete, the proportion of fine aggregate as defined below is preferably 30 to 65% by volume, more preferably 35 to 60% by volume, and even more preferably 40 to 55% by volume relative to the total volume of the aggregate in order to maintain fluidity or sufficient strength.
[0137] Fine aggregate ratio (vol%) = volume of fine aggregate / (volume of fine aggregate + volume of coarse aggregate) × 100
[0138] Furthermore, in the hydraulic composition, in addition to the above-mentioned liquid water reducing agent, other water reducing agents may be added as needed in order to maintain high fluidity with a small amount of water. 3 The amount of water reducing agent added to the concrete composition, relative to each m 3 The unit cement amount is preferably 0.50 to 2.50 weight %, more preferably 0.5 to 1.0 weight %. When the desired fluidity is not obtained, two or more water reducing agents can be used.
[0139] In the hydraulic composition, in order to provide the desired amount of air and to make the hydraulic composition durable, an air entraining (AE) agent can be added as needed. Suitable AE agents include anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and rosin-based surfactants. Examples of anionic surfactants include resinate type, carboxylic acid type, sulfate type, sulfonic acid type, and phosphate type surfactants. Examples of cationic surfactants include amine salt type, primary amine salt type, secondary amine salt type, tertiary amine salt type, and quaternary ammonium salt type surfactants. Nonionic surfactants may include ester type, ester-ether type, ether type, and alkanolamide type surfactants. Examples of amphoteric surfactants include amino acid type and sulfobetaine type surfactants. Examples of rosin-based surfactants include abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, and dehydroabietic acid.
[0140] The amount of AE agent used per cubic meter of concrete composition is relative to 1m 3 The unit cement amount C is preferably 0.0001 to 0.050% by weight, more preferably 0.0001 to 0.01% by weight.
[0141] In the hydraulic composition, in order to manage the physical properties of the fresh hydraulic composition (fresh concrete, fresh mortar or fresh cement paste), a setting accelerator such as calcium chloride, lithium chloride or calcium formate; and a setting retarder such as sodium citrate or sodium gluconate may be used as needed.
[0142] The amount of coagulation retarder used is relative to the amount of 3The unit cement amount is preferably 0.3 to 1.2% by weight.
[0143] Furthermore, in order to prevent cracking due to shrinkage during setting and drying and cracking due to thermal stress caused by water and reaction heat of cement, a hauyne-based or lime-based expansive material may be added to the hydraulic composition as needed.
[0144] About the air void amount in the hydraulic composition, in order to improve the frost resistance, it is preferred to reduce the large bubbles with a bubble diameter exceeding 500 μm and less than 2000 μm, and increase the small bubbles with a bubble diameter exceeding 50 μm and less than 500 μm. As an index for evaluating the size of the bubbles, the bubble spacing coefficient is used. It is believed that when the bubble spacing coefficient is less than 250 μm, the frost resistance is better. The bubble spacing coefficient can be measured by air void analysis. When evaluating the bubble spacing coefficient, the bubble spacing coefficient also changes due to the increase or decrease of the air volume, so it is preferred to uniformly evaluate the air volume of concrete or mortar.
[0145] <Method for producing hydraulic composition>
[0146] The present invention relates to a method for producing a hydraulic composition comprising (A) hydroxyalkyl alkyl cellulose, (B) PEG derivative, hydraulic material, and water and / or liquid water reducing agent, wherein component (B) is a PEG derivative, has an IOB value of 0.3 to 1.8 in an organic concept diagram, has an Mw of 300 to 2500 measured by GPC relative to a polystyrene standard, and has at least one RCOO (C2H4O) in the molecule. n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group. The method involves:
[0147] Step (I), mixing the PEG derivative (B) and the component (A) or the hydroxyalkyl alkyl cellulose to prepare a viscosity increasing agent,
[0148] Step (II), adding water and / or at least a portion of a liquid water reducing agent to a tackifier to prepare an additive containing a tackifier, or
[0149] Step (III), separately preparing (B) a PEG derivative, and
[0150] In the step of mixing the hydraulic composition, the thickener in step (I), the additive containing the thickener in step (II), or the PEG derivative in step (III) is added.
[0151] A preferred method for preparing the hydraulic composition of the present invention is a method for preparing the following hydraulic composition, wherein the hydraulic composition is a concrete composition further comprising fine aggregate, coarse aggregate and a water reducing agent, wherein the concrete composition has a slump of 8 to 21 cm as measured by the method of JIS A 1101 and a compressive strength of 18 to 45 N / mm at 28 days as measured by the method of JIS A 1108. 2 .
[0152] ((I) Preparation of Thickener)
[0153] The thickener for hydraulic composition can be prepared by mixing the above-mentioned components, ie, hydroxyalkyl alkyl cellulose (A), PEG derivative (B) and the above-mentioned other components by a conventional method. There is no particular limitation on the mixing method. For example, a stirrer can be used.
[0154] There is no particular restriction on the order in which the ingredients are added during mixing. An exemplary process includes: adding ingredient (A) to a blender, stirring, then adding ingredient (B) and optionally other ingredients, and stirring the contents. At this time, the PEG derivative (B) can be added in powder or liquid form. From the perspective of handling and solubility when manufacturing a hydraulic composition, it is preferred that ingredient (A) and ingredient (B) are in powder form. That is, the thickener is preferably in powder form.
[0155] In the method for producing a hydraulic composition, it is preferred to further add a water repellent in step (I) to prepare a thickener.
[0156] ((II) Preparation of Thickener-Containing Additive)
[0157] The thickener-containing additive is obtained by adding at least a part of water and / or a liquid water reducing agent as a component (C) to the thickener. For example, the thickener-containing additive can be prepared by heating a part or all of the water and / or the liquid water reducing agent constituting the component (C) to 80 to 95°C, adding the hydroxyalkyl alkyl cellulose (A), the PEG derivative (B), the balance (C) component (water and / or the liquid water reducing agent), and other components to the high-temperature water (hot water) and / or the liquid water reducing agent, stirring and mixing them to dissolve them, cooling to room temperature (25±15°C), and stirring for 15 minutes to 1 hour. There is no particular limitation on the mixing method. For example, a stirrer can be used.
[0158] (Step of mixing components of hydraulic composition)
[0159] The method for producing a hydraulic composition comprises at least the steps of mixing the components of the hydraulic composition and adding a thickener, an additive containing a thickener or a PEG derivative (B) to the mixing of the components of the hydraulic composition.
[0160] The step of mixing the components of the hydraulic composition preferably includes: mixing all the powdered components other than water and / or the liquid water reducing agent in a dry state, adding water and / or the liquid water reducing agent to the dry mixture, and further mixing the contents. Preferably, the thickener, the additive containing the thickener, and the powdered component of the PEG derivative (B), that is, the thickener and the powdered PEG derivative (B) are put into the dry mixing step. In addition, preferably, the thickener, the additive containing the thickener, and the liquid component of the PEG derivative (B), that is, the additive containing the thickener and the liquid (B) PEG derivative are put into the dry mixing step.
[0161] For example, a hydraulic material as a powder material, optional aggregates (fine aggregate and coarse aggregate), and further optional defoamer, and a thickener are placed in a forced twin-screw mixer, followed by dry mixing. Then, water and / or a liquid water reducer are added as a liquid material to perform dry mixing and mixing to form a hydraulic composition (i). Alternatively, a hydraulic material as a powder material, optional aggregates (fine aggregate and coarse aggregate), and further optional defoamer are placed in a forced twin-screw mixer, followed by dry mixing. Then, water and an additive containing a thickener are added as liquid materials, dry mixing and mixing to form a hydraulic composition (ii). Alternatively, (A) hydroxyalkyl alkyl cellulose, (B) an IOB value of 0.3 to 1.8 in the organic concept diagram, an Mw of 300 to 2500 measured by GPC relative to a polystyrene standard, and at least one RCOO (C2H4O) in the molecule are placed in a forced twin-screw mixer. n -(where R is C 10 ~C 24 A powdered polyethylene glycol derivative having a polyethylene glycol terminal OH or -OH group as a functional group, a hydraulic material, and optional aggregates (fine aggregate and coarse aggregate), and an optional defoamer are dry mixed. Then, water and / or a liquid water reducer are added as a liquid material and mixed to form a hydraulic composition (iii). Alternatively, a hydraulic material as a powder material, optional aggregates (fine aggregate and coarse aggregate), and an optional defoamer are placed in a forced twin-screw mixer and dry mixed. Then, an aqueous solution or dispersion in which component (B) is dissolved and dispersed in water and / or a liquid water reducer, and water and / or a liquid water reducer are added as liquid materials, and dry mixed to form a hydraulic composition (iii).
[0162] As described above, a thickener, an additive containing the thickener, and a hydraulic composition capable of improving the fluidity, bleeding, and frost damage resistance of the hydraulic composition are obtained.
[0163] Example
[0164] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0165] I) Preparation of tackifier or additive containing tackifier
[0166] The following ingredients are used to prepare a tackifier or an additive containing a tackifier.
[0167] <Ingredients>
[0168] (1) Water: tap water
[0169] (2) Hydroxyalkyl alkyl cellulose (CE): Details are shown in Table 1.
[0170] (3) PEG derivatives: Details are shown in Table 2.
[0171] <Calculation of IOB value>
[0172] The IOB (Inorganic Organic Balance) value of the PEG derivatives was determined as follows.
[0173] The organic value (OV) and inorganic value (IV) of the compound of the object are determined by adding the predetermined values of the groups or sites on the compound in the entire molecule. For the predetermined values of each group or site of each compound, refer to "Methods for Emulsification Formula Design Pages 2-9", "What is Emulsification Formula Design of Organic Concept Diagram?" (Non-Patent Document 1) by Nippon Emulsion Co., Ltd., Figure 2 "Calculation Method Example" on page 2 and Appendix 1 "Inorganic Group, Organic Group and Organic / Inorganic Group Table".
[0174] Substitute IV and OV into the following formula to obtain the IOB value.
[0175] IOB value = IV / OV
[0176] A calculation example is shown below.
[0177] B1: In polyethylene glycol monostearate (C 17 H 35 COO(C2H4O) 10 H), by transforming -C2H4- in the first repeating unit (C2H4O) and -COO- bound thereto into (-COOR)-OCH2CH2 and COO(C2H4O) 10 -O-(C2H4O) in H 10-1 H transforms to -(OCH2CH2) 10-1 -OH, determine the structural formula such as "C 17 H35 CO·OCH2CH2(OCH2CH2) 10-1 -OH".
[0178] OV = 38 (number of C) × 20 (OV of C) = 760
[0179] IV = 60 (IV of -COOR) + 75 (IV of -OCH2CH2) × 9 (number of -OCH2CH2) + 100 (IV of -OH) = 835
[0180] From the above values, we obtain an IOB value of 835 / 760≈1.10.
[0181] <Measurement of Mw>
[0182] Mw was measured as the weight average molecular weight by GPC analysis using a GPC system HLC-8220GPC (manufactured by Tosoh Corporation). The GPC system had a detector (differential refractometer RI-71S (manufactured by Showa Denko K.K.)), columns (TSK-gel G5000HxL (7.8×300 mm)×1, G4000HxL (7.8×300 mm)×1, G3000HxL (7.8×300 mm)×1, G2000HxL (7.8×300 mm)×1 (manufactured by Tosoh Corporation)), tetrahydrofuran (THF) as a developing solvent, and the calculation was performed relative to a polystyrene standard.
[0183] By sampling an aliquot of about 0.01g of the PEG derivative, and adding about 10mL of THF to dissolve the PEG derivative, a test solution is prepared. Each (100 μL) of the test solution and a polystyrene standard (manufactured by Tosoh Corporation) is injected into the GPC system. THF is used for the mobile phase, and the column temperature is 40°C at a flow rate of 1.0mL / min. The results thus obtained are analyzed using a 480II data station GPC program (System Instruments Co., Ltd.). The molecular weight is calculated by AUTO fitting using the extrapolation curve method (once). The molecular weight is estimated using a calibration curve drawn based on the dissolution time and molecular weight of the polystyrene solution of the molecular weight standard.
[0184] (4) Calcium stearate (StCa): reagent (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)
[0185] (5) Defoamer I (DF-1): Polyether defoamer I (silica impregnated with defoamer)
[0186] [Table 1]
[0187]
[0188] [Table 2]
[0189]
[0190] (PEG-10)C 17 H 35 COO(C2H4O) 10 H
[0191] (PEG-20)C 17 H 35 COO(C2H4O) 20 H
[0192] (PEG-6)iso-C 17 H 35 COO(C2H4O)6H
[0193] (PEG-10BG)
[0194] [Preparation of Thickener-Containing Additives]
[0195] In a 5000 mL beaker, 2480 g of hot water at 90° C. was stirred at 100 rpm using a stirrer NZ-1000 (manufactured by Tokyo Rika Instruments Co., Ltd.). The selected ingredients of the type and amount (wt%) shown in Table 3A were added to the hot water so that the total weight of the ingredients was 20 g. The contents were stirred at room temperature (25° C.) for 60 minutes to obtain an additive containing a thickener in the form of an aqueous solution containing 1 wt % of the thickener (Examples 1 to 8, 10 to 13).
[0196] [Preparation of Thickener]
[0197] The selected ingredients of the types and amounts (wt%) shown in Table 3A were mixed to prepare a thickener. PEG-20 stearate was previously ground using Wonder Blender WB-1 (AS ONE CORP.) for 5 seconds, and the ground material was classified through a sieve with a mesh size of 300 μm, and a portion having an average particle size (D50) of 148 μm and containing 0.3% by volume of particles with a particle size of 300 μm or more was collected (Example 9, Comparative Examples 1 to 3).
[0198] [Added separately]
[0199] In the preparation, the ingredients shown in Table 3A were added to the concrete composition (Example 14) without any mixing or preparation steps. Specifically, PEG-10 stearate was added as a liquid material, and the remaining ingredients were added as powder materials. Furthermore, specifically, PEG-10 stearate was prepared by mixing pure water and a coarse granular PEG derivative of about 1 mm to several cm in a weight ratio of 99:1 in advance, and stirring the mixture to form a 100-fold dilution of the PEG derivative. In particular, the pure water used for diluting the PEG derivative corresponds to water as component (C) in the additive containing the thickener.
[0200] II) Preparation of hydraulic composition (concrete composition)
[0201] A hydraulic composition (concrete composition) was prepared using the following ingredients.
[0202] <Ingredients>
[0203] (1) Thickener-containing additives or thickeners: Additives No. 1 to 8, 10 to 13, Thickener No. 9, Comparative Thickeners No. 1 to 3 (see Table 3A)
[0204] (2) Water (W): tap water
[0205] (3) Hydroxyalkyl alkyl cellulose (CE): HPMC-1 in Table 1
[0206] (4) PEG derivatives: PEG-10 stearate in Table 2 (used in 100-fold dilution)
[0207] (5) Cement (C): Ordinary Portland cement (density: 3.16 g / cm 3 , Pacific Cement Co., Ltd.)
[0208] (6) AE water reducer (WR): lignin sulfonic acid (Master Pozzolith No. 70, manufactured by BASF Pozzolith, used in a 4-fold dilution)
[0209] (7) High-performance AE water reducer (SP): polycarboxylic acid oligomer (Chupole HP-11, manufactured by Takemoto Oil & Fats Co., Ltd.) (C x 0.85%)
[0210] (8) AE agent: resin acid salt type anionic surfactant (AE-300, manufactured by Takemoto Oil & Fats Co., Ltd., used in a 100-fold dilution: 1A = C x 0.001%)
[0211] (9) Defoamer II (DF-2) Polyether defoamer (used in 100-fold dilution, 1T = C x 0.002%)
[0212] (10) Fine aggregate (S): Land sand (produced in Shinano River, surface dry density: 2.60 g / cm 3 , water absorption rate: 2.07%, coarse particle rate: 2.79, solid volume percentage: 66.3%)
[0213] (11) Coarse aggregate (G): crushed stone (20-5 mm, surface dry density: 2.69 g / cm 3 , water absorption rate: 1.35%, coarse particle rate: 6.55, solid volume percentage: 58.5%)
[0214] The concrete mix shown in Table 4 was used for the test, i.e., under the following conditions: water / cement ratio 55.0%, fine aggregate ratio 52.9%, water 175 kg / m 3 、Cement 318kg / m 3 , fine aggregate 931kg / m 3 , coarse aggregate 861kg / m 3 As a unit quantity.
[0215] A hydraulic composition (concrete composition) was prepared using the formulation (additive components) in concrete shown in Table 3B. In Table 3B, the amounts of component (A), component (B), calcium stearate, and defoamer I added as thickener-containing additives or thickeners were expressed as the amount of the concrete composition per cubic meter (m3) of the concrete composition. 3 ) in grams, i.e. g / m 3 The addition amount of AE water reducer and high performance AE water reducer is the amount (C×%) relative to the wt% of cement (C), and the addition amount of AE agent is the amount recorded (unit A: 1A amount relative to 0.001wt% of cement (C)). The addition amount of defoamer II is the amount recorded (unit T: 1T amount relative to 0.002wt% of cement (C)).
[0216] In particular, the addition amount of the AE agent and the possible addition amount of the antifoaming agent II is adjusted to provide an air amount of 4.5±0.5%.
[0217] In Examples 9, 10 and Comparative Example 2, the formulation of Example 1 was changed as follows to adjust the slump. Specifically, in Example 9, the amount of AE water reducer added was changed to adjust the slump to 13.0±1.0 cm. In Example 10, a high-performance AE water reducer was further added as a liquid material to change the amount of AE water reducer added to adjust the slump to 20.0±1.0 cm. In Comparative Example 2, the amount of AE water reducer added was changed to adjust the slump to 10.0±1.0 cm.
[0218] The concrete composition was prepared using a 60L forced twin-screw mixer (WHQ-60A, manufactured by Kitagawa Iron Works). First, a powder material was added. That is, as a powder material, cement, fine aggregate, coarse aggregate, and the thickeners (thickener No. 9, comparative thickeners No. 1 to 3) in Example 9 and Comparative Examples 1 to 3 were added, respectively, and then dry mixed for 10 seconds. In the case of independent addition in Example 14, materials other than PEG-10 stearate were added, respectively, and then dry mixed for 10 seconds. Then, a liquid material was added. That is, as a liquid material, water, AE water reducer, high-efficiency water reducer (high-performance AE water reducer), AE agent, optional defoamer II, the thickener-containing additive prepared in the above I) in Examples 1 to 8 and 10 to 13, or in the case of independent addition in Example 14, a 100-fold dilution of PEG-10 stearate was added, followed by mixing for 90 seconds to obtain a concrete composition. The volume of the mixed concrete composition per batch was 50 liters. The amount of water added at this stage is the necessary weight of water in the concrete mix from Table 4 (175000 g / m 3 ) minus the weight of the liquid materials (additives containing thickeners (additives No. 1 to 8, 10 to 13), a 100-fold dilution of PEG-10 stearate of Example 14 (added alone), AE water reducer, high-efficiency water reducer, and defoamer II).
[0219] [Table 3A]
[0220]
[0221] [Table 3B]
[0222]
[0223] [Table 4]
[0224]
[0225] *Fine aggregate ratio (vol%) = (fine aggregate volume) / [(fine aggregate volume) + (coarse aggregate volume)] × 100
[0226] The obtained concrete compositions were tested under the following conditions.
[0227] <Fresh properties>
[0228] (Concrete temperature)
[0229] The material temperature was adjusted in such a way that the temperature of the concrete composition reached 20±3° C. at the end of mixing.
[0230] The sensor of a digital thermometer (model SN3200II, Thermo Scientific Corporation) was inserted into the concrete composition to measure the concrete temperature. All the concrete compositions showed a temperature within the range of 20±3°C.
[0231] (Slump)
[0232] The test was conducted in accordance with JIS A1101.
[0233] (Air volume test)
[0234] The amount of air (vol %) was measured in accordance with JIS A 1128 for the concrete composition just prepared (immediately after mixing).
[0235] (Exudation rate)
[0236] The exudation rate was measured in accordance with JIS A 1123 for the concrete composition just prepared (immediately after mixing).
[0237] (Air Void Analyzer (AVA) test or Bubble Spacing Factor)
[0238] Use an air void analyzer ( Glycerin (manufactured by German Instruments) and water were mixed in advance at a weight ratio of glycerin / water = 83 / 17 to prepare an AVA measurement solution.
[0239] The mixed concrete composition is passed through a sieve with a mesh size of 5 mm to collect the mortar composition for evaluating the bubble spacing coefficient. 20 ml of the sample is taken in a special syringe, about 2000 ml of water is injected into the measurement column, the bubbles attached to the column wall are removed with a brush, and 250 ml of the AVA measurement solution is injected into the bottom of the column using a special device. After injection, a culture dish for bubble sampling is set near the water surface of the column and fixed to the measurement part. After injecting 20 ml of the mortar composition taken in the syringe into the bottom of the column, the mortar composition is stirred for 30 seconds to fully release the air introduced into the mortar in the liquid. The bubble spacing coefficient is determined by measuring the released bubbles over time.
[0240] In calculating the air bubble spacing factor, in addition to the air volume of fresh concrete, the volume occupied by aggregates 5 mm or larger (i.e., mortar volume percentage) and the volume occupied by paste (paste volume percentage) need to be subtracted from the total volume of the mortar composition. The mortar volume percentage and the paste volume percentage are calculated by the following equations (I) and (II).
[0241] Mortar volume percentage (%) = [(V B +V W +V S) / 1000]×100 (I)
[0242] Paste volume percentage (%) = [(V B +V W ) / 1000]×100 (II)
[0243] V B :Volume of cement (=unit amount of cement (kg) / specific gravity of cement)
[0244] V W : The volume of liquid additives including water, AE agent and water reducing agent (same as the unit water volume)
[0245] V S :Volume of aggregates less than 5mm (=unit amount of fine aggregate / specific gravity of fine aggregate)
[0246] (Ratio of bubbles in each bubble diameter range)
[0247] When the air void analyzer is started according to the above steps, automatic measurement begins. Large bubbles rise faster in the column and are trapped under the petri dish, while small bubbles rise slower in the column. The bubble ratio in each bubble diameter range is automatically calculated by measuring the weight of the petri dish over time.
[0248] (Air volume (vol%))
[0249] The sum of the bubble ratios in each bubble diameter range is the air volume (vol %).
[0250] <Curing Properties>
[0251] (Compression Strength)
[0252] The compressive strength test was conducted on 28-day-old concrete according to JIS A 1108. The sample size was 10 cm (diameter) x 20 cm. The average value of three samples was used as the compressive strength of each level for evaluation.
[0253] (Freeze-thaw test)
[0254] The freeze-thaw test was carried out according to the A method in JIS A 1148-2010. The relative dynamic elastic coefficient was measured up to a maximum of 300 cycles. The size of the sample was 100 mm × 100 mm × 400 mm long. The average value of the three samples was used as the relative dynamic elastic coefficient of each level for evaluation. When the relative dynamic elastic coefficient became less than 60% before 300 cycles, the test was terminated at that cycle.
[0255] The durability index was calculated according to the following formula using the relative dynamic elastic coefficient and rounded off to an integer. A durability index of 60 or more was judged to be excellent in frost damage resistance.
[0256] Durability index = P × N / M
[0257] P: Relative dynamic elastic coefficient at N cycles (%), N: The smaller number between the number of cycles at which the relative dynamic elastic coefficient reaches 60% and 300 cycles, M: 300 cycles
[0258] The above test results are shown in Tables 5A and 5B.
[0259] [Table 5A]
[0260]
[0261] [Table 5B]
[0262]
[0263] The following conclusions were drawn from the above results: Examples 1 to 7 demonstrate that even if the viscosity, DS, and / or chemical structure of the hydroxyalkyl alkyl cellulose as component (A) are changed, the addition of the PEG derivative as component (B) can advantageously improve the three factors of fluidity, exudation, and frost resistance of the hydraulic composition.
[0264] Examples 8 to 13 demonstrate that when the PEG derivative as component (B) is structurally modified or a defoaming agent is added, the hydraulic composition is advantageously improved in terms of fluidity, exudation, and resistance to freezing damage.
[0265] Example 11 demonstrates that when calcium stearate is added, the hydraulic composition (concrete composition) further improves the frost resistance while maintaining the fluidity and improving the exudation.
[0266] Example 14 demonstrates that when the components are added individually, the hydraulic composition is advantageously improved in terms of fluidity, exudation, and resistance to freezing damage.
[0267] It should be noted that the present invention is not limited to the above-mentioned embodiments. The embodiments are merely exemplary, and any embodiments having substantially the same structure as the technical concept described in the following claims and having equivalent functions and results are included in the spirit and scope of the present invention.
Claims
1. A tackifier for a hydraulic composition, comprising: (A) hydroxyalkyl alkyl cellulose, and (B) a polyethylene glycol derivative, wherein The IOB value in the organic concept diagram is 0.3 to 1.8, the weight average molecular weight Mw measured by gel permeation chromatography relative to a polystyrene standard is 300 to 2500, and there is at least one RCOO (C2H4O) in the molecule n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group.
2. The thickener according to claim 1, wherein Component (B) is at least one of polyethylene glycol derivatives having the general formula (B1) and (B2): RCOO-(C2H4O) n -H(B1) (RCOO-(C2H4O) n1 ) t R 1 ((OC2H4) n2 -OH) u (B2) Where R and n are as defined above, R 1 A residue obtained by removing a hydroxyl group from a polyol having 2 to 5 hydroxyl groups, wherein the residue is a 2- to 5-valent C2-C5 straight-chain or branched hydrocarbon group, t and u are each integers of 1 to 4, the sum of t and u is an integer of 2 to 5, n1 and n2 are each an integer greater than 0, and n1×t+n2×u is an integer of 3 to 30.
3. The thickener according to claim 1, wherein The hydroxyalkyl alkyl cellulose as the component (A) is hydroxypropyl methyl cellulose or hydroxyethyl methyl cellulose.
4. The thickener according to claim 1, wherein The viscosity of a 2 wt % aqueous solution of the hydroxyalkyl alkyl cellulose as the component (A) at 20° C. is 15 to 450,000 mPa·s. 5 . The thickener according to claim 1 , further comprising a water repellent.
6. A viscosity-enhancing agent-containing additive for a hydraulic composition, comprising: the viscosity-enhancing agent according to claim 1, and (C) water and / or a liquid water reducing agent.
7. A hydraulic composition comprising: the additive containing a thickener according to claim 6, a hydraulic substance and water.
8. A hydraulic composition comprising: the viscosity enhancer according to claim 1, a hydraulic substance, and water and / or a liquid water reducing agent.
9. A hydraulic composition comprising: (A) hydroxyalkyl alkyl cellulose; and (B) a polyethylene glycol derivative, wherein The IOB value in the organic concept diagram is 0.3 to 1.8, the weight average molecular weight Mw obtained by gel permeation chromatography relative to a polystyrene standard is 300 to 2500, and there is at least one RCOO (C2H4O) in the molecule n -, where R is C 10 ~C 24 A linear or branched monovalent hydrocarbon group, wherein n is an integer of 3 to 40, and has a polyethylene glycol terminal OH or -OH group as a functional group; Hydraulic substances; and Water and / or liquid water reducing agent. 10 . The hydraulic composition according to claim 7 , further comprising a water repellent.
11. The hydraulic composition according to any one of claims 7 to 9, which is a concrete composition further comprising fine aggregate, coarse aggregate and a water reducing agent, in, The concrete composition has a slump of 8 to 21 cm measured by the method of JIS A 1101, and a compressive strength of 18 to 45 N / mm2 measured by the method of JIS A 1108 at 28 days. 2 .