Retarding method of unfired building material prepared from original-state shield muck
By using acrylate and polyaluminum chloride as retarders, the settling time of shield slag is delayed, and the problem of the fast settling time of alkali-activated gelling materials is solved, achieving better operability and strength performance.
Patent Information
- Application Number
- CN202410865978.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-12-06
AI Technical Summary
The alkali-excited gelling materials set too fast during the curing process of shield slag, which affects operability, and the existing retarder effect is limited, especially sodium gluconate and borax are ineffective on alkali-excited gelling materials.
Acrylate and polyaluminum chloride are used as retarders to form composite polymers or gels to adhere to the surface of slag particles, delaying the formation of slag cured body strength and controlling the initial settling time.
Without affecting the strength, the initial setting time of the shield slag-free building materials is extended to 1h-6h, the construction operability is improved, and the compressive strength of 7d is achieved in the absence of cement to reach more than 7MPa.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building material technology and solid waste treatment, and specifically relates to a slow-setting method for original shield slag unburned building materials based on alkali activation. Background Art
[0002] Shield slag is generated during the tunneling process of the shield machine. After the cutterhead cuts the soil in front, it enters the soil bin and is transported or pumped to the ground slag pool by screw conveyors, belt conveyors, and rail slag trucks. The shield excavation method is usually selected based on the particle size distribution and permeability coefficient of the stratum to be crossed, mainly including slurry balance shield, earth pressure balance shield, and hard rock TBM shield. Among them, earth pressure balance shield accounts for more than 90%, so a large amount of shield slag will be generated. For example, cities such as Shenzhen and Wuhan generate more than 100 million cubic meters of slag each year, and the current disposal method is basically to transport it to designated slag disposal sites for disposal.
[0003] Therefore, how to deal with shield slag, especially earth pressure balance shield slag, will be an unavoidable problem in subway construction. Shield slag is composed of crushed stone, sand, silt, clay, water, etc., and is a good construction raw material. Such as traditional cement lime solidification, slag silicate solidification, ion solution solidification, bio-enzyme solidification, and microbial solidification, it can be prepared into unburned bricks, pavement bricks, lightweight blocks, fillers, etc. However, cement and lime are not environmentally friendly, and ion solutions, bio-enzymes, and microorganisms have the disadvantages of low strength of slag solidified soil, high solidification cost, and poor applicability to different soils.
[0004] Alkali-activated cementitious materials have the characteristics of abundant raw material sources, easy access, and low carbon emissions. Therefore, for shield slag in different regions, alkali-activated cementitious materials can be used for coordinated disposal to prepare green building materials, and "waste into treasure" can be achieved by "treating waste with waste" to increase added value. At the same time, although alkali-activated cementitious materials have the advantages of high strength, acid and alkali resistance, and high temperature resistance, they also have disadvantages such as fast setting time, high brittleness, and alkali efflux. In the preliminary work, it was found that alkali-activated waste slag solidified shield slag unburned building materials also have related problems. Among them, the fast setting time affects the operability of the shield slag solidification slurry, resulting in the inability to pour and discharge materials on site in time. Therefore, it is necessary to regulate the setting time of alkali-activated waste slag solidified original shield slag.
[0005] The retarding method for alkali-activated cementitious materials mainly involves adding retarders to control the setting time. Commonly used retarders include sodium gluconate, malic acid, sucrose, zinc salts, phosphoric acid and phosphates, borax and borates. Since the hydration reaction mechanism of alkali-activated cementitious materials is different from that of traditional cement-based materials, the retarding effect is also different. For example, sodium gluconate and borax are basically ineffective in retarding the setting of alkali-activated cementitious materials. Specifically, when the dosage is small, the setting time is almost unaffected, and when the dosage is increased, the strength is greatly affected. Therefore, it is necessary to explore retarders suitable for alkali-activated original shield slag unburned building materials. Summary of the invention
[0006] Based on the above technical problems existing in the prior art, the present invention provides a retarding method for original shield slag unburned building materials, aiming to solve the problem of fast setting time of original shield slag unburned building materials based on alkali excitation.
[0007] To achieve the above-mentioned purpose, the present invention provides a retarding method for original shield slag unburned building materials, which uses specific organic compounds and / or inorganic high molecular polymers as retarders to form composite polymers or coagulants attached to the surface of slag particles, delaying the formation of the strength of the slag solid body, thereby achieving the retarding effect.
[0008] The present invention can extend the initial setting time of the original shield slag unburned building material to 1h-6h without affecting the strength.
[0009] In order to achieve the above object, the technical solution of the present invention is as follows:
[0010] A method for retarding the setting of original shield slag unburned building materials, specifically comprising: the raw materials of the unburned building materials contain a retarder;
[0011] The fire-free building material comprises the following raw materials in percentage by mass: 55%-80% of original shield slag, 15%-40% of alkali-activated cementitious material, 1%-6% of water and 0%-1.5% of retarder; the content of retarder is greater than 0.
[0012] Preferably, the retarder is at least one of acrylate and polyaluminium chloride.
[0013] Preferably, the acrylate is at least one of magnesium acrylate, sodium acrylate and calcium acrylate.
[0014] Preferably, the original shield slag is the shield slag that has not been pre-treated by dehydration, screening, crushing, etc., and enters the soil bin after the shield machine's cutter head cuts the soil in front, and is transported or pumped to the ground slag pool by a screw conveyor, belt conveyor, or rail slag truck.
[0015] Preferably, the shield slag is at least one of earth pressure balance shield slag and slurry balance shield slag.
[0016] Preferably, the alkali-activated gelling material is composed of the following raw materials in mass percentage: 65%-95% of gelling component and 5%-35% of alkali activator.
[0017] Preferably, the gelling component is at least one of blast furnace slag, fly ash, silica fume, natural volcanic ash and steel slag.
[0018] Furthermore, the fineness of the gelling component is above 200 meshes.
[0019] Preferably, the alkaline activator is at least one of quicklime, sodium carbonate, sodium silicate, sodium aluminate, sodium hydroxide and sodium sulfate.
[0020] Preferably, the quicklime has a calcium content greater than 75% and a fineness greater than 100 meshes.
[0021] Preferably, the sodium carbonate is in powder form with a fineness greater than 100 mesh.
[0022] Preferably, the sodium silicate is in powder form, has a modulus of 2.0-3.2, and a fineness greater than 100 mesh.
[0023] Preferably, the sodium aluminate is in powder form with a fineness greater than 100 mesh.
[0024] Preferably, the sodium hydroxide is solid flake analytically pure with a purity greater than 99%.
[0025] Preferably, the acrylate is in solid or powder form.
[0026] Preferably, the polyaluminium chloride (PAC) is in solid or powder form and is easily soluble in water.
[0027] The present invention also provides an original shield slag unburned building material, wherein the raw materials of the unburned building material include the following components by mass percentage:
[0028] Original shield slag 55%-80%
[0029] Alkali activated gelling material 15%-40%
[0030] Water 1%-6%
[0031] Retarder 0%-1.5%;
[0032] Among them, the retarder content is greater than 0; the retarder includes at least one of acrylate and polyaluminium chloride; and the raw material of the fire-free building material does not contain cement.
[0033] Preferably, the acrylate is at least one of magnesium acrylate, sodium acrylate and calcium acrylate.
[0034] In some embodiments, the initial setting time of the fire-free building material is 1 hour to 6 hours.
[0035] Preferably, the original shield slag is the shield slag that has not been pre-treated by dehydration, screening, crushing, etc., and enters the soil bin after the shield machine's cutter head cuts the soil in front, and is transported or pumped to the ground slag pool by a screw conveyor, belt conveyor, or rail slag truck.
[0036] Preferably, the shield slag is at least one of earth pressure balance shield slag and slurry balance shield slag.
[0037] Preferably, the alkali-activated gelling material is composed of the following raw materials in mass percentage: 65%-95% of gelling component and 5%-35% of alkali activator.
[0038] Preferably, the gelling component is at least one of blast furnace slag, fly ash, silica fume, natural volcanic ash and steel slag.
[0039] Furthermore, the fineness of the gelling component is above 200 meshes.
[0040] Preferably, the alkaline activator is at least one of quicklime, sodium carbonate, sodium silicate, sodium aluminate, sodium hydroxide and sodium sulfate.
[0041] Preferably, the quicklime has a calcium content greater than 75% and a fineness greater than 100 meshes.
[0042] Preferably, the sodium carbonate is in powder form with a fineness greater than 100 mesh.
[0043] Preferably, the sodium silicate is in powder form, has a modulus of 2.0-3.2, and a fineness greater than 100 mesh.
[0044] Preferably, the sodium aluminate is in powder form with a fineness greater than 100 mesh.
[0045] Preferably, the sodium hydroxide is solid flake analytically pure with a purity greater than 99%.
[0046] Preferably, the acrylate is in solid or powder form.
[0047] Preferably, the polyaluminium chloride (PAC) is in solid or powder form and is easily soluble in water.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] The present invention uses organic compound acrylate and / or inorganic high molecular polymer polyaluminium chloride as retarders, and can regulate the setting time of alkali-activated waste slag solidified original shield slag by single or multiple doping of acrylate and polyaluminium chloride, thereby avoiding the situation that additional water is added to achieve retarding setting but the strength is greatly reduced, and the situation that traditional retarders such as sodium gluconate and borax are basically ineffective.
[0050] Acrylate is used as a retarder. Under a highly alkaline environment, it can initiate a free radical polymerization reaction to generate a gel with a three-dimensional network structure. The gel is a high molecular polymer that is insoluble in water but hygroscopic and swells. Therefore, in the original shield slag slurry based on alkali excitation, by adding a trace amount of acrylate, the generated high molecular gel can delay the gelling substances generated by the alkali-excited waste slag from enveloping the slag particles, thereby achieving a retarding effect. In the case of single polyaluminium chloride, the high water content and high mud content of the original shield slag are fully utilized. During the hydrolysis process, it is accompanied by physical and chemical processes such as coagulation, adsorption and precipitation, which wraps up the fine particles in the shield slag, especially the clay particles, and releases a small amount of water, which has the effect of dispersing the slag particles, that is, achieving a retarding effect. In addition, when acrylate and polyaluminium chloride are co-doped, the two are intricately intertwined and directly react to generate a composite polymer. The polymer gel component is relatively stable, does not decompose in water, and gradually adheres to the surface of the slag particles, delaying the formation of the strength of the slag solid body, thereby achieving a retarding effect.
[0051] The slow setting method of the original shield slag unburned building material provided by the present invention is suitable for solidification of the original shield slag based on alkali excitation, and solves the operability problem of preparing the original shield slag unburned building material on site. The present invention can extend the initial setting time of the original shield slag unburned building material to 1h-6h without affecting the strength. The present invention provides a new method for controlling the setting time of the shield slag unburned building material based on alkali excitation, which has important practical significance.
[0052] The original shield slag unburned building material provided by the present invention has an initial setting time of 1-6 hours. Construction personnel can adjust the initial setting time by adjusting the amount of retarder according to actual needs. In addition, in the absence of cement, the 7d compressive strength can reach more than 7MPa. DETAILED DESCRIPTION
[0053] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific implementation of the present invention is described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific implementation disclosed below.
[0054] The present invention aims to provide a retarding method for original shield slag unburned building materials based on alkali activation, the method comprising: the raw material of the unburned building materials contains a retarder;
[0055] The fire-free building material comprises the following raw materials in percentage by mass: 55%-80% of original shield slag, 15%-40% of alkali-activated cementitious material, 1%-6% of water and 0%-1.5% of retarder; the retarder content is greater than 0;
[0056] The retarder is at least one of acrylate and polyaluminium chloride.
[0057] Preferably, the acrylate is at least one of magnesium acrylate, sodium acrylate and calcium acrylate.
[0058] The original shield slag is the shield slag that enters the soil bin after the shield machine's cutter head cuts the soil in front, and is transported or pumped to the ground slag pool by a screw conveyor, belt conveyor, or rail slag truck, and has not been pre-treated by dehydration, screening, crushing, etc.
[0059] The shield slag is at least one of earth pressure balance shield slag and slurry balance shield slag.
[0060] The alkali-activated gelling material is composed of the following raw materials in percentage by mass: 65%-95% of gelling component and 5%-35% of alkali activator.
[0061] The gelling component is at least one of blast furnace slag, fly ash, silica fume, natural volcanic ash and steel slag.
[0062] The fineness of the gelling component is above 200 meshes.
[0063] The alkaline activator is at least one of quicklime, sodium carbonate, sodium silicate, sodium aluminate, sodium hydroxide and sodium sulfate.
[0064] The quicklime has a calcium content greater than 75% and a fineness greater than 100 meshes.
[0065] The sodium carbonate is in powder form with a fineness greater than 100 meshes.
[0066] The sodium silicate is in powder form, has a modulus of 2.0-3.2, and a fineness greater than 100 meshes.
[0067] The sodium aluminate is in powder form with a fineness greater than 100 meshes.
[0068] The sodium hydroxide is solid flake analytically pure with a purity greater than 99%.
[0069] The acrylate is in solid or powder form.
[0070] The polyaluminium chloride (PAC) is in solid or powder form and is easily soluble in water.
[0071] The slow setting method of the original shield slag unburned building material disclosed in the present invention is proposed based on the alkali-activated waste slag solidification system of the shield slag.
[0072] This specific embodiment also includes an alkali-activated original shield slag unburned building material prepared by the above-mentioned slow setting method; the raw materials of the unburned building material include the following components by mass percentage:
[0073] Original shield slag 55%-80%
[0074] Alkali activated gelling material 15%-40%
[0075] Water 1%-6%
[0076] Retarder 0%-1.5%;
[0077] Among them, the retarder content is greater than 0; the retarder includes at least one of acrylate and polyaluminium chloride; and the raw material of the fire-free building material does not contain cement.
[0078] The initial setting time of the fire-free building material is 1h-6h.
[0079] The following further lists relevant embodiments for detailed description. The original shield slag in the following embodiments is taken from the muddy siltstone slag of Changsha Metro Line 7.
[0080] Example 1
[0081] A slow setting method for original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.58% original shield slag, 4.78% water, 20.73% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.17% magnesium acrylate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0082] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 1 was 1h5min, and the 7d strength was 7.88MPa.
[0083] Example 2
[0084] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.47% original shield slag, 4.78% water, 20.70% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.31% magnesium acrylate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0085] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 2 was 1h32min, and the 7d strength was 7.98MPa.
[0086] Example 3
[0087] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.64% original shield slag, 4.79% water, 20.75% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.08% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0088] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 3 was 1h30min, and the 7d strength was 7.48MPa.
[0089] Example 4
[0090] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.58% original shield slag, 4.79% water, 20.73% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.16% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0091] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 4 was 3h30min, and the 7d strength was 7.43MPa.
[0092] Example 5
[0093] A slow setting method for original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.58% original shield slag, 4.79% water, 20.73% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, 0.08% magnesium acrylate, and 0.08% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0094] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 5 was 1h40min, and the 7d strength was 7.77MPa.
[0095] Example 6
[0096] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.53% original shield slag, 4.78% water, 20.71% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, 0.16% magnesium acrylate, and 0.08% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0097] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 6 was 1h18min, and the 7d strength was 7.31MPa.
[0098] Example 7
[0099] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.36% original shield slag, 4.77% water, 20.67% blast furnace slag, 2.38% quicklime, 1.91% sodium carbonate, 1.43% sodium silicate, and 0.48% magnesium acrylate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0100] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 7 was 3h32min, and the 7d strength was 7.82MPa.
[0101] Example 8
[0102] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.15% original shield slag, 4.75% water, 20.60% blast furnace slag, 2.38% quicklime, 1.90% sodium carbonate, 1.43% sodium silicate, and 0.79% magnesium acrylate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0103] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 8 was 4h7min, and the 7d strength was 7.52MPa.
[0104] Example 9
[0105] A slow setting method for original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.53% original shield slag, 4.78% water, 20.72% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.43% sodium silicate, and 0.24% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0106] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 9 was 4h51min, and the 7d strength was 8.14MPa.
[0107] It can be seen from the above-mentioned Examples 1, 2, 7 and 8 that when magnesium acrylate is added alone, the initial setting time of the original shield slag unburned building material gradually increases with the increase of the added magnesium acrylate. It can be seen from Examples 3, 4 and 9 that when polyaluminium chloride is added alone, the initial setting time of the original shield slag unburned building material also gradually increases with the increase of the added polyaluminium chloride. At the same time, it can be seen from Examples 5 and 6 that the co-addition of magnesium acrylate and polyaluminium chloride can also effectively prolong the initial setting time, that is, the purpose of regulating the initial setting time can be achieved by controlling the addition amount of magnesium acrylate and polyaluminium chloride.
[0108] The following Comparative Examples 1 and 2 are used as comparative examples of Examples 1 to 9. It can be seen that the initial setting time of Comparative Example 1 is only 30 minutes without adding a retarder, which is relatively short. Although Comparative Example 2 prolongs the initial setting time by adding added water, the strength loss is relatively large. In addition, it can be seen from the 7d strength of Examples 1 to 9 that, compared with the 7d strength of Comparative Example 1, the initial setting time is effectively prolonged while the strength remains basically unchanged.
[0109] Comparative Example 1
[0110] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.69% original shield slag, 4.79% water, 20.77% blast furnace slag, 2.39% quicklime, 1.92% sodium carbonate, and 1.44% sodium silicate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0111] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Methods for Standard Consistency Water Consumption, Setting Time and Stability of Cement". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in this comparative example 1 was 30 minutes, and the 7d strength was 7.79MPa.
[0112] Comparative Example 2
[0113] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by weight: 66.56% original shield slag, 7.57% water, 20.12% blast furnace slag, 2.32% quicklime, 1.86% sodium carbonate, 1.40% sodium silicate, and 0.17% magnesium acrylate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0114] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Methods for Testing Water Consumption, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in this comparative example 2 was 4h10min, and the 7d strength was 4.53MPa. From the above results, it can be seen that by adding a certain amount of additional water, the initial setting time can be effectively extended to 4h10min, but the strength is greatly affected. Compared with comparative example 1, the 7d strength decreased by about 42%.
[0115] Example 10
[0116] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 69.52% original shield slag, 4.85% water, 19.40% blast furnace slag, 3.23% fly ash, 1.13% sodium hydroxide, 1.46% sodium silicate, 0.33% sodium sulfate, and 0.08% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0117] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 10 was 1h53min, and the 7d strength was 15.19MPa.
[0118] Embodiment 11
[0119] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 69.47% original shield slag, 4.85% water, 19.39% blast furnace slag, 3.23% fly ash, 1.13% sodium hydroxide, 1.45% sodium silicate, 0.32% sodium sulfate, and 0.16% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0120] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 11 was 3h45min, and the 7d strength was 15.12MPa.
[0121] Example 12
[0122] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 69.41% original shield slag, 4.84% water, 19.38% blast furnace slag, 3.23% fly ash, 1.13% sodium hydroxide, 1.45% sodium silicate, 0.32% sodium sulfate, 0.16% magnesium acrylate, and 0.08% polyaluminium chloride. The raw materials are mixed and stirred evenly, then put into a mould, and the setting time of the slurry is tested.
[0123] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Methods for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 12 was 1h18min, and the 7d strength was 14.29MPa.
[0124] It can be seen from the above-mentioned Examples 10, 11 and 12 that, compared with Comparative Example 3, the initial setting time can be effectively extended to more than 1 hour by co-adding magnesium acrylate and polyaluminium chloride, and the 7d strength is slightly increased. The following Comparative Example 3 is used as a comparative example of Examples 10 to 12. It can be seen that the initial setting time of Comparative Example 3 is only 47 minutes, less than 1 hour, without adding a retarder, which shows that magnesium acrylate and polyaluminium chloride can play a role as retarders in different alkali activator systems.
[0125] Comparative Example 3
[0126] A method for retarding the setting of original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 69.58% original shield slag, 4.85% water, 19.42% blast furnace slag, 3.24% fly ash, 1.13% sodium hydroxide, 1.46% sodium silicate, and 0.32% sodium sulfate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0127] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Method for Testing Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in Example 12 was 47 minutes, and the 7d strength was 13.92 MPa.
[0128] As a comparative example of Example 1 to Example 12 (especially Example 3 and Example 4), the following Comparative Examples 4 and 5 select sodium gluconate as a retarder. It can be seen from the results that after adding the same weight of sodium gluconate, the initial setting time of the original shield slag unburned building material slurry is directly extended to more than 22 hours, which seriously affects demoulding. At the same time, it also greatly reduces the 7d strength of the unburned building material. Compared with Comparative Example 4, after adding twice the sodium gluconate, the 7d strength of Comparative Example 5 is close to 0. In summary, this shows that sodium gluconate is not suitable for the retarding of the original shield slag unburned building material solidified by alkali-activated waste slag.
[0129] Comparative Example 4
[0130] A slow setting method for original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.64% original shield slag, 4.79% water, 20.75% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.08% sodium gluconate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0131] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Methods for Standard Consistency Water Consumption, Setting Time and Stability of Cement". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in this comparative example 4 was 22h4min, and the 7d strength was 4.30MPa.
[0132] Comparative Example 5
[0133] A slow setting method for original shield slag unburned building materials, comprising the following raw materials in percentage by mass: 68.58% original shield slag, 4.79% water, 20.73% blast furnace slag, 2.39% quicklime, 1.91% sodium carbonate, 1.44% sodium silicate, and 0.16% sodium gluconate. The raw materials are mixed and stirred evenly, then put into a mold, and the setting time of the slurry is tested.
[0134] The initial setting time of the original shield slag slurry was tested with reference to GBT1346-2011 "Test Methods for Water Consistency, Setting Time and Stability of Cement Standard Consistency". After testing, the initial setting time of the original shield slag unburned building material slurry prepared in this comparative example 5 was 21h23min, and the 7d strength was 0.12MPa.
[0135] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The various technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the various technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
Claims
1. A method for retarding the setting of original shield slag unburned building materials, characterized in that: The raw materials of the fire-free building material contain a retarder; The fire-free building material comprises the following raw materials in percentage by mass: 55%-80% of original shield slag, 15%-40% of alkali-activated cementitious material, 1%-6% of water and 0%-1.5% of retarder; Wherein, the retarder content is greater than 0; the retarder is at least one of acrylate and polyaluminium chloride.
2. The slow setting method of original shield slag unburned building materials according to claim 1 is characterized in that: The acrylate is at least one of magnesium acrylate, sodium acrylate and calcium acrylate.
3. The slow setting method of original shield slag unburned building materials according to claim 1, characterized in that: The alkali-activated gelling material is composed of the following raw materials in percentage by mass: 65%-95% of gelling component and 5%-35% of alkali activator.
4. The slow setting method of original shield slag unburned building materials according to claim 3 is characterized in that: The fineness of the gelling component is above 200 meshes.
5. The slow setting method of original shield slag unburned building materials according to claim 3, characterized in that: The gelling component is at least one of blast furnace slag, fly ash, silica fume, natural volcanic ash and steel slag.
6. The slow setting method of original shield slag unburned building materials according to claim 3, characterized in that: The alkaline activator is at least one of quicklime, sodium carbonate, sodium silicate, sodium aluminate, sodium hydroxide and sodium sulfate.
7. The slow setting method of original shield slag unburned building materials according to claim 1, characterized in that: The original shield slag is shield slag that has not been pre-treated by dehydration, screening, crushing, etc.
8. The slow setting method of original shield slag unburned building materials according to claim 1, characterized in that: The retarder is in the form of solid particles or powder.
9. A kind of original shield slag unburned building material, characterized in that: The raw materials include the following components by mass percentage: Original shield slag 55%-80% Alkali activated gelling material 15%-40% Water 1%-6% Retarder 0%-1.5%; Among them, the retarder content is greater than 0; the retarder includes at least one of acrylate and polyaluminium chloride; and the raw material of the fire-free building material does not contain cement.