Green body of sanitary ceramic prepared from molybdenum tailings as well as preparation method and application of green body

Through the combination formula and ball milling of molybdenum tailings and other minerals, a sanitary ceramic blank with low water absorption rate and high strength is formed, which solves the problem of large resource and energy consumption in the existing technology, and realizes the low sintering temperature High-performance ceramic preparation.

CN119080485APending Publication Date: 2024-12-06HEBEI UNIV OF TECH

Patent Information

Application Number
CN202411224091.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sanitary ceramics consume a large resource and energy consumption, and high-quality mineral resources are scarce, making it difficult to achieve high strength and low water absorption rate ceramic products.

Method used

Molybdenum tailings are used as the main raw material, combined with minerals such as spherical soil, kaolin, illite clay, etc., and through reasonable formulation and ball milling treatment, the chemical composition and particle size distribution of the blank are regulated, the sintering temperature is reduced, and the formation is mainly composed of quartz and mullite. ceramic body.

Benefits of technology

A large amount of molybdenum tailings is consumed at a lower sintering temperature (1100-1150℃), reducing energy consumption, improving the strength and performance of ceramic blanks, reducing resource waste, and suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080485A_ABST
    Figure CN119080485A_ABST
Patent Text Reader

Abstract

The invention discloses a sanitary ceramic green body prepared from molybdenum tailings and a preparation method and application thereof. The green body is prepared from the following components with specific contents: SiO2, Al2O3, Fe2O3, TiO2, CaO, MgO, K2O, Na2O and other optional components; the green body is prepared from the following raw materials in specific content: ball clay, high-alumina chinastone, kaolin, illite clay, microcline, dolomite and molybdenum tailings. Results show that the sanitary ceramic green body with good performance can be obtained at a lower sintering temperature by adding the molybdenum tailings and regulating and controlling the components in the green body, the bending strength of the sanitary ceramic green body is improved, and a new way is provided for preparing the sanitary ceramic green body by utilizing the molybdenum tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sanitary ceramic production, and in particular relates to a green body of sanitary ceramic prepared by utilizing molybdenum tailings, and a preparation method and application thereof. Background Art

[0002] Mineral resources, as an important material basis for human life and production, play an important role in safeguarding social construction and development. However, resource issues have become the focus of global attention. Tailings generated in the process of mineral resource development are the main component of industrial solid waste. Its main mineral components include a series of gangue minerals such as quartz, feldspar, pyroxene and amphibole, and its chemical composition is mainly composed of oxides and silicates of elements such as iron, silicon and aluminum. According to the data of the "2022-2028 China Tailings Comprehensive Utilization Industry Competition Status and Development Prospects Planning Report", as of 2020, my country's tailings stockpile has reached about 23 billion tons, mainly including iron tailings, copper tailings and some non-ferrous metal tailings, and the accumulation volume has shown an increasing trend year by year. The large accumulation of tailings not only causes serious pollution to the environment, but also occupies a large amount of land resources. Therefore, it is urgent to take measures to comprehensively utilize tailings resources and improve resource utilization to reduce the pollution of tailings to the environment and achieve the goals of sustainable economic development and green development.

[0003] Sanitary ceramics are glazed ceramic products that use molybdenum tailings in bathrooms, kitchens, laboratories and other places, also known as sanitary ware. As a common daily necessity, sanitary ceramics have brought great convenience to people's lives and improved people's quality of life to a certain extent. At present, the sanitary ceramics manufacturing industry is an important field of resource consumption and energy consumption, and a large amount of high-quality clay and various minerals are required every year. According to data, from 2017 to 2019, my country's sanitary ceramics production remained between 230 million and 240 million pieces. The production process of sanitary ceramics consumes a lot of raw material resources, and high-quality mineral resources are becoming increasingly scarce. Raw materials such as Suzhou soil, Jiepai soil, Zhangcun soil, Datong soil, and Guangdong black mud commonly used by ceramic companies have been exhausted or are facing exhaustion. Therefore, using other resources (such as tailings, silt, etc.) to replace natural minerals to prepare sanitary ceramics has become a key research area.

[0004] The literature Recycling detoxified cement asbestos slates in the production of ceramic sanitary wares (Bernasconi A, Pellegrino L, Vergani F, et al. 2022, 49(2): 1836-1845.) uses cement asbestos slate (CAS) heat-treated in air at 1100°C as a secondary raw material in the production of sanitary ware, and uses deactivated cement asbestos powder (DCAP) alone to replace quartz or feldspar. When its dosage is 5wt%, the overall process performance of the prepared ceramics is equivalent to that of normal production, indicating that DCAP powder can be used to produce sanitary ware using molybdenum tailings, but its usage is only 5wt%.

[0005] The literature Mixed Alkali and Mixed Alkaline-Earth Effect in Ceramic Sanitaryware Bodies Incorporated with Blast Furnace Slag (Aydin T, Casin E. 2020, 12 (5): 2685-2702.) uses slag and spodumene to replace albite for the preparation of sanitary ceramics. The results show that the sanitary ceramics prepared with 15% blast furnace slag and 4% spodumene have the best performance, with dry strength increased by about 47% and bending strength increased by about 67%. The use of a higher ratio of the two will cause the sintered body to expand.

[0006] The literature Incorporation of quartzite waste in mixtures used to prepare sanitary ware (Medeiros P SSD, Lira HDL, Rodriguez MA, et al. 2019, 8 (2): 2148-2159.) uses quartzite waste to replace feldspar to prepare sanitary ceramics. The results show that when the quartzite doping amount is 15%, the sanitary ceramics have the best performance, with a Vickers hardness of 6.4 GPa and a rupture modulus of 44.9 MPa, which just meets the water absorption rate standard of sanitary ceramics.

[0007] Therefore, providing a strategy to utilize other cheap resources to achieve high-strength and low-water absorption sanitary ceramics is a technical problem that needs to be solved urgently. Summary of the invention

[0008] In view of the above problems existing in the prior art, the object of the present invention is to provide a green body for preparing sanitary ceramics using molybdenum tailings, and a preparation method and use thereof.

[0009] In order to achieve the following objectives, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a green body for preparing sanitary ceramics using molybdenum tailings, wherein the chemical composition of the green body comprises, by mass fraction:

[0011]

[0012] The raw materials for preparing the green body include mineral raw materials, which include, by mass fraction:

[0013]

[0014] In the green body of sanitary ceramics prepared by using molybdenum tailings provided by the present invention, the mass fraction of SiO2 is 59-63%, for example, it can be 59%, 59.5%, 60%, 60.5%, 61%, 62% or 63%.

[0015] The mass fraction of Al2O3 is 21-25%, for example, it can be 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24% or 25%, etc.

[0016] The mass fraction of Fe2O3 is 1.4-1.8%, for example, it can be 1.4%, 1.5%, 1.6%, 1.7% or 1.8%.

[0017] The mass fraction of TiO2 is 0.5-0.7%, for example, it can be 0.5%, 0.55%, 0.6%, 0.65% or 0.7%.

[0018] The mass fraction of CaO is 0-0.2%, for example, it can be 0%, 0.05%, 0.1%, 0.15% or 0.2%, etc. Wherein, the mass fraction of CaO being 0% means that no CaO is contained.

[0019] The mass fraction of MgO is 0-0.9%, for example, it can be 0%, 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8% or 0.9%, etc.

[0020] The mass fraction of K2O is 3.6-4%, for example, it can be 3.6%, 3.7%, 3.8%, 3.9% or 4%.

[0021] The mass fraction of Na2O is 0.9-1.3%, for example, it can be 0.9%, 0.95%, 1%, 1.05%, 1.1%, 1.15%, 1.2%, 1.25% or 1.3%, etc.

[0022] In the present invention, "optional other components" means that in addition to the components listed above, other components may be included, or the composition may only consist of the components listed above.

[0023] In the mineral raw material of the present invention, the mass fraction of ball soil is 0-15%, for example, it can be 0%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc. Among them, the mass fraction of ball soil of 0% means that no ball soil is contained.

[0024] The mass fraction of high alumina porcelain stone is 8-23%, for example, it can be 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22% or 23%, etc.

[0025] The mass fraction of kaolin is 0-15%, for example, it can be 0%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, etc. Among them, the mass fraction of kaolin of 0% means that no kaolin is contained.

[0026] The mass fraction of illite clay is 0-22%, for example, it can be 0%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21% or 22%, etc. Among them, the mass fraction of illite clay is 0% means that no illite clay is contained.

[0027] The mass fraction of microcline is 0-13%, for example, it can be 0%, 0.5%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12% or 13%, etc. Among them, the mass fraction of microcline is 0%, which means that no microcline is contained.

[0028] The mass fraction of dolomite is 0-2%, for example, it can be 0%, 0.1%, 0.3%, 0.5%, 0.7%, 0.8%, 1%, 1.2%, 1.3%, 1.5%, 1.7%, 1.8% or 2%.

[0029] The mass fraction of the molybdenum tailings is 15-25%, for example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, etc.

[0030] The present invention introduces molybdenum tailings into the mineral raw materials, and cooperates with other raw materials to adjust the type and content of each component in the green body. Among them, ball clay, kaolin and illite clay are plastic raw materials, which provide certain suspension and stability for the grouting mud; high-aluminum porcelain stone and molybdenum tailings respectively provide Al2O3 and SiO2 required for the ceramic green body; microcline has a good solvent effect, which improves the temperature control effect of the sanitary ceramic green body; a small amount of CaO and MgO provided by dolomite can weaken the adverse coloring effect of iron and titanium. In addition, the above-mentioned mineral raw materials can provide alkali metal oxide components such as K2O and Na2O, so that low water absorption and high strength sanitary ceramic green bodies can be prepared at a lower sintering temperature, thereby reducing the resource and energy consumption in the production process of sanitary ceramics. More critical: the main crystal phases of molybdenum tailings are quartz, microcline and albite, and the crystal phases are all silicate minerals, which can not only provide a large amount of quartz, but also some feldspar minerals can act as co-solvents to reduce the sintering temperature during the sintering process, providing conditions for preparing ceramic materials.

[0031] Traditional sanitary ceramics are SiO2-Al2O3-CaO-MgO-K2O-Na2O high temperature component systems, with a firing temperature between 1200-1250°C, forming a main skeleton with mullite and quartz as the main and secondary crystal phases. The present invention uses the characteristics of molybdenum tailings with high silicon and containing some feldspar minerals to design a reasonable formula based on the traditional formula, which can consume a large amount of molybdenum tailings, and obtain a sanitary ceramic body with quartz and mullite as the main crystal phases at a lower proportion of natural minerals and a lower sintering temperature (for example, 1100-1150°C), thereby reducing energy consumption and improving product performance.

[0032] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0033] Preferably, the chemical composition of the molybdenum tailings comprises, by mass fraction:

[0034]

[0035] In this technical solution, the mass fraction of SiO2 is 72.6-74.6%, for example, it can be 72.6%, 72.7%, 72.8%, 73.0%, 73.2%, 72.4%, 72.6%, 72.8%, 73.0%, 73.5%, 74.0% or 74.5%, etc.

[0036] The mass fraction of Al2O3 is 12.5-13.43%, for example, it can be 12.5%, 12.6%, 12.7%, 12.8%, 13.0%, 13.2%, 13.3% or 13.4%, etc.

[0037] The mass fraction of Fe2O3 is 1.86-2.39%, for example, it can be 1.86%, 1.87%, 1.88%, 1.89%, 1.90%, 1.93%, 1.95%, 1.97%, 2.00%, 2.03%, 2.05%, 2.08%, 2.10%, 2.15%, 2.20%, 2.25%, 2.30%, 2.32%, 2.34%, 2.36%, 2.38% or 2.39%, etc.

[0038] The mass fraction of TiO2 is 0.2-0.45%, for example, it can be 0.2%, 0.25%, 0.3%, 0.35%, 0.4% or 0.45%.

[0039] The mass fraction of CaO is 0.8-1.22%, for example, it can be 0.8%, 0.85%, 0.9%, 0.95%, 1.00%, 1.05%, 1.10%, 1.15%, 1.20% or 1.22%.

[0040] The mass fraction of MgO is 0.28-0.34%, for example, it can be 0.28%, 0.29%, 0.30%, 0.31%, 0.32%, 0.33% or 0.34%.

[0041] The mass fraction of K2O is 5.71-5.90%, for example, it can be 5.71%, 5.72%, 5.73%, 5.75%, 5.80%, 5.85% or 5.90, etc.

[0042] The mass fraction of Na2O is 2.26-2.64%, for example, it can be 2.26%, 2.28%, 2.30%, 2.35%, 2.38%, 2.40%, 2.45%, 2.50%, 2.55% or 2.60%, etc.

[0043] As a preferred technical solution for preparing a sanitary ceramic body using molybdenum tailings as described in the present invention, based on the total mass of the mineral raw materials as 100%, the total mass percentage of the molybdenum tailings and the high-aluminum porcelain stone is controlled at 30-35%, for example, it can be 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5% or 35%, etc.

[0044] Preferably, in the chemical composition of the green body, the total mass proportion of SiO2 and Al2O3 is 83-85%, for example, it can be 83%, 83.5%, 84%, 84.5% or 85%.

[0045] Preferably, in the chemical composition of the green body, the molar ratio of SiO2 to Al2O3 is (4-5):1, for example, it can be 4:1, 4.2:1, 4.3:1, 4.5:1, 4.7:1 or 5:1, etc.

[0046] Preferably, in the chemical composition of the blank, the total mass proportion of K2O and Na2O is 3-5%, for example, it can be 3%, 3.5%, 4%, 4.5% or 5%.

[0047] In a second aspect, the present invention provides a method for preparing the green body according to the first aspect, the method comprising the following steps:

[0048] (1) Mixing the mineral raw materials with water, water glass and alkali, ball milling and sieving to obtain slurry;

[0049] (2) The slurry is injected into a mold for molding, and then dried after demoulding to obtain the green body.

[0050] In the method of the present invention, powder with uniform particle size distribution can be obtained by ball milling, which is conducive to making the slurry particle size distribution more uniform and concentrated in a small particle size range, which is conducive to reducing the activation energy of the sintering reaction.

[0051] In the method of the present invention, by using water glass and alkali to assist ball milling, D50 and D90 can be significantly reduced, which can significantly reduce the sintering activation energy of the green body, and a small amount of flux can achieve full vitrification sintering; at the same time, the formation of local low-viscosity areas by strong flux elements Na and K is suppressed, the uniform distribution of grains in the liquid phase is promoted, the shear viscosity of the melt suspension is increased, and it is beneficial to reduce the deformation of the green body.

[0052] Preferably, in step (1), the rotation speed of the ball mill is 600-1000 r / min, for example, it can be 600 r / min, 700 r / min, 750 r / min, 800 r / min, 850 r / min, 900 r / min, 950 r / min or 1000 r / min, etc.; the ball milling time is 0.5-2 h, for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 1 h, 1.2 h, 1.4 h, 1.5 h, 1.6 h, 1.8 h or 2 h, etc.

[0053] Preferably, during the ball milling process of step (1), the ratio of material to grinding ball is 1:(1.5-3) by mass, for example, it can be 1:1.5, 1:1.7, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8 or 1:3, etc.; the amount of water added is 40-60% of the mass of all materials, for example, it can be 40%, 42%, 44%, 45%, 46%, 48%, 50%, 52%, 55%, 57%, 58% or 60%, etc.

[0054] Preferably, in step (1), the amount of water glass added is 0.5-1.5% of the total raw material mass, for example, it can be 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.3%, 1.4% or 1.5%, etc.

[0055] Preferably, in step (1), the amount of alkali added is 0.3-0.5% by mass of the total raw materials, for example, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%.

[0056] Preferably, the alkali in step (1) is sodium carbonate.

[0057] Preferably, the particle size D50 of the mud in step (1) is less than 10μm, for example, it can be 9.5μm, 9μm, 8.5μm, 8μm, 7.5μm, 7μm, 6.5μm, 6μm, 5.5μm, 5μm, 4.5μm, 4μm, 3.5μm, 3μm, 2.5μm, 2μm, 1.5μm, 1μm or 0.5μm, etc.

[0058] Preferably, the mesh size of the sieve used in step (1) is 70-90 mesh, for example, it can be 70 mesh, 80 mesh or 90 mesh.

[0059] Preferably, before injecting the slurry into the mold in step (2), water glass is used to adjust the concentration, viscosity and thickening coefficient of the slurry. The concentration is 170-180 g / 100 mL, for example, 170 g / 100 mL, 172 g / 100 mL, 175 g / 100 mL, 177 g / 100 mL, 178 g / 100 mL or 180 g / 100 mL; the viscosity is 400-600 mP a·s, for example, it can be 400mPa·s, 420mPa·s, 450mPa·s, 460mPa·s, 480mPa·s, 500mPa·s, 525mPa·s, 550mPa·s, 560mPa·s, 580mPa·s or 600mPa·s, etc.; the thickening coefficient is 1.5-2.0, for example, it can be 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0, etc.

[0060] Preferably, the drying in step (2) is: first drying at room temperature for 10-14 h (for example, it can be 10 h, 11 h, 12 h, 13 h or 14 h, etc.), and then drying in an oven for 10-14 h (for example, it can be 10 h, 11 h, 12 h, 13 h or 14 h, etc.), wherein the temperature of the oven is 60-80 ° C (for example, it can be 60 ° C, 62 ° C, 65 ° C, 68 ° C, 70 ° C, 75 ° C or 80 ° C, etc.).

[0061] Preferably, the mineral raw material in step (1) is crushed into powder before use.

[0062] Preferably, the molybdenum tailings in the mineral raw material are crushed in the following manner: the molybdenum tailings are ball-milled at a rotation speed of 1000-1200r / min (for example, 1000r / min, 1050r / min, 1100r / min, 1150r / min or 1200r / min, etc.) for 2-3h (for example, 2h, 2.2h, 2.5h, 2.7h or 3h, etc.) and passed through a 180-200 mesh sieve to obtain molybdenum tailings powder.

[0063] Preferably, the particle size of the molybdenum tailings powder is D10≤1.5μm, D50≤7.0μm, and D90≤23.0μm. For example, D10 may be 1.5μm, 1.4μm, 1.3μm, 1.2μm, 1.1μm, 1.0μm, 0.8μm, 0.5μm or 0.3μm, etc.; D50 may be 7.0μm, 6.5μm, 6.0μm, 5.5μm, 5.0μm, 4.5μm, 4.0μm, 3.0μm or 2.0μm. etc.; D90 can be, for example, 23.0μm, 22.0μm, 21.0μm, 20.0μm, 19.0μm, 18.0μm, 16.0μm, 15.0μm, 14.0μm, 12.0μm, 10.0μm, 9.0μm, 8.5μm, 8.0μm, 7.5μm, 7.0μm, 6.0μm or 5.0μm, etc.

[0064] In a third aspect, the present invention provides a sanitary ceramic blank, which is obtained by sintering the blank described in the first aspect, and the sanitary ceramic blank includes quartz and mullite.

[0065] In a fourth aspect, the present invention provides a method for preparing the sanitary ceramic body as described in the third aspect, comprising the following steps:

[0066] The green body described in the first aspect is sintered to obtain the sanitary ceramic green body.

[0067] Preferably, the burn-out rate of the green body in the sintering step is 7-8%, for example, it may be 7%, 7.2%, 7.3%, 7.5%, 7.7%, 7.8% or 8%.

[0068] Preferably, the sintering is normal pressure sintering.

[0069] The present invention does not specifically limit the equipment used for atmospheric pressure sintering, and it may be a muffle furnace, for example.

[0070] Preferably, the sintering comprises: heating to a maximum sintering temperature and maintaining the temperature.

[0071] Preferably, the maximum temperature is 1050-1200°C, for example, it may be 1050°C, 1070°C, 1080°C, 1090°C, 1100°C, 1120°C, 1130°C, 1150°C, 1170°C or 1200°C, etc.

[0072] Preferably, the insulation time is 1-3h, for example, it can be 1h, 1.2h, 1.3h, 1.4h, 1.5h, 1.7h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h.

[0073] Preferably, the process of heating to the maximum sintering temperature is: heating to 900°C at a rate of 5-8°C / min (for example, 5°C / min, 5.5°C / min, 6°C / min, 6.5°C / min, 7°C / min, 7.5°C / min or 8°C / min, etc.), and then heating to the maximum sintering temperature at a rate of 1-3°C / min (for example, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min or 3°C / min, etc.).

[0074] Preferably, a cooling process is performed after the heat preservation, specifically, cooling to room temperature along with the furnace.

[0075] In the present invention, room temperature refers to 20-25°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C or 25°C.

[0076] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0077] Compared with the prior art, the present invention has the following beneficial effects:

[0078] The present invention utilizes the characteristics of molybdenum tailings that are high in silicon and contain some feldspar minerals to design a reasonable formula on the basis of the traditional formula. It can consume a large amount of molybdenum tailings and obtain a sanitary ceramic body with quartz and mullite as the main crystal phases at a lower proportion of natural minerals and a lower sintering temperature (for example, 1100-1150°C), thereby reducing energy consumption and improving product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0079] Figure 1 This is the XRD pattern of molybdenum tailings after ball milling;

[0080] Figure 2 The following are the actual photos and microscopic morphology of molybdenum tailings after ball milling treatment;

[0081] Figure 3To measure the particle size distribution of molybdenum tailings after ball milling;

[0082] Figure 4 The slurry particle size distribution diagrams of Comparative Example 1-1, Example 1-1, Example 2-1 and Example 3-1, wherein (a) corresponds to Comparative Example 1-1, (b) corresponds to Example 1-1, (c) corresponds to Example 2-1, and (d) corresponds to Example 3-1;

[0083] Figure 5 XRD patterns of ceramic bodies of different samples at different sintering temperatures, where (a) corresponds to comparative examples 1-2 to 1-4, (b) corresponds to examples 1-1 to 1-4, (c) corresponds to examples 2-1 to 2-4, and (d) corresponds to examples 3-1 to 3-4. DETAILED DESCRIPTION

[0084] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0085] The specific embodiments described herein only use molybdenum tailings to explain the present invention, and do not use molybdenum tailings to limit the present invention.

[0086] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiments of the present invention:

[0087] The chemical compositions of the raw materials used in the present invention and the comparative examples are shown in Table 1.

[0088] Table 1 Chemical composition of raw materials

[0089]

[0090] Note: "LOI" stands for loss on ignition.

[0091] The test methods used in the embodiments of the present invention and the comparative examples are as follows:

[0092] Particle size test: Laser particle size analyzer, model Mastersizer 2000, dispersant is deionized water. Particle size value is expressed as D50.

[0093] Water absorption test: The water absorption of ceramic samples was tested using an electronic balance in accordance with ASTM C373-88 (2006).

[0094] Viscosity test: NDJ-5S digital viscometer was used for the test. The test conditions were: No. 2 rotor, speed of 30 r / min.

[0095] Fluidity test: Stir the slurry thoroughly and pour it into the coating cup. After it is left to stand for 30 seconds, open the outlet hole at the bottom and press the stopwatch at the same time. When the liquid column is obviously interrupted for the first time, stop the timing and record t 30s , unit is s.

[0096] Thixotropy test: In the production process, the thickening coefficient is generally used to indicate the thixotropy of the mud. After the mud is fully stirred and evenly mixed, pour it into the coating cup and let it stand for 30 minutes. Then open the outlet hole at the bottom and press the stopwatch at the same time until the liquid column is obviously interrupted for the first time. Then stop the timing and record t 30min , the unit is s. Then the mud thickening coefficient is t 30min / t 30s .

[0097] Drying shrinkage test: By measuring the length N0 of the ceramic test strip before drying and the length N after drying, the unit is mm, and the drying shrinkage rate can be calculated using the following formula: G = (N0-N) / N0×100%. In the formula, G is the drying shrinkage rate of the test strip; N0 is the length of the test strip before drying; N is the length of the test strip after drying.

[0098] Sintering shrinkage test: By measuring the length L0 of the ceramic test strip before sintering and the length L after sintering, the unit is mm, and the linear shrinkage can be calculated using the following formula: λ = (L0-L) / L0×100%. In the formula, λ is the linear shrinkage of the test strip; L0 is the length of the test strip before sintering; L is the length of the test strip after sintering.

[0099] Bulk density test: MDJ-120TEMS solid-liquid-powder integrated density meter is used for testing.

[0100] Bending strength test: The flexural strength test of the sintered ceramic samples was carried out on a Shenzhen Xinsansi CMT-6140 universal testing machine using the three-point bending method in accordance with the GB / T6569-2006 standard.

[0101] Phase composition XRD analysis: Japan Smartlab 9KW X-ray powder diffractometer.

[0102] In the embodiment 1-1 of the present invention, the "others" in the chemical composition of the green body are not listed one by one, because they are mainly trace metal oxides and have no effect on the performance of the green body, so they are not repeated.

[0103] Example 1-1

[0104] A green body for preparing sanitary ceramics using molybdenum tailings, wherein the chemical composition of the green body comprises, by mass fraction:

[0105] 59.49% SiO2, 24.41% Al2O3, 1.68% Fe2O3, 0.69% TiO2, 1.09% CaO, 0.83% MgO, 3.89% K2O, 1.02% Na2O, 6.9% others, among which the total mass proportion of SiO2 and Al2O3 is 83.90%, the SiO2 / Al2O3 molar ratio is 4.14, and the total mass proportion of K2O and Na2O is 4.91%.

[0106] The raw materials for preparing the green body include mineral raw materials, which include, by mass fraction, 15% ball clay, 18% high-alumina porcelain stone, 15% kaolin, 22% illite clay, 13% microcline, 2% dolomite, and 15% molybdenum tailings powder.

[0107] The green body provided in this embodiment has a ignition loss of 7.79% during the sintering process.

[0108] This embodiment also provides a method for preparing the above-mentioned green body, comprising the following steps:

[0109] (1) preparing sanitary ceramic raw materials: crushing and drying natural minerals (ball clay, high-alumina porcelain stone, kaolin, illite clay, microcline and dolomite) to obtain natural mineral powders;

[0110] The molybdenum tailings were ball milled at a speed of 1200 r / min for 2 h and passed through a 200-mesh sieve to obtain molybdenum tailings powder. The actual photos and microscopic morphology are shown in Figure 2 , where the left side is a real photo and the right side is a microscopic morphology diagram. Figure 2 It can be seen that its appearance is light green, and from a microscopic perspective it is composed of many irregular blocks with small particles attached to the blocks.

[0111] (2) adding natural mineral powder, molybdenum tailings powder, water, water glass and alkaline noodles into a ball mill according to the formula ratio, and ball milling with zirconium oxide balls;

[0112] The ball milling speed is 800 r / min, the time is 1 h, the amount of water glass added is 1.0% of the total raw material mass, the amount of alkaline noodles added is 0.4% of the total raw material mass, and the amount of water added is 50% of the total raw material mass.

[0113] (3) Release the mill, pass through an 80-mesh sieve, and adjust the mud viscosity by adding water glass to control the mud concentration at 175 g / 100 ml, the mud viscosity at 500 mPa·s, the mud particle size D50 < 10 μm, and the thickening coefficient at 1.7.

[0114] (4) The slurry is injected into a plaster mold for molding. After demoulding, it is first placed at room temperature to dry for 12 hours, and then placed in an oven for 12 hours to obtain a green body.

[0115] This embodiment also provides a sanitary ceramic body prepared using the above-mentioned body, and the preparation method thereof comprises the following steps:

[0116] The green body was placed in a muffle furnace, heated to 900°C at a rate of 5°C / min, and continued to be heated to a maximum sintering temperature of 1050°C at a rate of 3°C / min, kept at this temperature for 2 hours, and then cooled to room temperature with the furnace to obtain a sanitary ceramic green body, the contents of quartz and mullite of which are shown in Table 2.

[0117] Example 1-2

[0118] The difference between this embodiment and embodiment 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1100°C.

[0119] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0120] Examples 1-3

[0121] The difference between this embodiment and embodiment 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1150°C.

[0122] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0123] Examples 1-4

[0124] The difference between this embodiment and embodiment 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1200°C.

[0125] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0126] Example 2-1

[0127] The differences in the chemical composition of the blank and the composition of the mineral raw materials between this embodiment and embodiment 1-1 are shown in Table 3.

[0128] The green body provided in this embodiment has a ignition loss of 7.80% during the sintering process.

[0129] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0130] Example 2-2

[0131] The difference between this embodiment and embodiment 2-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1100°C.

[0132] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0133] Example 2-3

[0134] The difference between this embodiment and embodiment 2-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1150°C.

[0135] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0136] Embodiment 2-4

[0137] The difference between this embodiment and embodiment 2-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1200°C.

[0138] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0139] Example 3-1

[0140] The differences in the chemical composition of the blanks and the composition of the mineral raw materials between this embodiment and embodiment 1-1 are shown in Tables 1 and 2.

[0141] The green body provided in this embodiment has a ignition loss of 7.80% during the sintering process.

[0142] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0143] Example 3-2

[0144] The difference between this embodiment and embodiment 3-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1100°C.

[0145] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0146] Example 3-3

[0147] The difference between this embodiment and embodiment 3-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1150°C.

[0148] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0149] Embodiment 3-4

[0150] The difference between this embodiment and embodiment 3-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1200°C.

[0151] The contents of quartz and mullite in the sanitary ceramic body prepared in this example are shown in Table 2.

[0152] Comparative Example 1-1

[0153] The differences in the chemical composition of the blanks of this comparative example and Example 1-1 and the composition of the mineral raw materials are shown in Tables 1 and 2.

[0154] The contents of quartz and mullite in the sanitary ceramic body prepared in this comparative example are shown in Table 2.

[0155] Comparative Example 1-2

[0156] The difference between this comparative example and Example 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1100°C.

[0157] The contents of quartz and mullite in the sanitary ceramic body prepared in this comparative example are shown in Table 2.

[0158] Comparative Examples 1-3

[0159] The difference between this comparative example and Example 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1150°C.

[0160] The contents of quartz and mullite in the sanitary ceramic body prepared in this comparative example are shown in Table 2.

[0161] Comparative Examples 1-4

[0162] The difference between this comparative example and Example 1-1 is that the maximum sintering temperature when preparing the sanitary ceramic body is 1200°C.

[0163] The contents of quartz and mullite in the sanitary ceramic body prepared in this comparative example are shown in Table 2.

[0164] Table 2

[0165]

[0166]

[0167] Table 3

[0168]

[0169] Table 4

[0170]

[0171] The performance of each embodiment and comparative example was tested. The comparison of mud performance is shown in Table 5, and the performance of the sanitary ceramic body is shown in Table 6.

[0172] Table 5

[0173]

[0174]

[0175] Table 6

[0176]

[0177] Through various analyses, it can be known that the molybdenum tailings dosage of the present invention can reach 15-25%, which can realize the resource recycling of tailings, reduce solid waste environmental pollution, save high-quality mineral resources, reduce enterprise production costs, and promote the vigorous development of the industry's circular economy. At the same time, the bending strength of each embodiment at the optimal sintering temperature is increased by more than 40% compared with the current level (comparative example), and the production process is simple, without adding new equipment, and can be realized on the basis of the original grinding equipment, which is suitable for industrial large-scale production.

[0178] Combined with the chemical composition of molybdenum tailings in Table 1 and the Figure 1 It can be seen that the main crystal phases of molybdenum tailings are quartz [SiO2, PDF#99-0088], microcline [KAlSi3O8, PDF#19-0932], and albite [Na(AlSi3O8), PDF#80-1094]. The crystal phases in the tailings are all silicate minerals, which can not only provide a large amount of quartz, but also some feldspar minerals can act as co-solvents in the sintering process to reduce the sintering temperature, providing conditions for the preparation of ceramic materials.

[0179] The surface and microstructure of molybdenum tailings after ball milling Figure 2 As shown in the figure, its appearance is light green, and from a microscopic point of view, it is composed of many irregular blocks with small particles attached to the blocks. The particle size distribution of the tailings after ball milling for 2 hours is shown in the attached figure. Figure 3 As shown, D10, D50, and D90 are 1.25 μm, 6.62 μm, and 22.43 μm, respectively.

[0180] The particle size distribution of the slurry in Comparative Example 1-1, Example 1-1, Example 2-1 and Example 3-1 is shown in the attached figure. Figure 4As shown, (a) corresponds to comparative example 1-1, (b) corresponds to example 1-1, (c) corresponds to example 2-1, and (d) corresponds to example 3-1. The particle size of the conventional sanitary ceramic body slurry of comparative example 1-1 is D10=1.41μm, D50=9.19μm, and D90=50.27μm, while the particle size of the molybdenum tailings slurry sample of example 1-1 is D10=1.45μm, D50=6. 9μm, D90=21.53μm, the particle size of the molybdenum tailings slurry sample of Example 2-1 is D10=1.45μm, D50=7.05μm, D90=22.01μm, and the particle size of the molybdenum tailings slurry sample of Example 3-1 is D10=1.4μm, D50=6.98μm, D90=21.81μm. It can be seen that the particle size distribution of the slurry sample is uniform, and D50 is less than 10μm. In general, the particle size D10 of the fine particles of the embodiment is close to that of the comparative example, while the median particle size D50 and the large particle D90 are significantly smaller than the comparative example, which significantly reduces the sintering activation energy of the embodiment blank, and a small amount of flux can achieve full vitrification sintering; at the same time, it inhibits the formation of local low viscosity areas of strong flux Na and K elements, promotes the uniform distribution of grains in the liquid phase, and increases the shear viscosity of the melt suspension, which is beneficial to reduce the deformation of the blank.

[0181] It can be seen from Table 5 that after adding water glass to adjust the performance of the mud discharged from the mill once, the performance parameters of Example 1-1, Example 2-1 and Example 3-1 reach the required range for grouting. At the same time, compared with the comparative example, the drying shrinkage of the example is slightly larger.

[0182] Combined with Table 6, the maximum sintering temperature of Example 1-1 to Example 1-4 changes from low to high, the maximum sintering temperature of Example 2-1 to Example 2-4 changes from low to high, and the maximum sintering temperature of Example 3-1 to Example 3-4 changes from low to high. The results show that the sintering shrinkage, bulk density and flexural strength show a trend of first increasing and then decreasing with the increase of temperature. This is because the addition of molybdenum tailings increases the content of K2O and Na2O in the ceramic body, the fluxing effect is better, and the ceramic sintering temperature is reduced. Overburning occurs at 1200°C and its flexural strength decreases. Compared with Comparative Example 1, which can only obtain a body with good performance at 1200°C, the chemical composition of Example 1-1, Example 2-1 and Example 3-1 and the composition of mineral raw materials can obtain a ceramic body with good performance and water absorption rate that meets the standard at 1150°C, 1100°C, and 1100°C, respectively, and its flexural strength is increased by 57%, 59%, and 58%, respectively.

[0183] Combined with Table 2 and Appendix Figure 5It can be seen that the sintering reaction of the embodiment is roughly the same as that of the comparative example: some microcline exists at 1050°C, and only a small amount of mullite crystal phase is generated. However, as the temperature gradually increases, the microcline gradually decomposes and disappears, the quartz content decreases, and the diffraction peak intensity gradually decreases, mainly because it begins to combine with the alumina in the blank to form a mullite crystal phase, which leads to a gradual increase in the content of the mullite crystal phase. However, the mullite crystal phase content of Example 3-4 decreases at 1200°C mainly because n(SiO2) / n(Al2O3) is too high, so that there is not too much Al2O3 in the blank to combine with SiO2 to form mullite.

[0184] The applicant declares that the present invention illustrates the detailed method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed method, that is, it does not mean that the present invention must rely on the above-mentioned detailed method to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A green body for preparing sanitary ceramics using molybdenum tailings, characterized in that: The chemical composition of the green body includes, by mass fraction: The raw materials for preparing the green body include mineral raw materials, which include, by mass fraction:

2. The method for preparing a green body of sanitary ceramics using molybdenum tailings according to claim 1, wherein: The chemical composition of the molybdenum tailings includes, by mass fraction:

3. The method for preparing a green body of sanitary ceramics using molybdenum tailings according to claim 1 or 2, characterized in that: Taking the total mass of the mineral raw materials as 100%, the total mass percentage of the molybdenum tailings and the high-aluminum porcelain stone is controlled at 30-35%; Preferably, in the chemical composition of the green body, the total mass proportion of SiO2 and Al2O3 is 83-85%; Preferably, in the chemical composition of the green body, the molar ratio of SiO2 to Al2O3 is (4-5):1; Preferably, in the chemical composition of the green body, the total mass proportion of K2O and Na2O is 3-5%.

4. A method for preparing a green body according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) Mixing the mineral raw materials with water, water glass and alkali, ball milling and sieving to obtain mud; (2) injecting the slurry into a mold for molding, demolding and drying to obtain the green body.

5. The preparation method according to claim 4, characterized in that: In step (1), the rotation speed of the ball mill is 600-1000 r / min, and the time of the ball mill is 0.5-2 h; Preferably, during the ball milling process of step (1), the ratio of material to grinding ball is 1:(1.5-3) by mass; the amount of water added is 40-60% of the mass of the total material; Preferably, in step (1), the amount of water glass added is 0.5-1.5% of the total raw material mass; Preferably, in step (1), the amount of alkali added is 0.3-0.5% by weight of the total raw materials; Preferably, the base in step (1) is alkaline noodles; Preferably, the particle size D50 of the slurry in step (1) is less than 10 μm; Preferably, the mesh size of the sieve used in step (1) is 70-90 mesh.

6. The preparation method according to claim 4 or 5, characterized in that: Step (2) Before injecting the slurry into the mold, water glass is used to adjust the concentration, viscosity and thickening coefficient of the slurry, wherein the concentration is 170-180 g / 100 mL, the viscosity is 400-600 mPa·s, and the thickening coefficient is 1.5-2.0; Preferably, the drying in step (2) is: first drying at room temperature for 10-14 hours, and then drying in an oven for 10-14 hours, wherein the temperature of the oven is 60-80°C.

7. The preparation method according to any one of claims 4 to 6, characterized in that: The mineral raw material in step (1) is crushed into powder before use; Preferably, the molybdenum tailings in the mineral raw material are crushed in the following manner: the molybdenum tailings are ball-milled at a rotation speed of 1000-1200 r / min for 2-3 hours and passed through a 180-200 mesh sieve to obtain molybdenum tailings powder; Preferably, the particle size of the molybdenum tailings powder is D10≤1.5 μm, D50≤7.0 μm, and D90≤23.0 μm.

8. A sanitary ceramic body, characterized in that: The sanitary ceramic blank is obtained by sintering the blank according to any one of claims 1 to 3, and the sanitary ceramic blank comprises quartz and mullite.

9. A method for preparing a sanitary ceramic body as claimed in claim 8, characterized in that: The following steps are involved: The green body described in any one of claims 1 to 4 is sintered to obtain the sanitary ceramic green body.

10. The method for preparing a sanitary ceramic body according to claim 9, characterized in that: The burn-out rate of the green body in the sintering step is 7-8%; Preferably, the sintering is atmospheric pressure sintering; Preferably, the sintering comprises: heating to a maximum sintering temperature and maintaining the temperature; Preferably, the maximum temperature is 1050-1200°C; Preferably, the insulation time is 1-3h; Preferably, the process of heating to the maximum sintering temperature is: heating to 900° C. at a rate of 5-8° C. / min, and then heating to the maximum sintering temperature at a rate of 1-3° C. / min.

Citation Information

Patent Citations

  • High-temperature-resistant material and preparation method thereof

    CN110818396A

  • Low-temperature sintered sanitary ceramic green body and preparation method thereof

    CN113929437A

  • Method for preparing high-strength ceramic body at low temperature by doping molybdenum slag and rubidium tailings and product thereof

    CN117550875A

  • Tailing compounded cordierite-based far infrared emission ceramic as well as preparation method and application thereof

    CN117886588A

  • Process for manufacturing pellets from tailings for use in engineering applications

    WO2023122839A1

Cited By

  • Ceramic fluorescent nanocrystalline composite particle and preparation method thereof

    CN120059742A