Blast furnace iron runner skimmer suitable for oscillating sintering and preparation method of blast furnace iron runner skimmer

By using the synergistic effect of submicron SiO2 micropowder and boron oxide powder in the iron groove skimmer, a high-strength boron doped mullite network structure is formed, which solves the problems of excessive rigidity of traditional cement bonds and low particle rearrangement efficiency. High temperature performance improvement and volume stability are achieved, extending service life and reducing maintenance costs.

CN119080516AActive Publication Date: 2024-12-06WUHAN METALLURGY ARCHITECTURE RES YUAN CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411188309.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

The castable material of traditional iron groove skimmers is too rigid because of the excessive rigidity of the cement combination, which makes it difficult to adapt to the oscillation sintering process. The lack of liquefaction conditions at medium and low temperatures leads to low particle rearrangement efficiency, resulting in easy material damage and short service life.

Method used

Submicron SiO2 micropowder and boron oxide powder are used as bonding agents to form a high-strength/high-even-to-diameter boron-doped mullite network structure through oscillation sintering process, optimize the particle rearrangement and densification process, and improve high-temperature performance.

Benefits of technology

It improves the high-temperature performance and volume stability of the iron groove skimmer, extends the service life, reduces the overall operation and maintenance costs, and increases the amount of iron throughput at one time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014208190000061
    Figure BDA0005014208190000061
Patent Text Reader

Abstract

The invention discloses a blast furnace iron runner skimmer suitable for oscillating sintering. The blast furnace iron runner skimmer comprises the following raw materials in percentage by mass: 18-25% of brown fused alumina aggregate with the particle size of 5-8mm; 18%-25% of brown fused alumina aggregate with the particle size of 3-5 mm; 10%-18% of brown fused alumina particles with the particle size of 1-3 mm; 8%-15% of compact corundum particles with the particle size of 0.074-1 mm; 5-9% of dense corundum fine powder with the particle size of less than or equal to 0.074 mm; 6%-12% of silicon carbide particles with the particle size of 0.074-1 mm; 6-12% of silicon carbide fine powder with a particle size of less than or equal to 0.074 mm; 0.5%-3% of spherical asphalt with the particle size of 0.1-0.8 mm; 3%-6% of submicron SiO2 micro powder with the particle size being smaller than or equal to 0.020 mm; 2%-7% of alpha-Al2O3 micro powder with the particle size of less than or equal to 0.020 0.5%-1.0% of boron oxide powder with the particle size being smaller than or equal to 0.044 mm; by redesigning the formula, the raw materials of the blast furnace iron runner skimmer are well matched with oscillation sintering, and the obtained product is good in high-temperature performance, high in volume stability, excellent in erosion resistance, long in service life and low in comprehensive operation and maintenance cost and has remarkable economic and social benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory materials, and in particular relates to a blast furnace iron ditch slag skimmer and a preparation method thereof. Background Art

[0002] The iron ditch skimmer is an important part of the blast furnace iron ditch. It is located at the tail end of the main ditch of the iron ditch, connecting the main iron ditch, branch iron ditch and slag ditch in the horizontal flow area. It is the key part for separating slag and iron during iron tapping. The iron ditch skimmer separates slag and iron based on the principle of slag and iron density difference. Therefore, it needs to withstand chemical erosion and physical erosion of high-temperature slag and molten iron. The damage of the skimmer is common in its lower half and is often faster than other parts of the main ditch. The asynchronous life of the refractory material of the skimmer and the main ditch leads to premature offline, which is bound to cause waste of refractory materials and unstable and discontinuous steel production. The service condition of the iron ditch skimmer determines the overall service life of the iron ditch and the stable and efficient operation of the steel industry.

[0003] CN 202010463673.6 discloses a silicon nitride combined castable and a blast furnace slag skimmer for a blast furnace. The technical solution is to introduce silicon nitride powder on the basis of high-purity raw materials to enhance the density of the castable, thereby improving its oxidation resistance and slag resistance. However, since silicon nitride has good chemical stability at high temperatures, it is difficult to sinter it as a whole, which is not conducive to the improvement of high-temperature service performance. In addition, the cordierite introduced in the raw materials will decompose at the service temperature of the slag skimmer, which will cause the high-temperature service performance of the castable to further decrease.

[0004] CN 202311633692.9 discloses a castable for a slag skimmer at an iron outlet ditch. The technical solution is to modify the Al2O3-SiC-C castable by chromium oxide green and spinel, and use a transmission assembly to realize remote disassembly and maintenance of the skimmer; but since it still uses cement as a binder, the strength of the material at high temperatures cannot be effectively improved, and the problem of the skimmer being easily damaged is not fundamentally solved. In addition, due to the introduction of chromium oxide green, toxic hexavalent chromium may be formed under high-temperature oxidation conditions, which also limits its use conditions.

[0005] CN 202010205168.1 discloses a method for online repair of a slag skimmer, and the technical scheme repairs the damaged parts of the iron ditch slag skimmer by spraying; however, it requires complex operations such as lowering the molten iron level and laying an insulation layer, and requires maintenance for more than 1 hour. It has many restrictive conditions, which not only fails to fundamentally improve the service performance of the slag skimmer, but also affects normal production operations.

[0006] Oscillating hot pressing sintering is a new type of dynamic pressure sintering technology, that is, a clamping pressure with a certain frequency and amplitude is applied during the sintering process, which is conducive to solving the defects of low density and cracks in the traditional sintering process, and can be applied to the preparation of oxide / non-oxide ceramics and high-temperature alloys. In the early stage of oscillating sintering, the clamping pressure can promote particle sliding, deflection and rearrangement, and eliminate agglomeration; in the later stage of sintering, the clamping pressure can provide a greater sintering driving force, stimulate grain boundary sliding and plastic deformation, and more effectively promote the merging and discharge of residual closed pores at the grain boundary.

[0007] At present, the castables of iron ditch skimmers are all cement-bonded, and the CA6 structure formed after hydration makes the compressive strength of the material greater than 40MPa after hardening. If the traditional cement-bonded castables are used to prepare prefabricated parts, the rigidity of the prefabricated parts is too large, and the internal microcracks are easily extended during the oscillation pressure process, destroying the original structure; and because the high-purity raw materials used have no liquid phase under low temperature conditions, the particle rearrangement efficiency is low, or even no particle rearrangement. Therefore, traditional cement-bonded castables are difficult to adapt to the oscillation sintering process. Summary of the invention

[0008] The traditional iron ditch skimmer uses cement for bonding, which has the problem of excessive rigidity. At the same time, the lack of liquefaction conditions at medium and low temperatures leads to the obstruction of particle rearrangement, which makes the preparation of the traditional iron ditch skimmer unable to be well adapted to the oscillation sintering system. The present invention provides a blast furnace iron ditch skimmer suitable for oscillation sintering and a preparation method thereof. By redesigning the formula, the raw materials of the blast furnace iron ditch skimmer are well adapted to oscillation sintering. The obtained product has good high temperature performance, high volume stability, excellent corrosion resistance, long service life, and low comprehensive operation and maintenance costs. The iron throughput of large and medium-sized blast furnace skimmers is increased to 350,000 to 400,000 tons at a time, which effectively improves the service life of the skimmer and has significant economic and social benefits.

[0009] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0010] The raw material composition of the blast furnace iron ditch slag skimmer suitable for oscillating sintering is as follows in terms of mass percentage:

[0011] Brown corundum aggregate with a particle size of 5 to 8 mm: 18% to 25%;

[0012] Brown corundum aggregate with a particle size of 3 to 5 mm: 18% to 25%;

[0013] Brown corundum particles with a particle size of 1 to 3 mm 10% to 18%;

[0014] 8% to 15% of dense corundum particles with a particle size of 0.074 to 1 mm;

[0015] 5% to 9% of dense corundum fine powder with a particle size of ≤0.074mm;

[0016] 6% to 12% of silicon carbide particles with a particle size of 0.074 to 1 mm;

[0017] Silicon carbide fine powder with a particle size of ≤0.074mm 6% to 12%;

[0018] Spherical asphalt with a particle size of 0.1 to 0.8 mm 0.5% to 3%;

[0019] Submicron SiO2 powder with a particle size of ≤0.020mm 3% to 6%;

[0020] α-Al2O3 powder with a particle size of ≤0.020mm 2% to 7%;

[0021] Boron oxide powder with a particle size of ≤0.044 mm 0.5% to 1.0%.

[0022] According to the above scheme, the Al2O3 content of the brown corundum is not less than 95.0wt%, the Fe2O3 content is not higher than 0.5wt%, and the C content is not higher than 0.2wt%.

[0023] According to the above scheme, the Al2O3 content of the dense corundum is not less than 99.0wt%, the Fe2O3 content is not higher than 0.2wt%, and the C content is not higher than 0.1wt%.

[0024] According to the above solution, the SiC content of the silicon carbide is not less than 98.0wt%.

[0025] According to the above scheme, the C content of the spherical asphalt is not less than 55.0wt%.

[0026] According to the above scheme, the SiO2 content of the submicron SiO2 powder is not less than 99.8wt%, D 90 Not higher than 3μm.

[0027] According to the above scheme, the Al2O3 content of the α-Al2O3 powder is not less than 99.5wt%, D 50 Not higher than 5μm.

[0028] In the above scheme, the B2O3 content of the boron oxide powder is not less than 99.9wt%, D 50 Not higher than 25μm.

[0029] The preparation method of the blast furnace iron ditch slag skimmer suitable for oscillating sintering comprises the following steps:

[0030] (1) After the raw materials are mixed, 3% to 5% of water is added to mix evenly, and after pouring, vibration molding is performed to obtain a prefabricated part;

[0031] (2) One-stage oscillation sintering: the temperature is raised to 1100-1150°C at a rate of 4-5°C / min at room temperature. When the temperature reaches 500-550°C, the preform is clamped and oscillated, wherein the clamping pressure is 2-5 MPa and the oscillation frequency is 2-4 Hz;

[0032] (3) Second stage oscillation sintering: Continue to raise the temperature to 1350-1370°C at a rate of 2-3°C / min, while clamping the preform and oscillating it, wherein the clamping pressure is 5-8 MPa and the oscillation frequency is 4-5 Hz.

[0033] According to the above solution, the clamping pressure application direction is consistent with the oscillation direction.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] The present invention changes the original castable cement bonding system and adopts submicron SiO2 powder bonding. The Si-O-Si bond formed can be broken and reorganized during the oscillation process, and the submicron SiO2 powder can fill the pores more effectively, which effectively solves the problem that the CA6 formed by traditional cement bonding has excessive rigidity and too many pores in the structure, which is not suitable for oscillation sintering.

[0036] The present invention introduces boron oxide powder and utilizes its low-temperature liquefaction (liquefaction temperature < 500° C.) characteristics to form a proper amount of liquid phase, thereby improving the particle rearrangement rate and effect of the first-stage oscillation sintering and accelerating the densification process.

[0037] The present invention develops the synergistic effect of submicron SiO2 powder and boron oxide powder in oscillation sintering. Under the medium temperature conditions of oscillation and pressurization, the high-activity submicron SiO2 powder undergoes mullite reaction in advance, and the boron oxide liquid phase is dissolved in the mullite phase to form a high-strength / high aspect ratio boron-doped mullite network structure, avoiding the residue of excess liquid phase and the formation of aluminum borate phase, ensuring the volume stability of the preform and improving the high-temperature performance.

[0038] In the first-stage oscillation sintering process, the present invention adopts a method of rapid heating at medium and low temperatures, applying small pressure, and low oscillation frequency, which is beneficial to optimizing the quality and effect of particle rearrangement by oscillation sintering; in the second-stage oscillation sintering process, the development and growth of boron-doped mullite are accelerated by slow heating, applying large pressure, and high oscillation frequency at high temperature, thereby improving high-temperature performance.

[0039] The present invention makes the raw materials of the blast furnace iron ditch slag skimmer well adapted to the oscillation sintering by redesigning the formula. The volume change rate of the obtained product during service is -0.1% to 0.1%, the flexural strength at room temperature is not less than 20.0MPa, the flexural strength at high temperature is not less than 15.0MPa, the erosion index is not higher than 0.10, the service life of the main body exceeds 180 days, and the comprehensive operation and maintenance cost is reduced by more than 20%. DETAILED DESCRIPTION

[0040] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0041] In a specific embodiment, the selected brown corundum has an Al2O3 content of 95.2%, a Fe2O3 content of 0.14%, and a C content of 0.07%; the dense corundum has an Al2O3 content of 99.1%, a Fe2O3 content of 0.11%, and a C content of 0.05%; the submicron SiO2 powder has an SiO2 content of 99.9%, and the D 90 1.8μm; Al2O3 content in α-Al2O3 powder is 99.6%, D 50 4.7μm; B2O3 content in boron oxide powder is 99.9%, D 50 Unless otherwise specified, the raw materials used were purchased from the market.

[0042] Example 1

[0043] The raw materials and contents of the iron ditch skimmer are: 24.5% brown corundum aggregate with a particle size of 5-8mm, 18% brown corundum aggregate with a particle size of 3-5mm, 10% brown corundum particles with a particle size of 1-3mm, 12% dense corundum particles with a particle size of 0.074-1mm, 9% dense corundum fine powder with a particle size of ≤0.074mm, 6% silicon carbide particles with a particle size of 0.074-1mm, 12% silicon carbide fine powder with a particle size of ≤0.074mm, 3% spherical asphalt with a particle size of 0.1-0.8mm, 3% submicron SiO2 powder with a particle size of ≤0.020mm, 2% α-Al2O3 powder with a particle size of ≤0.020mm, and 0.5% boron oxide powder with a particle size of ≤0.044mm.

[0044] The preparation method of the oscillating sintering blast furnace iron ditch slag skimmer is as follows: (1) mixing the raw materials until uniform, adding 3.0% water and continuing to stir and mix for 3 minutes, and casting and vibrating to form a prefabricated part; (2) casting the prefabricated part and oscillating and sintering it into a finished part; (3) casting and embedding the finished skimmer part in the corresponding position of the main ditch of the iron ditch on site to start service.

[0045] One-stage oscillation sintering: the heating rate is 4.0°C / min, the preform is clamped and oscillated when the temperature reaches 500°C, and the end temperature is 1100°C; the clamping pressure is 2MPa and the oscillation frequency is 2Hz.

[0046] Second stage oscillation sintering: continue to heat up to 1350°C at 2.0°C / min, while clamping the preform and oscillating it, with a clamping pressure of 5 MPa and an oscillation frequency of 4 Hz.

[0047] Example 2

[0048] The raw materials and contents of the iron ditch skimmer are: 18% brown corundum aggregate with a particle size of 5-8mm, 25% brown corundum aggregate with a particle size of 3-5mm, 18% brown corundum particles with a particle size of 1-3mm, 8% dense corundum particles with a particle size of 0.074-1mm, 5% dense corundum fine powder with a particle size of ≤0.074mm, 10% silicon carbide particles with a particle size of 0.074-1mm, 6% silicon carbide fine powder with a particle size of ≤0.074mm, 1.3% spherical asphalt with a particle size of 0.1-0.8mm, 6% submicron SiO2 powder with a particle size of ≤0.020mm, 2% α-Al2O3 powder with a particle size of ≤0.020mm, and 0.7% boron oxide powder with a particle size of ≤0.044mm.

[0049] The preparation method of the oscillating sintering blast furnace iron ditch slag skimmer is as follows: (1) mixing the raw materials until uniform, adding 5.0% water and continuing to stir and mix for 5 minutes, and casting and vibrating to form a prefabricated part; (2) casting the prefabricated part and oscillating and sintering it into a finished part; (3) casting and embedding the finished skimmer part in the corresponding position of the main ditch of the iron ditch on site to start service.

[0050] One-stage oscillation sintering: the heating rate is 4.5°C / min, the preform is clamped and oscillated when the temperature reaches 520°C, and the end temperature is 1110°C; the clamping pressure is 2.5MPa and the oscillation frequency is 3Hz.

[0051] Second stage oscillation sintering: continue to heat up to 1355°C at 2.5°C / min, while clamping the preform and oscillating it, with a clamping pressure of 6 MPa and an oscillation frequency of 5 Hz.

[0052] Example 3

[0053] The raw materials and contents of the iron ditch skimmer are: 20% brown corundum aggregate with a particle size of 5-8mm, 20% brown corundum aggregate with a particle size of 3-5mm, 12.7% brown corundum particles with a particle size of 1-3mm, 15% dense corundum particles with a particle size of 0.074-1mm, 6% dense corundum fine powder with a particle size of ≤0.074mm, 7% silicon carbide particles with a particle size of 0.074-1mm, 7% silicon carbide fine powder with a particle size of ≤0.074mm, 1.5% spherical asphalt with a particle size of 0.1-0.8mm, 5% submicron SiO2 powder with a particle size of ≤0.020mm, 5% α-Al2O3 powder with a particle size of ≤0.020mm, and 0.8% boron oxide powder with a particle size of ≤0.044mm.

[0054] The preparation method of the oscillating sintering blast furnace iron ditch slag skimmer is as follows: (1) mixing the raw materials until uniform, adding 4.0% water and continuing to stir and mix for 4 minutes, and casting and vibrating to form a prefabricated part; (2) casting the prefabricated part and oscillating and sintering it into a finished part; (3) casting and embedding the finished skimmer part in the corresponding position of the main ditch of the iron ditch on site to start service.

[0055] One-stage oscillation sintering: the heating rate is 5.0°C / min, the preform is clamped and oscillated when the temperature reaches 550°C, and the end temperature is 1150°C; the clamping pressure is 5.0MPa and the oscillation frequency is 4Hz.

[0056] Second stage oscillation sintering: continue to heat up to 1360°C at 3.0°C / min, while clamping the preform and oscillating it, with a clamping pressure of 7 MPa and an oscillation frequency of 4 Hz.

[0057] Example 4

[0058] The raw materials and contents of the iron ditch skimmer are: 25% brown corundum aggregate with a particle size of 5-8mm, 18% brown corundum aggregate with a particle size of 3-5mm, 10% brown corundum particles with a particle size of 1-3mm, 10% dense corundum particles with a particle size of 0.074-1mm, 6.5% dense corundum fine powder with a particle size of ≤0.074mm, 12% silicon carbide particles with a particle size of 0.074-1mm, 6% silicon carbide fine powder with a particle size of ≤0.074mm, 0.5% spherical asphalt with a particle size of 0.1-0.8mm, 4% submicron SiO2 powder with a particle size of ≤0.020mm, 7% α-Al2O3 powder with a particle size of ≤0.020mm, and 1.0% boron oxide powder with a particle size of ≤0.044mm.

[0059] The preparation method of the oscillating sintering blast furnace iron ditch slag skimmer is as follows: (1) mixing the raw materials until uniform, adding 3.5% of water and continuing to stir and mix for 4 minutes, and casting and vibrating to form a prefabricated part; (2) casting the prefabricated part and oscillating and sintering it into a finished part; (3) casting and embedding the finished skimmer part in the corresponding position of the main ditch of the iron ditch on site to start service.

[0060] One-stage oscillation sintering: the heating rate is 4.0°C / min, the preform is clamped and oscillated when the temperature reaches 540°C, and the end temperature is 1150°C; the clamping pressure is 4.0MPa and the oscillation frequency is 3Hz.

[0061] Second stage oscillation sintering: continue to heat up to 1370°C at 2.0°C / min, while clamping the preform and oscillating it, with a clamping pressure of 8 MPa and an oscillation frequency of 5 Hz.

[0062] Comparative Example 1

[0063] Example 1 was repeated, except that the submicron SiO2 powder with a particle size of ≤0.020 mm in the formula was replaced with aluminate cement, and the amount used remained unchanged.

[0064] Comparative Example 2

[0065] Example 1 was repeated, except that the boron oxide powder with a particle size of ≤0.044 mm in the formula was replaced with α-Al2O3 micropowder with a particle size of ≤0.020 mm, and the amount used remained unchanged.

[0066] Comparative Example 3

[0067] Example 1 was repeated, using the same temperature-raising sintering method, but the clamping and oscillation were eliminated.

[0068] Comparative Example 4

[0069] Example 1 was repeated, and one-time oscillation sintering was adopted: the temperature was directly raised to 1350° C. at a heating rate of 4.0° C. / min, and the preform was clamped and oscillated when the temperature reached 500° C.; the clamping pressure was 2 MPa and the oscillation frequency was 2 Hz.

[0070] The permanent linear change rate of the finished part at 1450°C × 3h was determined by the method in GB / T 5988-2022, the room temperature flexural strength of the finished part after heat treatment at 1450°C × 3h was determined by the method in GB / T3001-2017, the high temperature flexural strength of the castable at 1400°C × 1h was determined by the method in GB / T 3002-2017, and the slag iron corrosion resistance was determined by the method in GB / T 8931-2007 (static crucible method). The performance of each embodiment and each comparative example is compared, as shown in Table 1.

[0071] Table 1

[0072]

[0073] In Comparative Example 1, since aluminate cement is used as a binder, the prefabricated part has excessive rigidity, which can easily cause internal microcracks to extend during the oscillation pressure process and destroy the original structure. In addition, the CaO in the cement will be converted into a liquid phase at high temperatures, resulting in a significant decrease in high-temperature strength.

[0074] In Comparative Example 2, α-Al2O3 powder is used to replace boron oxide powder, which significantly reduces the efficiency of particle rearrangement and densification during the low-temperature oscillation sintering process and cannot be adapted to the oscillation sintering process.

[0075] In Comparative Example 3, a pre-sintering treatment method is adopted. The lack of clamping pressure and vibration causes a significant decrease in the sintering densification degree of the preform. Compared with the traditional method, the performance and use effect are not significantly improved, and the overall cost is not much different.

[0076] In Comparative Example 4, oscillation sintering was not performed in stages, resulting in incomplete particle rearrangement and incomplete boron-doped mullite formation, which resulted in failure to fully exert the effect of oscillation sintering, and the performance and use effect were lower than those of Example 1.

[0077] The above embodiments are merely examples for clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the protection scope of the invention.

Claims

1. The blast furnace iron ditch slag skimmer suitable for oscillating sintering is characterized by The raw material composition is calculated by mass percentage as follows: Brown corundum aggregate with a particle size of 5 to 8 mm: 18% to 25%; Brown corundum aggregate with a particle size of 3 to 5 mm: 18% to 25%; Brown corundum particles with a particle size of 1 to 3 mm 10% to 18%; 8% to 15% of dense corundum particles with a particle size of 0.074 to 1 mm; 5% to 9% of dense corundum fine powder with a particle size of ≤0.074mm; 6% to 12% of silicon carbide particles with a particle size of 0.074 to 1 mm; Silicon carbide fine powder with a particle size of ≤0.074mm 6% to 12%; Spherical asphalt with a particle size of 0.1 to 0.8 mm 0.5% to 3%; Submicron SiO2 powder with a particle size of ≤0.020mm 3% to 6%; α-Al2O3 powder with a particle size of ≤0.020mm 2% to 7%; Boron oxide powder with a particle size of ≤0.044 mm 0.5% to 1.0%.

2. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The brown corundum has an Al2O3 content of not less than 95.0wt%, a Fe2O3 content of not more than 0.5wt%, and a C content of not more than 0.2wt%.

3. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The dense corundum has an Al2O3 content of not less than 99.0wt%, a Fe2O3 content of not more than 0.2wt%, and a C content of not more than 0.1wt%.

4. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The SiC content of the silicon carbide is not less than 98.0 wt %.

5. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The C content of the spherical asphalt is not less than 55.0 wt %.

6. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The SiO2 content of the submicron SiO2 powder is not less than 99.8wt%, D 90 Not higher than 3μm.

7. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The Al2O3 content of the α-Al2O3 powder is not less than 99.5wt%, D 50 Not higher than 5μm.

8. The blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 1, characterized in that The boron oxide powder has a B2O3 content of not less than 99.9wt%, D 50 Not higher than 25μm.

9. The method for preparing the blast furnace iron ditch slag skimmer suitable for oscillating sintering according to claim 1, characterized in that The following steps are involved: (1) After the raw materials are mixed, 3% to 5% of water is added to mix evenly, and after pouring, vibration molding is performed to obtain a prefabricated part; (2) One-stage oscillation sintering: the temperature is raised to 1100-1150°C at a rate of 4-5°C / min at room temperature. When the temperature reaches 500-550°C, the preform is clamped and oscillated, wherein the clamping pressure is 2-5 MPa and the oscillation frequency is 2-4 Hz; (3) Second stage oscillation sintering: Continue to raise the temperature to 1350-1370°C at a rate of 2-3°C / min, while clamping the preform and oscillating it, wherein the clamping pressure is 5-8 MPa and the oscillation frequency is 4-5 Hz.

10. The method for preparing the blast furnace iron ditch slag skimmer suitable for oscillating sintering as claimed in claim 9, characterized in that The clamping pressure application direction is consistent with the oscillation direction.

Citation Information

Patent Citations

  • PROCESS FOR PREPARING A HYDRAULIC REFERENCE CEMENT COMPOSITION

    ATA187286A

  • Anhydrous stemming and preparation method thereof

    CN102951909A

  • Cement-free iron runner castable for skimmer preformed unit

    CN110372342A

  • Silicon carbide whisker / aluminum oxide ceramic composite material and preparation method thereof

    CN111892415A

  • Submicron SiO2 micro powder combined iron runner castable and preparation method thereof

    CN112830772A