Low-melting-point furan copolyester and preparation method thereof
A low-melting-point furan copolyester is synthesized via melt random copolymerization, addressing the limitations of high processing temperatures in existing polyester materials by enhancing flexibility and reducing melting points for broader applications.
Patent Information
- Application Number
- CN202411270136.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
Existing polyester materials face challenges in achieving low melting points and flexibility due to their high processing temperatures, which limits their application in areas like hot melt adhesives and core-skin fibers, and there is a need for bio-based alternatives to reduce environmental impact.
A low-melting-point furan copolyester is prepared using 2,5-furandicarboxylic acid, 1,4-butanediol, aliphatic chain dibasic acid, and polyether diol through a melt random copolymerization method, disrupting the macromolecular chain regularity and increasing flexibility.
The resulting furan copolyester is bio-based, environmentally friendly, and has a controlled melting point of 130-160°C, suitable for applications in hot melt adhesives, core-skin composite fibers, and electronic packaging films.
Smart Images

Figure HDA0005038459570000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyester materials and synthesis thereof, and particularly relates to a low melting point furan copolyester and a preparation method thereof. Background Art
[0002] Polyester refers to a type of polymer containing ester bonds in the main chain, usually formed by the condensation of polyols and polyacids. It has excellent comprehensive performance, good mechanical properties, heat resistance, easy processing and other characteristics. It can be widely used in fibers, engineering plastics, adhesives, coatings and other fields.
[0003] With the development of society, the large-scale application of polyester is also expanding. Most polyester raw materials come from petroleum-based products. The excessive consumption of petrochemical resources has also brought certain pressures to the ecological environment and social development, such as resource depletion, greenhouse effect, ecological sustainability and other issues. In order to alleviate the pressure on resources and the environment, finding new biomass renewable resources to replace existing fossil resources will be a major development direction of polyester in the future.
[0004] As a bio-based monomer, 2,5-furandicarboxylic acid is considered by the U.S. Department of Energy to be one of the 12 important platform compounds with great market potential in the future. Among them, 2,5-furandicarboxylic acid is a renewable biomass resource with abundant sources. It can be prepared from multiple biomass routes, such as the dehydration and cyclization of hexose to generate 5-hydroxymethylfurfural and then oxidized to 2,5-furandicarboxylic acid. 2,5-furandicarboxylic acid contains a five-membered aromatic ring structure and has a similar structure and physical properties to terephthalic acid. It can be used to develop new environmentally friendly bio-based furan polyester materials.
[0005] As a bio-based material with great potential for future applications, furan polyester has outstanding barrier properties and heat resistance, and can largely replace existing polyester products based on petroleum terephthalic acid. At present, the large-scale production and application of furan polyester are still in the initial stage. The application research is mainly based on polyethylene 2,5-furandicarboxylate (PEF), with a single variety. Moreover, PEF is a slow-crystallizing brittle material with a melting point of 210-220°C and a high processing temperature. These factors are not conducive to the in-depth development of furan polyester. At the same time, considering the large-scale application of low-melting-point polyester in hot melt adhesives and core-skin fibers, the development and application of low-melting-point polyester products in my country still have a large gap compared with developed countries abroad, and most of them still need to rely on imports.
[0006] To sum up, in order to achieve low-carbon and environmental protection, promote the development of furan polyester at a deeper level, further expand the application and development of furan polyester products, it is particularly important to develop differentiated and functional products. Summary of the invention
[0007] In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a low-melting-point furan copolyester and a preparation method thereof. In the preparation method, 2,5-furandicarboxylic acid, 1,4-butanediol, aliphatic chain dibasic acid and polyether diol are used as main raw materials, and a melt random copolymerization method is adopted to prepare the furan copolyester, which has a bio-based poly 2,5-furandicarboxylic acid butylene glycol ester molecular chain as the main chain, and introduces part of the aliphatic chain dibasic acid and flexible polyether diol chain segments to destroy the regularity of the macromolecular main chain, increase the molecular distance, reduce the intermolecular interaction force, and increase the overall flexibility of the molecular chain, so that the prepared furan copolyester is not only a bio-based environmentally friendly material, but also has the characteristics of a low melting point.
[0008] To achieve the purpose of the present invention, the present invention adopts the following technical solutions:
[0009] In the first aspect, the present invention provides a method for preparing a low-melting furan copolyester, the method comprising: subjecting 2,5-furandicarboxylic acid, 1,4-butanediol and aliphatic chain dibasic acid to an esterification reaction, and then adding polyether diol to the system for copolymerization to obtain a low-melting furan copolyester.
[0010] Furthermore, the fatty chain dibasic acid is selected from at least one of succinic acid, adipic acid, azelaic acid, sebacic acid, and dibasic acids with a carbon chain length greater than 10, preferably at least one of succinic acid, adipic acid, and sebacic acid.
[0011] Furthermore, the polyether diol is selected from at least one of polyethylene glycol and polypropylene glycol.
[0012] In a preferred embodiment, the method for preparing the low melting point furan copolyester comprises the following steps:
[0013] (1) adding 2,5-furandicarboxylic acid, 1,4-butanediol, aliphatic dibasic acid and a catalyst into a polymerization reactor, mixing, stirring and heating under closed oxygen-free conditions, staying at 70-80° C. for 0.5-1 h, then heating to 160-190° C., and reacting at normal pressure for 1-2 h, then adding a certain amount of 1,4-butanediol, and reacting for 1.5-3 h to complete the esterification reaction;
[0014] (2) adding polyether diol and antioxidant to the polymerization system after the esterification reaction in step (1), heating to 190-210° C. for reaction for 1-3 h, and simultaneously performing vacuum operation. Finally, after the reaction is completed at 220-240° C. and the system vacuum pressure is less than 100 Pa, nitrogen is filled, discharged, and pelletized to obtain low-melting-point furan copolyester chips.
[0015] Furthermore, in step (1), the catalyst is selected from at least one of tetrabutyl titanate, isopropyl titanate, antimony glycol, antimony trioxide, germanium oxide, and stannous oxide, preferably at least one of tetrabutyl titanate and isopropyl titanate.
[0016] Furthermore, in step (2), the antioxidant is selected from at least one of antioxidants 1010, 1098, 168, triphenyl phosphite, and trimethyl phosphate.
[0017] Furthermore, in step (1):
[0018] The molar ratio of the total amount of 2,5-furandicarboxylic acid and aliphatic chain dibasic acid to 1,4-butanediol is 1:2.0-3.5, preferably 1:2.5-3.5.
[0019] The mass ratio of the 2,5-furandicarboxylic acid to the fatty chain dibasic acid is 1:0.1-0.5, preferably 1:0.2-0.5.
[0020] The mass ratio of the 2,5-furandicarboxylic acid to the catalyst is 1:0.002-0.005, preferably 1:0.003-0.005.
[0021] Furthermore, in step (2):
[0022] The mass ratio of the polyether diol to the total amount of 2,5-furandicarboxylic acid, 1,4-butanediol and aliphatic chain dibasic acid is 0.05-0.25:1, preferably 0.08-0.25:1.
[0023] The mass ratio of the antioxidant to 2,5-furandicarboxylic acid is 0.001-0.005:1, preferably 0.002-0.004:1.
[0024] In a second aspect, the present invention provides a low melting point furan copolyester prepared by the above method, wherein the low melting point furan copolyester chips have an intrinsic viscosity of 0.65-1.0 dL / g and a melting point of 130-160°C.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The preparation method of the low melting point furan copolyester provided by the present invention has a simple production process and is easy to industrialize. The present invention adopts a melt random copolymerization method, takes the bio-based poly 2,5-furandicarboxylic acid butylene glycol ester molecular chain as the main chain, introduces part of the fatty chain dibasic acid and the flexible polyether diol chain segment, so as to destroy the regularity of the macromolecular main chain, increase the molecular distance, reduce the intermolecular interaction force, and increase the overall flexibility of the molecular chain. The furan copolyester prepared in this way is not only a bio-based environmentally friendly material, but also has the characteristics of a low melting point, and the melting point can be controlled at 130-160°C, and can be used in the fields of hot melt adhesives, core-skin composite fibers, electronic packaging films, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0028] Figure 1 The DSC spectra of the low melting point furan copolyester prepared in Example 1 and the polybutylene 2,5-furandicarboxylate prepared in Comparative Example 1 are shown. DETAILED DESCRIPTION
[0029] The embodiments of the present invention are described in detail below. The embodiments are given to better illustrate the contents of the present invention and are only used to explain the present invention, but should not be understood as limiting the present invention.
[0030] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased through regular channels.
[0031] The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are commercially available products unless otherwise specified, and the following parts are by mass.
[0032] Embodiment 1:
[0033] A method for preparing a low-melting-point furan copolyester, wherein the main raw materials include 2,5-furandicarboxylic acid, 1,4-butanediol, succinic acid, and polyethylene glycol, and specifically comprises the following steps:
[0034] (1) 100 parts of 2,5-furandicarboxylic acid, 20 parts of succinic acid, 146 parts of 1,4-butanediol, and 0.3 parts of tetrabutyl titanate are added to a polymerization reactor, mixed, stirred, and heated under closed oxygen-free conditions, and kept at 80° C. for 0.5 h, then heated to 185° C., and esterified at normal pressure for 2 h, and then 45 parts of 1,4-butanediol are added, and the esterification reaction is completed after reacting for 3 h;
[0035] (2) 31 parts of polyethylene glycol and 0.2 parts of antioxidant 1010 were added to the polymerization system after the esterification reaction was completed, and the temperature was raised to 200° C. for reaction for 1.5 hours, and vacuum operation was performed simultaneously. Finally, after the reaction was completed at 230° C. and the system vacuum pressure was less than 100 Pa, nitrogen was filled, the material was discharged, and pelletized to obtain low melting point furan copolyester chips, whose DSC spectrum is shown as follows: Figure 1 shown.
[0036] Embodiment 2:
[0037] A method for preparing a low-melting-point furan copolyester, wherein the main raw materials include 2,5-furandicarboxylic acid, 1,4-butanediol, succinic acid, and polyethylene glycol, and specifically comprises the following steps:
[0038] (1) 100 parts of 2,5-furandicarboxylic acid, 30 parts of succinic acid, 185 parts of 1,4-butanediol, and 0.4 parts of tetrabutyl titanate are added to a polymerization reactor, mixed, stirred, and heated under closed oxygen-free conditions, and kept at 80° C. for 1 hour, then heated to 185° C., and esterified at normal pressure for 2 hours, and then 49 parts of 1,4-butanediol are added, and the esterification reaction is completed after reacting for 3 hours;
[0039] (2) 72 parts of polyethylene glycol and 0.3 parts of antioxidant 1010 were added to the polymerization system after the esterification reaction was completed, the temperature was raised to 200° C. and the reaction was carried out for 1.5 hours, and a vacuum operation was simultaneously performed. Finally, after the reaction was completed at 230° C. and the system vacuum pressure was less than 100 Pa, nitrogen was filled, the material was discharged, and pelletized to obtain low-melting-point furan copolyester chips.
[0040] Embodiment 3:
[0041] A method for preparing a low-melting-point furan copolyester, wherein the main raw materials include 2,5-furandicarboxylic acid, 1,4-butanediol, adipic acid, and polypropylene glycol, and specifically comprises the following steps:
[0042] (1) 100 parts of 2,5-furandicarboxylic acid, 30 parts of adipic acid, 190 parts of 1,4-butanediol, and 0.4 parts of tetrabutyl titanate are added to a polymerization reactor, mixed, stirred, and heated under closed oxygen-free conditions, kept at 80° C. for 1 hour, then heated to 180° C., and esterified at normal pressure for 2 hours, and then 39 parts of 1,4-butanediol are added, and the esterification reaction is completed after reacting for 3 hours;
[0043] (2) 80 parts of polypropylene glycol and 0.3 parts of antioxidant 1010 were added to the polymerization system after the esterification reaction was completed, the temperature was raised to 200° C. for reaction for 2 h, and vacuum operation was simultaneously performed. Finally, after the reaction was completed at 220° C. and the system vacuum pressure was less than 100 Pa, nitrogen was filled, the material was discharged, and pelletized to obtain low-melting-point furan copolyester chips.
[0044] Comparative Example 1:
[0045] Comparative Example 1 is the preparation of polybutylene 2,5-furandicarboxylate, the main raw materials include 2,5-furandicarboxylic acid and 1,4-butanediol, and specifically includes the following steps:
[0046] (1) 100 parts of 2,5-furandicarboxylic acid, 116 parts of 1,4-butanediol, and 0.3 parts of tetrabutyl titanate are added to a polymerization reactor, mixed, stirred, and heated under closed oxygen-free conditions, and kept at 80° C. for 0.5 h, then heated to 185° C., and esterified at normal pressure for 2 h, and then 35 parts of 1,4-butanediol are added, and the esterification reaction is completed after reacting for 3 h;
[0047] (2) 0.2 parts of antioxidant 1010 were added to the polymerization system after the esterification reaction was completed, the temperature was raised to 200° C. and the reaction was carried out for 1.5 hours, and a vacuum operation was simultaneously performed. Finally, after the reaction was completed at 240° C. and the system vacuum pressure was less than 100 Pa, nitrogen was filled, the material was discharged, and pelletized to obtain poly (butylene 2,5-furandicarboxylate) slices, whose DSC spectrum is shown as follows: Figure 1 shown.
[0048] Comparative Example 2:
[0049] The difference between Comparative Example 2 and Example 1 is that the comparative example 2 does not contain succinic acid, that is, the main raw materials include 2,5-furandicarboxylic acid, 1,4-butanediol, and polyethylene glycol, and the specific preparation process is similar to that of Example 1.
[0050] Comparative Example 3:
[0051] The difference between Comparative Example 3 and Example 1 is that the polyethylene glycol component is not included, that is, the main raw materials include 2,5-furandicarboxylic acid, 1,4-butanediol, and succinic acid, and the specific preparation process is similar to that of Example 1.
[0052] The viscosity and melting point of each embodiment and comparative example were tested respectively, and the relevant test results are shown in Table 1:
[0053] Table 1: Viscosity and melting point test results of products prepared in Examples and Comparative Examples
[0054] Intrinsic viscosity / dL / g Melting point / ℃ Example 1 0.73 156 Example 2 0.70 145 Example 3 0.69 139 Comparative Example 1 0.80 170 Comparative Example 2 0.66 161 Comparative Example 3 0.75 165
[0055] As can be seen from Table 1, the furan copolyester slices prepared in Examples 1-3 have lower melting points than the slices prepared in Comparative Example 1, and the change in melting point is related to the content of the introduced fatty chain dibasic acid and flexible polyether diol segments. The higher the content of the two, the more obvious the drop in melting point. In addition, it can be seen from Comparative Examples 2 and 3 that the effects of fatty chain dibasic acid and flexible polyether diol segments on the melting point of furan copolyester are different, but both can play a role in reducing the melting point of furan copolyester to a certain extent. This shows that by introducing fatty chain dibasic acid and flexible polyether diol segments into the main chain of poly-2,5-furandicarboxylic acid butylene glycol ester molecules, the regularity of the macromolecular chain can be destroyed, the intermolecular force can be effectively reduced, and the overall flexibility of the molecular chain can be further increased, so that the crystallization effect of the prepared furan copolyester is deteriorated, thereby achieving the effect of reducing the melting point.
[0056] Obviously, the above embodiments are only examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art may make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a low melting point furan copolyester, It is characterized in that The method comprises: subjecting 2,5-furandicarboxylic acid, 1,4-butanediol and aliphatic chain dibasic acid to an esterification reaction, and then adding polyether diol into the system for copolymerization to obtain a low melting point furan copolyester.
2. The preparation method according to claim 1, It is characterized in that The fatty chain dibasic acid is at least one selected from succinic acid, adipic acid, azelaic acid, sebacic acid, and dibasic acids with a carbon chain length greater than 10.
3. The preparation method according to claim 1, It is characterized in that The polyether diol is selected from at least one of polyethylene glycol and polypropylene glycol.
4. The preparation method according to claim 1, It is characterized in that The preparation method of the low melting point furan copolyester specifically comprises the following steps: (1) adding 2,5-furandicarboxylic acid, 1,4-butanediol, aliphatic dibasic acid and a catalyst into a polymerization reactor, mixing, stirring and heating under closed oxygen-free conditions, staying at 70-80° C. for 0.5-1 h, then heating to 160-190° C., and reacting at normal pressure for 1-2 h, then adding a certain amount of 1,4-butanediol, and reacting for 1.5-3 h to complete the esterification reaction; (2) adding polyether diol and antioxidant to the polymerization system after the esterification reaction in step (1), heating to 190-210° C. for reaction for 1-3 h, and simultaneously performing vacuum operation. Finally, after the reaction is completed at 220-240° C. and the system vacuum pressure is less than 100 Pa, nitrogen is filled, discharged, and pelletized to obtain low-melting-point furan copolyester chips.
5. The preparation method according to claim 4, It is characterized in that The catalyst is selected from at least one of tetrabutyl titanate, isopropyl titanate, antimony glycolate, antimony trioxide, germanium oxide, and stannous oxide.
6. The preparation method according to claim 4, It is characterized in that The antioxidant is selected from at least one of antioxidants 1010, 1098, 168, triphenyl phosphite and trimethyl phosphate.
7. The preparation method according to claim 4, It is characterized in that The molar ratio of the total amount of 2,5-furandicarboxylic acid and fatty chain dibasic acid to 1,4-butanediol is 1:2.0-3.5, the mass ratio of 2,5-furandicarboxylic acid to fatty chain dibasic acid is 1:0.1-0.5, and the mass ratio of 2,5-furandicarboxylic acid to catalyst is 1:0.002-0.
005.
8. The preparation method according to claim 4, It is characterized in that The mass ratio of the polyether diol to the total amount of 2,5-furandicarboxylic acid, 1,4-butanediol and aliphatic chain dibasic acid is 0.05-0.25:1, and the mass ratio of the antioxidant to 2,5-furandicarboxylic acid is 0.001-0.005:
1.