Axial heat-conducting zeolite honeycomb material as well as preparation method and application thereof
By combining low boiling point organic solvents and n-level wedge filters, the fiber thermal conductivity materials are distributed in a directional manner in zeolite honeycomb materials, solving the problem of insufficient thermal conductivity of traditional zeolite honeycomb materials and achieving higher thermal conductivity and adsorption efficiency .
Patent Information
- Application Number
- CN202411197578.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-08-29
AI Technical Summary
Traditional zeolite honeycomb materials have insufficient thermal conductivity during high-temperature desorption, resulting in increased energy consumption and extended processing time. Methods that improve thermal conductivity are likely to lead to decreased adsorption performance.
By using an n-level wedge filter to distribute the fiber thermally conductive material in the presence of low boiling point organic solvents, axial heat-conducting zeolite honeycomb materials are prepared to ensure adsorption performance while improving thermal conductivity.
It improves the axial thermal conductivity of zeolite honeycomb materials, enhances the heat transfer efficiency during the VOCs desorption process, shortens the time to reach the desorption temperature, and maintains the original good adsorption performance.
Smart Images

Figure BDA0005016914210000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of zeolite materials, and in particular relates to an axially heat-conducting zeolite honeycomb material and a preparation method and application thereof. Background Art
[0002] Zeolite material is a kind of aluminosilicate material, which is mainly composed of silicon-oxygen tetrahedron and aluminum-oxygen tetrahedron with a regular nanoporous structure. Due to its porous structure and good thermal stability and acid resistance, it is widely used in catalysis, adsorption separation and other fields.
[0003] In the adsorption treatment application of volatile organic pollutants (VOCs), zeolite honeycomb materials have received extensive attention and application due to their good adsorption performance and low pressure loss. However, traditional zeolite honeycomb materials have poor thermal conductivity, which limits their efficiency in the high-temperature desorption process, resulting in increased energy consumption and extended processing time. At present, the thermal conductivity of zeolite honeycomb materials is often improved by increasing the proportion of thermally conductive fillers in zeolite honeycomb materials, but this method easily leads to a decrease in the adsorption performance of zeolite honeycomb materials. Therefore, how to improve the thermal conductivity of zeolite honeycomb materials while ensuring good adsorption performance of zeolite honeycomb materials is of great significance to improving the efficiency of the overall process system. Summary of the invention
[0004] One of the purposes of the present invention is to solve the problem of how to improve the thermal conductivity and desorption efficiency of zeolite honeycomb materials while ensuring good adsorption performance of the zeolite honeycomb materials, and to provide a method for preparing axially heat-conducting zeolite honeycomb materials.
[0005] The second object of the present invention is to provide an axially heat-conducting zeolite honeycomb material prepared by the above preparation method.
[0006] The third object of the present invention is to provide the use of the above-mentioned axial heat-conducting zeolite honeycomb material in the treatment of volatile organic pollutants.
[0007] Specifically, the preparation method of the axially heat-conducting zeolite honeycomb material includes: S1. filtering a first mud material through an n-stage filter in the presence of a low-boiling point organic solvent, the first mud material containing zeolite material, fiber thermal conductive material, adhesive, water and optional additives, each stage of the filter is provided with a wedge-shaped filter hole, the pore size of the wedge-shaped filter hole gradually decreases along the filtering direction, and the outlet pore size of the wedge-shaped filter hole in each stage of the filter is smaller than the length of the fiber thermal conductive material, so that the fiber thermal conductive material in the first mud material is directionally distributed to obtain a second mud material, wherein n≧2; S2. extruding the second mud material after aging treatment, and then performing shaping and sintering treatment to obtain an axially heat-conducting zeolite honeycomb material.
[0008] In a preferred embodiment, the outlet aperture size of the wedge-shaped filter holes in each filter stage of the n-stage filter is independently 10-60% of the length of the fiber thermal conductive material.
[0009] In a preferred embodiment, the outlet aperture size of the wedge-shaped filter holes of the upper filter stage in the n-stage filter is larger than the outlet aperture size of the wedge-shaped filter holes of the lower filter stage.
[0010] In a preferred embodiment, based on the dry total amount of the first mud material, the content of the zeolite material is 50-70wt%, the content of the fiber thermal conductive material is 5-9wt%, the content of the adhesive is 20-40wt%, and the content of the auxiliary agent is 3-8wt%.
[0011] In a preferred embodiment, the low boiling point organic solvent is selected from at least one of methanol, ethanol and isopropanol.
[0012] In a preferred embodiment, the low boiling point organic solvent is used in an amount such that the pressure of the first mud material passing through the n-stage wedge filter is 2 to 10 MPa.
[0013] In a preferred embodiment, the zeolite material is selected from at least one of ZSM5 zeolite, NaY zeolite, Beta zeolite and Y zeolite.
[0014] In a preferred embodiment, the average particle size of the zeolite material is 150-300 mesh.
[0015] In a preferred embodiment, the fiber thermal conductive material is selected from at least one of carbon fiber, metal fiber, silicon carbide fiber, aluminum nitride fiber and aluminum oxide fiber.
[0016] In a preferred embodiment, the average length of the fiber thermal conductive material is 1 to 3 mm.
[0017] In a preferred embodiment, the average diameter of the fiber thermal conductive material is 0.02-0.05 mm.
[0018] In a preferred embodiment, before step S1, the first mud material is further filtered through a first filter and a low-boiling point organic solvent is added during the filtering to soften the first mud material.
[0019] In a preferred embodiment, the pore size of the filter holes in the first filter is 2-3 mm.
[0020] In a preferred embodiment, the outlet aperture size of the wedge-shaped filter holes of each stage of the n-stage filter is independently 0.1 to 1.8 mm.
[0021] In a preferred embodiment, the binder is a mixture of clay and cellulose.
[0022] In a preferred embodiment, the mass ratio of the clay to the cellulose is (3-9):1.
[0023] In a preferred embodiment, the auxiliary agent is selected from at least one of a humectant, a lubricant, a sintering aid, a dispersant, a stabilizer, a flow agent, and an anti-foaming agent.
[0024] In a preferred embodiment, the sintering treatment conditions include a temperature of 500-700° C. and a time of 4-6 hours.
[0025] The key to the present invention is to control the softness of the mud material by adding a low-boiling point organic solvent, and on this basis, the fiber heat-conducting material in the mud material is directional distributed through the action of an n-stage filter with a wedge-shaped filter hole, so that the fiber heat-conducting material in the obtained zeolite honeycomb material is distributed along the axial direction, and the axial heat-conducting performance is improved. The improvement of the axial heat-conducting performance is conducive to enhancing the heat transfer of the zeolite honeycomb material in the VOCs desorption process, which can improve the thermal energy utilization efficiency and shorten the time to reach the desorption temperature, thereby helping to improve the desorption efficiency of the zeolite honeycomb material. It is speculated that the reason may be that: the fiber heat-conducting material is directional distributed through the combined action of the low-boiling point organic solvent and the n-stage filter with a wedge-shaped filter hole. Compared with adding water or other high-boiling point organic solvents, the low-boiling point organic solvent in the mud material obtained after filtration can evaporate quickly, so that the fiber heat-conducting material in the mud material can maintain a good directional distribution state during the aging treatment and enter the subsequent operation, and the directional distribution of the fiber heat-conducting material will not be reduced due to the untimely evaporation of the solvent, and the mud material after filtration maintains a high softness. Compared with the prior art method of improving the thermal conductivity of zeolite honeycomb materials by increasing the addition ratio of thermal conductive materials, which method will lead to a decrease in the adsorption performance of the zeolite honeycomb materials, under the condition that the addition ratio of fiber thermal conductive materials is the same, the zeolite honeycomb material prepared by the method provided by the present invention not only has better thermal conductivity and higher desorption efficiency, but also can maintain the original good adsorption performance. DETAILED DESCRIPTION
[0026] The preparation method of the axially heat-conducting zeolite honeycomb material provided by the present invention comprises: S1. filtering a first mud material through an n-stage filter in the presence of a low-boiling-point organic solvent, wherein the first mud material contains a zeolite material, a fiber heat-conducting material, an adhesive, water and optional additives, and each stage of the filter is provided with a wedge-shaped filter hole, the aperture size of the wedge-shaped filter hole gradually decreases along the filtering direction, and the outlet aperture size of the wedge-shaped filter hole in each stage of the filter is smaller than the length of the fiber heat-conducting material, so that the fiber heat-conducting material in the first mud material is distributed in a direction, and a second mud material is obtained, wherein n≧2, such as 2, 3, 4, 5, etc.; S2. after the second mud material is extruded and formed, it is subjected to shaping and sintering treatment, i.e., the axially heat-conducting zeolite honeycomb material is obtained.
[0027] It should be noted that “axial direction” refers to the central axis direction of the pore structure of the zeolite honeycomb material. When the zeolite honeycomb material is used to treat volatile organic pollutants, the “axial direction” is the same as the direction of gas passing through the zeolite honeycomb material.
[0028] In addition, the terms "first" and "second" are only used to refer to clay materials that appear in different orders for easy distinction. They have no other special meanings and cannot be understood as limitations on the components and contents of the clay materials.
[0029] In the present invention, the outlet aperture size of the wedge-shaped filter holes in each filter of the n-stage filter is preferably 10-60% of the length of the fiber heat conductive material, such as 10%, 20%, 30%, 40%, 50%, 60% or any value therebetween. Controlling the outlet aperture size of the wedge-shaped filter holes in the final filter within the above preferred range is more conducive to improving the directional distribution of the fiber heat conductive material in the mud after filtering through the n-stage filter, thereby being more conducive to improving the axial heat conductive performance of the zeolite honeycomb material.
[0030] In the present invention, the outlet aperture size of the wedge-shaped filter holes of each filter in the n-stage filter can be the same or different. More preferably, the outlet aperture size of the wedge-shaped filter holes of the upper filter in the n-stage filter is larger than the outlet aperture size of the wedge-shaped filter holes of the lower filter. At this time, by designing the outlet aperture size of the wedge-shaped filter holes in the n-stage filter to decrease step by step, it is more conducive to the directional distribution of the fiber heat-conducting material in the mud obtained after filtering through the n-stage filter, thereby improving the axial heat conduction performance of the zeolite honeycomb material. The outlet aperture size of the wedge-shaped filter holes of the lower filter in the n-stage filter can be 65-100% of the outlet aperture size of the wedge-shaped filter holes of the upper filter, such as 65%, 68%, 70%, 75%, 80%, 85%, 90%, 95%, 100% or any value therebetween. When it is less than the above preferred range, it may cause excessive pressure during mud filtering, which is not conducive to achieving directional distribution of fiber heat-conducting materials.
[0031] In the present invention, based on the dry total of the first mud material, the content of the zeolite material is preferably 50-70wt%, such as 50wt%, 60wt%, 70wt% or any value therebetween. The content of the fiber thermal conductive material is preferably 5-9wt%, such as 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or any value therebetween. The content of the adhesive is preferably 20-40wt%, such as 20wt%, 25wt%, 30wt%, 35wt%, 40wt% or any value therebetween. The content of the auxiliary agent is preferably 3-8wt%, such as 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt% or any value therebetween.
[0032] The present invention does not limit the specific type of the low boiling point organic solvent, as long as it can soften the clay after addition and is easily volatilized under normal temperature and pressure conditions. The boiling point of the low boiling point organic solvent is preferably below 85°C, and specific examples thereof include but are not limited to: at least one of methanol, ethanol and isopropanol, and more preferably ethanol.
[0033] The present invention does not specifically limit the amount of the low-boiling point organic solvent, as long as it can soften the mud after addition and make the fiber thermal conductive material in the mud oriented and distributed through the action of the n-stage filter. The amount of the low-boiling point organic solvent is preferably such that the pressure of the first mud passing through the n-stage filter is 2 to 10 MPa, such as 2 MPa, 5 MPa, 8 MPa, 10 MPa or any value therebetween.
[0034] The present invention does not specifically limit the type of the zeolite material, as long as it has a porous structure formed by an aluminosilicate skeleton and can adsorb pollutants, it can be various existing natural zeolite materials, or various existing artificially prepared or modified zeolite materials, and its specific examples include but are not limited to: at least one of ZSM5 zeolite, NaY zeolite, Beta zeolite and Y zeolite. The average particle size of the zeolite material is preferably 150 to 300 mesh, such as 150 mesh, 180 mesh, 200 mesh, 220 mesh, 250 mesh, 280 mesh, 300 mesh or any value therebetween. Within this preferred range, the zeolite material can be better mixed with the directional distributed fiber thermal conductive material, so as to be more conducive to improving the desorption rate through the axial thermal conductivity of the fiber thermal conductive material.
[0035] The present invention does not limit the specific type of the fiber thermal conductive material, which can be any existing fiber-shaped material that can perform a thermal conductive function, and its specific examples include but are not limited to: at least one of carbon fiber, metal fiber, silicon carbide fiber, aluminum nitride fiber and aluminum oxide fiber. The average length of the fiber thermal conductive material is preferably 1-3 mm, such as 1 mm, 1.5 mm, 2 mm, 2.5 mm, 3 mm or any value therebetween. Controlling the average length of the fiber thermal conductive material within the above preferred range is more conducive to the directional distribution of the fiber thermal conductive material through the action of the n-stage filter, and will not cause the fiber of the thermal conductive material to break during the n-stage filter treatment process due to the excessively long fiber length, or the n-stage filter with a small outlet aperture of the wedge-shaped filter hole due to the excessively short fiber length is easy to clog and is not conducive to the directional distribution of the fiber thermal conductive material, which is more conducive to improving the axial thermal conductivity of the zeolite honeycomb material. The average diameter of the fiber thermal conductive material is preferably 0.02-0.05 mm, such as 0.02 mm, 0.03 mm, 0.04 mm, 0.05 mm or any value therebetween.
[0036] The present invention does not limit the specific type of the adhesive, as long as it is a substance that can play a bonding role on the various raw materials added, and its specific examples include but are not limited to: at least one of pseudo-boehmite, polyurethane-based adhesives, epoxy resin-based adhesives, clay and cellulose. The adhesive is preferably a mixture of clay and cellulose. The mass ratio of the clay to the cellulose is preferably (3 to 9):1, such as 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or any value therebetween. Among them, the clay can be at least one of palygorskite, kaolin, bentonite and activated white clay. The cellulose can be at least one of carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose and hydroxypropyl methyl cellulose.
[0037] In the present invention, the auxiliary agent is preferably at least one selected from the group consisting of a humectant, a lubricant, a sintering aid, a dispersant, a stabilizer, a flow agent, and an antifoaming agent.
[0038] In the present invention, in step S1, the first raw material can be obtained by mixing zeolite material, fiber thermal conductive material, adhesive, water and optional auxiliary agent in any order, and the mixing order of each component is not fixed, and they can be added at the same time and then mixed together, or at least one of the remaining components except water can be mixed with water first and then the remaining components can be added at the same time or in sequence. Step S1 of the present invention is preferably carried out in the following manner: pre-mix the zeolite material and a part of the adhesive, then add the remaining adhesive and water and stir and mix, and then add the fiber thermal conductive material and the auxiliary agent and stir and mix, so as to obtain the first mud material.
[0039] In the present invention, before step S1, the first mud material may be filtered through a first filter and a low-boiling organic solvent may be added during the process to soften the first mud material. At this time, the function of the first filter is to first form the first mud material into small thin strips, which makes it easier for the first mud material to be oriented and distributed to the fiber thermal conductive material through the subsequent n-stage filter. The filter holes in the first filter may be wedge-shaped filter holes or conventional filter holes with the same inlet and outlet aperture sizes. The present invention does not specifically limit the aperture size of the filter holes in the first filter, which is preferably 2 to 3 mm, such as 2 mm, 2.2 mm, 2.5 mm, 2.8 mm, 3 mm or any value therebetween. The outlet aperture size of the wedge-shaped filter holes of the final filter in the n-stage filter is preferably 0.1 to 1.8 mm, such as 0.1 mm, 0.2 mm, 0.5 mm, 0.8 mm, 1 mm, 1.2 mm, 1.5 mm, 1.8 mm or any value therebetween.
[0040] In the present invention, the aging treatment in step S2 preferably includes placing the second mud material in a constant temperature and humidity environment, and the placement time can be determined according to actual conditions, and is preferably 12 to 36 hours, such as 12 hours, 15 hours, 18 hours, 20 hours, 24 hours, 30 hours, 36 hours or any value therebetween.
[0041] In the present invention, the shaping treatment in step S2 may be natural drying of the semi-finished zeolite honeycomb material formed by extrusion, or shaping by microwave treatment, or other shaping treatment methods in the prior art, preferably shaping by microwave treatment. The microwave treatment conditions may be conventionally selected in the art, preferably including a total microwave power of 10 to 15 kW, such as 10 kW, 11 kW, 12 kW, 13 kW, 14 kW, 15 kW or any value therebetween; a microwave frequency of 0.5 to 10 GHz, such as 0.5 GHz, 1 GHz, 2 GHz, 5 GHz, 8 GHz, 10 GHz; a time of 1 to 5 min, such as 1 min, 2 min, 3 min, 4 min, 5 min or any value therebetween; a temperature of 90 to 150 ° C, such as 90 ° C, 100 ° C, 120 ° C, 150 ° C or any value therebetween.
[0042] In the present invention, the sintering treatment conditions include a temperature preferably of 500-700°C, such as 500°C, 550°C, 600°C, 650°C, 700°C or any value therebetween; and a time preferably of 4-6h, such as 4h, 4.5h, 5h, 5.5h, 6h or any value therebetween.
[0043] The present invention will be described in detail below through specific embodiments.
[0044] Example 1
[0045] The raw materials include: 140 kg ZSM5 zeolite (average particle size is 200 mesh), 14 kg silicon carbide fiber (average length is 2 mm, average diameter is 0.03 mm), 40 kg clay material (palygorskite), 12 kg methyl cellulose, 2 kg moisturizer, 2 kg lubricant, 6 kg sintering aid, and 72 kg pure water.
[0046] S1. Pre-mix the ZSM5 zeolite and clay materials by ball milling, transfer them into a mixing tank and add methyl cellulose and pure water. After stirring for 20 minutes, add the moisturizer and continue stirring for 10 minutes. Then add the lubricant, silicon carbide fiber and sintering aid and continue stirring for 10 minutes to form small spherical mud. Then, knead the mud through a twin-screw extruder. The kneading cycle is repeated 3 times and the mud is extruded into a cylindrical shape to obtain the first mud.
[0047] The first mud is filtered through a first filter (the inlet aperture size of the wedge-shaped filter hole is 5.0 mm, and the outlet aperture size is 2.5 mm). During the process, ethanol spray is added to soften the mud. The amount of ethanol added is the amount observed when the pressure gauge drops to 5 MPa. At this time, the mud is squeezed from a cylindrical shape into small strips, and then passed through a primary filter (the inlet aperture size of the wedge-shaped filter hole is 2.5 mm, and the outlet aperture size is 1.0 mm) and a secondary filter (the inlet aperture size of the wedge-shaped filter hole is 1.5 mm, and the outlet aperture size is 0.7 mm) for directional treatment of the mud, thereby obtaining a second mud with a directional distribution of fiber thermal conductive material.
[0048] S2. The second mud material is placed in a constant temperature and humidity space for 24 hours for aging treatment to evaporate ethanol and excess water. When the humidity of the mud material is tested to be about 80% by a hygrometer and the extrusion pressure of the mud material is verified to be 5MPa by a small extrusion device, the mud material can be extruded through a mold to obtain a semi-finished zeolite honeycomb material, and then treated with microwaves (total microwave power 14kW, microwave frequency 5GHz, time 2min, temperature 120°C), and then sintered at 600°C for 4h to obtain an axially heat-conducting zeolite honeycomb material.
[0049] Example 2
[0050] The raw materials include: 100 kg NaY zeolite (average particle size is 250 mesh), 18 kg carbon fiber (average length is 1 mm, average diameter is 0.02 mm), 64 kg clay material (palygorskite), 8 kg carboxymethyl cellulose, 2 kg moisturizer, 2 kg lubricant, 6 kg sintering aid, and 72 kg pure water.
[0051] S1. Pre-mix NaY zeolite and clay materials by ball milling, transfer to a stirring tank and add carboxymethyl cellulose and 72 kg of pure water. After stirring for 20 minutes, add a moisturizer and continue stirring for 10 minutes. Then add a lubricant, carbon fiber and a sintering aid and continue stirring for 10 minutes to form small spherical mud. Then, knead the mud through a twin-screw extruder. The kneading cycle is repeated 3 times and the mud is extruded into a cylindrical shape to obtain the first mud.
[0052] The first mud material is filtered through a first filter (the inlet aperture size of the wedge-shaped filter hole is 4.0 mm, and the outlet aperture size is 2.0 mm), during which ethanol is added to soften the mud material by spraying, and the amount of ethanol added is the amount used when the pressure gauge is observed to drop to 5 MPa. At this time, the mud material is squeezed from a cylindrical shape into small thin strips, and then the mud material is oriented through a primary filter (the inlet aperture size of the wedge-shaped filter hole is 2.0 mm, and the outlet aperture size is 0.3 mm) and a secondary filter (the inlet aperture size of the wedge-shaped filter hole is 0.5 mm, and the outlet aperture size is 0.2 mm), so as to obtain a second mud material with oriented distribution of fiber thermal conductive material;
[0053] S2. The second mud material is placed in a constant temperature and humidity space for 24 hours for aging treatment to evaporate ethanol and excess water. When the humidity of the mud material is tested to be about 80% by a hygrometer and the extrusion pressure of the mud material is verified to be 5MPa by a small extrusion device, the mud material can be extruded through a mold to obtain a semi-finished zeolite honeycomb material, and then treated with microwaves (total microwave power 14kW, microwave frequency 5GHz, time 2min, temperature 120°C), and then sintered at 500°C for 6h to obtain an axially heat-conducting zeolite honeycomb material.
[0054] Example 3
[0055] The raw materials include: 120 kg Beta zeolite (average particle size is 200 mesh), 10 kg aluminum nitride fiber (average length is 3 mm, average diameter is 0.04 mm), 50 kg clay material (palyorczyle), 14 kg hydroxypropyl cellulose, 2 kg moisturizer, 2 kg lubricant, 2 kg sintering aid, and 72 kg pure water.
[0056] S1. Pre-mix Beta zeolite and clay materials by ball milling, transfer to a mixing tank and add hydroxypropyl cellulose and 72 kg of pure water. After stirring for 20 minutes, add a moisturizer and continue stirring for 10 minutes. Then add a lubricant, aluminum nitride fiber and a sintering aid and continue stirring for 10 minutes to form a small spherical mud. Then, knead the mud through a twin-screw extruder. The kneading cycle is repeated 3 times and extruded into a cylindrical shape to obtain the first mud.
[0057] The first mud is filtered through a first filter (the inlet aperture size of the wedge-shaped filter hole is 5.5 mm, and the outlet aperture size is 3.0 mm). During the process, ethanol spray is added to soften the mud. The amount of ethanol added is the amount observed when the pressure gauge drops to 5 MPa. At this time, the mud is squeezed from a cylindrical shape into small strips, and then passed through a primary filter device (the inlet aperture size of the wedge-shaped filter hole is 3.2 mm, and the outlet aperture size is 1.5 mm) and a secondary filter (the inlet aperture size of the wedge-shaped filter hole is 2.0 mm, and the outlet aperture size is 1.2 mm) for directionally processing the mud to obtain a second mud with a directionally distributed fiber thermal conductive material.
[0058] S2. The second mud material is placed in a constant temperature and humidity space for 24 hours for aging treatment to evaporate ethanol and excess water. When the humidity of the mud material is tested to be about 80% by a hygrometer and the extrusion pressure of the mud material is verified to be 5MPa by a small extrusion device, the mud material can be extruded through a mold to obtain a semi-finished zeolite honeycomb material, which is then treated with microwaves (total microwave power 14kW, microwave frequency 5GHz, time 2min, temperature 120°C) and then sintered at 550°C for 5h to obtain an axially heat-conducting zeolite honeycomb material.
[0059] Example 4
[0060] Axial heat conduction zeolite honeycomb material was prepared according to the method of Example 1, except that silicon carbide fibers with an average length of 6 mm and an average diameter of 0.03 mm of the same mass were used instead of silicon carbide fibers with an average length of 2 mm and an average diameter of 0.03 mm, and other conditions were the same, thus obtaining axial heat conduction zeolite honeycomb material.
[0061] Comparative Example 1
[0062] A reference zeolite honeycomb material was prepared according to the method of Example 1, except that the inlet pore size and the outlet pore size of the wedge-shaped filter holes in the first filter, the primary filter and the secondary filter were both 5 mm (the average length of the silicon carbide fiber was 2 mm), and the other conditions were the same, thus obtaining a reference zeolite honeycomb material.
[0063] Comparative Example 2
[0064] A reference zeolite honeycomb material was prepared according to the method of Example 1, except that in step S1, water of the same mass was used instead of ethanol, and other conditions were the same, thus obtaining a reference zeolite honeycomb material.
[0065] Test Case
[0066] The zeolite honeycomb materials prepared in the above examples and comparative examples were tested for axial thermal conductivity and adsorption / desorption efficiency according to the following method. The results are shown in Table 1.
[0067] (1) Axial thermal conductivity: A heat flow meter is used to apply a heat flux in the axial direction of the zeolite honeycomb material and measure the heat energy flowing through the material to calculate its axial thermal conductivity.
[0068] (2) Adsorption and desorption efficiency: The honeycomb prepared in the comparative example was cut into 4 small pieces of 3*3*10 cm and loaded into a glass tube. During adsorption, VOCs (concentration of 1000 ppm, flow rate of 1 m / s) were introduced into the inlet, and the VOCs concentration curve at the tube outlet was recorded; during desorption, hot air at 180° C. (flow rate of 0.2 m / s) was introduced into the inlet, and the VOCs concentration curve and temperature curve at the tube outlet were recorded; the adsorption efficiency was calculated based on the VOCs adsorption concentration curve, the VOCs desorption concentration curve and the desorption temperature curve, and the desorption temperature and the time required to reach the desorption temperature were recorded.
[0069] Wherein, adsorption efficiency = (adsorption inlet concentration - adsorption outlet concentration) / adsorption inlet concentration * 100%.
[0070] Table 1
[0071]
[0072] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.
Claims
1. A method for preparing a zeolite honeycomb material, It is characterized in that The preparation method comprises: S1. filtering a first mud material through an n-stage filter in the presence of a low-boiling-point organic solvent, wherein the first mud material contains a zeolite material, a fiber thermal conductive material, an adhesive, water and optional auxiliary agents, wherein each stage of the filter is provided with a wedge-shaped filter hole, the aperture size of the wedge-shaped filter hole gradually decreases along the filtering direction, and the outlet aperture size of the wedge-shaped filter hole in each stage of the filter is smaller than the length of the fiber thermal conductive material, so that the fiber thermal conductive material in the first mud material is distributed in a direction, thereby obtaining a second mud material, wherein n≧2; S2. subjecting the second mud material to an aging treatment and then extruding it into a shape, and then subjecting it to a shaping and sintering treatment, thereby obtaining a zeolite honeycomb material.
2. The method for preparing the zeolite honeycomb material according to claim 1, It is characterized in that The outlet aperture size of the wedge-shaped filter holes of each filter in the n-stage filter is independently 10 to 60% of the length of the fiber thermal conductive material; Preferably, in the n-stage filter, the outlet aperture size of the wedge-shaped filter holes of the upper-stage filter is larger than the outlet aperture size of the wedge-shaped filter holes of the lower-stage filter.
3. The method for preparing the zeolite honeycomb material according to claim 1, It is characterized in that Based on the total dry weight of the first mud material, the content of the zeolite material is 50-70wt%, the content of the fiber thermal conductive material is 5-9wt%, the content of the adhesive is 20-40wt%, and the content of the auxiliary agent is 3-8wt%.
4. The method for preparing the zeolite honeycomb material according to claim 1 or 2, It is characterized in that The low boiling point organic solvent is selected from at least one of methanol, ethanol and isopropanol; Preferably, the low boiling point organic solvent is used in an amount such that the pressure of the first mud material passing through the n-stage filter is 2 to 10 MPa.
5. The method for preparing the zeolite honeycomb material according to claim 1 or 2, It is characterized in that The zeolite material is selected from at least one of ZSM5 zeolite, NaY zeolite, Beta zeolite and Y zeolite; Preferably, the average particle size of the zeolite material is 150-300 mesh; Preferably, the fiber thermal conductive material is selected from at least one of carbon fiber, metal fiber, silicon carbide fiber, aluminum nitride fiber and aluminum oxide fiber; Preferably, the average length of the fiber thermal conductive material is 1 to 3 mm; Preferably, the average diameter of the fiber thermal conductive material is 0.02-0.05 mm.
6. The method for preparing the zeolite honeycomb material according to claim 5, It is characterized in that Before step S1, the method further includes filtering the first mud material through a first filter and adding a low boiling point organic solvent during the filtering to soften the first mud material; Preferably, the pore size of the filter holes in the first filter is 2 to 3 mm; Preferably, the outlet aperture size of the wedge-shaped filter holes of each stage of the n-stage filter is independently 0.1-1.8 mm.
7. The method for preparing the zeolite honeycomb material according to claim 1 or 2, It is characterized in that The binder is a mixture of clay and cellulose; Preferably, the mass ratio of clay to cellulose is (3-9):1; Preferably, the auxiliary agent is selected from at least one of a humectant, a lubricant, a sintering aid, a dispersant, a stabilizer, a flow agent and an anti-foaming agent.
8. The method for preparing the zeolite honeycomb material according to claim 1 or 2, It is characterized in that The aging treatment includes placing the second clay material in a constant temperature and humidity environment; Preferably, the sintering treatment conditions include a temperature of 500-700° C. and a time of 4-6 hours.
9. Axially heat-conducting zeolite honeycomb material produced by the method for producing a zeolite honeycomb material according to any one of claims 1 to 8.
10. Use of the zeolite honeycomb material according to claim 9 in the treatment of volatile organic pollutants.
Citation Information
Patent Citations
Preparation method of filter element of fly-ash filter for clean coal power generation
CN101642651A
Hierarchical-structured honeycomb material capable of adsorbing volatile organic compound and preparation method of honeycomb material
CN106732342A
Preparation method of cellular high-thermal-conductivity material
CN110421958A
High-strength low-volume-density honeycomb zeolite and production method thereof
CN113426406A
Honeycomb-like ceramic body containing adsorptive zeolite and production thereof
JP1993146676A